High-elongation precise coupling fixing glue and preparation method thereof
Through the combination of specific components and process steps, the elongation of the break and bonding strength of the precision coupled fixing glue is improved, the problem of insufficient toughness in the prior art is solved, the bonding needs of miniaturized electronic equipment is met, and the bonding requirements of small-scale electronic equipment is met, and Maintain performance in high temperature and high humidity environments.
Patent Information
- Application Number
- CN202411144883.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-12
AI Technical Summary
The existing precision coupled fixing glue cannot meet the needs of smaller and smaller fixing parts due to insufficient toughness in miniaturized electronic equipment. To improve toughness, it requires sacrificing colloid strength, affecting the bonding and fixing effect.
Using polyurethane acrylic resin, acrylic active diluent, epoxy resin, epoxy active diluent, alicyclic primary amine and initiator, the elongation of the rubber break and stickiness of the glue through specific formula ratios and process steps. The bonding strength includes the reaction of the reaction of the reactive mono-operated epoxy active diluent to the alicyclic primary amine, followed by the addition of the tetrafunctional epoxy resin in batches, controlling the temperature and time, ensuring the balance of bond strength and elongation at break.
On the basis of maintaining high bonding strength, it has significantly improved the elongation of break to reach more than 35%, meets the bonding requirements of small precision equipment, and maintains good performance in high temperature and high humidity environments.
Smart Images

Figure BDA0005001935660000041 
Figure BDA0005001935660000061
Abstract
Description
Technical Field
[0001] The present invention relates to the field of adhesive technology, in particular to the field of IPCC09F, and more specifically to a high-elongation precision coupling fixing adhesive and a preparation method thereof. Background Art
[0002] Precision coupling fixing glue is a bonding material used between precision equipment or components. It is used in situations where precise alignment and fixing are required to provide a strong bonding effect. Most existing fixing glues have high strength and low toughness. With the miniaturization of electronic devices, the fixing parts are getting smaller and smaller. The toughness of existing glues can no longer meet the needs. Improving the toughness of the glue requires sacrificing the strength of the glue, which affects the bonding and fixing effect.
[0003] CN103497723B discloses a novel optical fiber precision fixing glue, which is composed of the following components by weight: 20-50 parts of epoxy resin; 5-10 parts of active diluent; 5-20 parts of latent curing agent; 20-50 parts of filler; 1.0-5.0 parts of thixotropic agent; 0.1-5.0 parts of other auxiliary agents; 0.1-5.0 parts of pigment; the glue of the invention has an extremely low curing shrinkage rate and can meet the precision requirements of optical transceiver module (BOSA) assembly. However, the addition of a large amount of fillers affects the toughness of the glue. Summary of the invention
[0004] The first aspect of the present invention provides a high elongation precision coupling fixing glue, which comprises, by weight, 5-15 parts of polyurethane acrylic resin, 2-6 parts of acrylic reactive diluent, 6-15 parts of epoxy resin, 5-12 parts of epoxy reactive diluent, 2-12 parts of alicyclic primary amine, 4-8 parts of initiator, and 0.5-4 parts of antioxidant.
[0005] The acrylic acid reactive diluent includes a monofunctional acrylic acid reactive diluent and a trifunctional acrylic acid reactive diluent.
[0006] Preferably, the weight ratio of the trifunctional acrylic acid reactive diluent to the monofunctional acrylic acid reactive diluent is (0.3-3):1.
[0007] Preferably, the monofunctional acrylic acid reactive diluent includes at least one of the following brands of Sartomer: SR506NS, SR423NS.
[0008] Preferably, the trifunctional acrylic acid reactive diluent includes at least one of the following brands of Sartomer: SR351NS, SR368NS.
[0009] The epoxy reactive diluent includes a monofunctional epoxy reactive diluent and a difunctional epoxy reactive diluent.
[0010] Preferably, the monofunctional epoxy reactive diluent includes at least one of the following brands of Anhui Xinyuan Technology Co., Ltd.: XY693, XY757, and XY690.
[0011] Preferably, the difunctional epoxy reactive diluent includes at least one of the following brands produced by Anhui Xinyuan Technology Co., Ltd.: XY207A, XY622.
[0012] The initiator includes a free radical photoinitiator and an imidazole thermal initiator.
[0013] Preferably, the weight ratio of the free radical photoinitiator to the imidazole thermal initiator is (1-2): (2-1).
[0014] Preferably, the free radical photoinitiator is selected from at least one of the following brands: IGMOmnirad819, Omnirad184.
[0015] Preferably, the imidazole thermal initiator is selected from at least one of the following brands: Ajinomoto PN-40, Ajinomoto PN-50.
[0016] The viscosity of the polyurethane acrylic resin at 60° C. is 6000-30000 mPa·s.
[0017] Preferably, the polyurethane acrylic resin includes at least one of the following brands of Sartomer: CN8888NS, CN8887NS, CN996NS, and CN9010NS.
[0018] The epoxy resin includes a difunctional epoxy resin and a tetrafunctional epoxy resin.
[0019] Preferably, the weight ratio of the difunctional epoxy resin to the tetrafunctional epoxy resin is (1-6):(3-8).
[0020] Preferably, the difunctional epoxy resin is selected from at least one of polyether-modified bisphenol A epoxy resin and alicyclic epoxy resin.
[0021] Further preferably, the difunctional epoxy resin is selected from at least one of the following brands: Daicel PB3600 and Adec EP-4000.
[0022] Preferably, the tetrafunctional epoxy resin contains a naphthalene ring in its structure.
[0023] Further preferably, the tetrafunctional epoxy resin is purchased from DIC, P-9500.
[0024] Preferably, the molar ratio of the alicyclic primary amine to the monofunctional epoxy reactive diluent is (1-3):1.
[0025] A second aspect of the present invention provides a method for preparing a high-elongation precision coupling fixing adhesive, comprising the following steps:
[0026] S1, adding a monofunctional epoxy reactive diluent dropwise to an alicyclic primary amine for reaction to obtain a mixture 1;
[0027] S2, adding mixture 1 to the tetrafunctional epoxy resin in 5-10 batches, stirring evenly after the addition is completed, and cooling to 20-35° C. to obtain mixture 2;
[0028] S3, uniformly mixing the remaining components with the mixture 2 to obtain.
[0029] Preferably, the interval time of each batch during the addition in step S2 is 0.5-1h, and the temperature is maintained at 80-120°C during the addition process.
[0030] The applicant has found that the elongation at break of the material can be improved by first dropping a monofunctional epoxy reactive diluent into an alicyclic primary amine for reaction to obtain mixture 1, which may be due to the partial pre-toughening of the epoxy structure. In step 2, mixture 1 is then added to a tetrafunctional epoxy resin in 5-10 batches, which can further increase the elongation at break to more than 20% while maintaining the bonding strength. This may be due to the specific orderly arrangement of the structure during curing, which allows the polyurethane structure to fully exert its toughening and buffering effects. It is further defined that the interval time between each batch during addition in step S2 is 0.5-1h, and the temperature is maintained at 80-120°C during the addition process, which can make the elongation at break reach more than 35% on the basis of a bonding strength greater than 20MPa, so that it meets the bonding requirements between small precision equipment or components.
[0031] Preferably, the stirring time is 2-6 hours.
[0032] Preferably, the molar ratio of the mixture 1 to the tetrafunctional epoxy resin is (1-3):1.
[0033] Beneficial Effects
[0034] 1. The weight ratio of the trifunctional acrylic acid reactive diluent to the monofunctional acrylic acid reactive diluent is (0.3-3):1, which can improve the structural stability of the adhesive layer after curing, and improve the bonding strength and aging strength.
[0035] 2. The monofunctional epoxy active diluent is added dropwise to the alicyclic primary amine to react to obtain a mixture 1, which can improve the elongation at break of the material.
[0036] 3. Step 2: Add the mixture 1 into the tetrafunctional epoxy resin in 5-10 batches, which can further increase the elongation at break to more than 20% while maintaining the bonding strength.
[0037] 4. The interval time of each batch of addition in step S2 is limited to 0.5-1h, and the temperature is maintained at 80-120°C during the addition process, which can make the bonding strength greater than 20MPa and the elongation at break reach more than 35%.
[0038] 5. The initiator includes a free radical photoinitiator and an imidazole thermal initiator, which can enable the glue to maintain good performance even in a high temperature and high humidity environment. DETAILED DESCRIPTION
[0039] Examples 1-6, Comparative Examples 1-8
[0040] A high elongation precision coupling fixing glue, the formula is shown in Table 1:
[0041] Among them, the formula of comparative example 1 is the same as that of embodiment 1; the formula of comparative example 2 is the same as that of embodiment 2; the formula of comparative example 4 is the same as that of embodiment 1; the formula of comparative example 5 is the same as that of embodiment 2; and the formulas of comparative examples 6-8 are the same as that of embodiment 1.
[0042] Polyurethane acrylic resin, Sartomer, model: CN8888NS; monofunctional acrylic reactive diluent, Sartomer, model: SR506NS; trifunctional reactive diluent includes Sartomer, model: SR351NS; difunctional epoxy resin, Daicel, model: PB3600; tetrafunctional epoxy resin, DICHP-9500; monofunctional epoxy reactive diluent, Anhui Xinyuan Technology Co., Ltd., XY693; difunctional epoxy reactive diluent, Anhui Xinyuan Technology Co., Ltd., XY207A; alicyclic primary amine, Evonik Ancamine450; free radical photoinitiator, IGMOmnirad819; imidazole thermal initiator, Ajinomoto PN-40; antioxidant, Shanghai Feige Chemical Co., Ltd. BHT.
[0043] Table 1
[0044]
[0045] Embodiment 1-6, a method for preparing a high elongation precision coupling fixing adhesive, comprises the following steps:
[0046] S1, adding a monofunctional epoxy reactive diluent dropwise to an alicyclic primary amine for reaction to obtain a mixture 1;
[0047] S2, adding mixture 1 into the tetrafunctional epoxy resin in 8 batches, with an interval of 0.8 h between each batch, maintaining the temperature at 100° C. during the addition process, continuing to stir for 4 h to mix evenly, and cooling to 25° C. to obtain mixture 2;
[0048] S3, uniformly mixing the remaining components with the mixture 2 to obtain.
[0049] Comparative Example 1-2, a method for preparing a coupling fixing glue, comprises the following steps: all components are mixed evenly to obtain the coupling fixing glue.
[0050] Comparative Example 3, a method for preparing a coupling fixing glue, comprising the following steps:
[0051] S1, adding a monofunctional epoxy reactive diluent dropwise to an alicyclic primary amine for reaction to obtain a mixture 1;
[0052] S2, adding mixture 1 into the tetrafunctional epoxy resin in 8 batches, with an interval of 0.8 h between each batch, maintaining the temperature at 100° C. during the addition process, continuing to stir for 4 h to mix evenly, and cooling to 25° C. to obtain mixture 2;
[0053] S3, uniformly mixing the remaining components with the mixture 2 to obtain.
[0054] Comparative Example 4-5, a method for preparing a coupling fixing glue, comprising the following steps:
[0055] S1, adding a monofunctional epoxy reactive diluent dropwise to an alicyclic primary amine for reaction to obtain a mixture 1;
[0056] S2, uniformly mix the remaining components with the mixture 1 to obtain.
[0057] Comparative Example 6: A method for preparing a coupling fixing glue, comprising the following steps:
[0058] S1, adding a monofunctional epoxy reactive diluent dropwise to an alicyclic primary amine for reaction to obtain a mixture 1;
[0059] S2, adding the mixture to the tetrafunctional epoxy resin, maintaining the temperature at 100° C. during the addition process, continuing to stir for 4 hours to mix evenly, and cooling to 25° C. to obtain a mixture 2;
[0060] S3, uniformly mixing the remaining components with the mixture 2 to obtain.
[0061] Comparative Example 7: A method for preparing a coupling fixing glue, comprising the following steps:
[0062] S1, adding a monofunctional epoxy reactive diluent dropwise to an alicyclic primary amine for reaction to obtain a mixture 1;
[0063] S2, adding mixture 1 into the tetrafunctional epoxy resin in 8 batches, with an interval of 0.8 h between each batch, maintaining the temperature at 100° C. during the addition process, continuing to stir for 1 h to mix evenly, and cooling to 25° C. to obtain mixture 2;
[0064] S3, uniformly mixing the remaining components with the mixture 2 to obtain.
[0065] Comparative Example 8: A method for preparing a coupling fixing glue, comprising the following steps:
[0066] S1, adding a monofunctional epoxy reactive diluent dropwise to an alicyclic primary amine for reaction to obtain a mixture 1;
[0067] S2, adding mixture 1 into the tetrafunctional epoxy resin in 8 batches, with an interval of 0.8 h between each batch, maintaining the temperature at 70° C. during the addition process, and continuing to stir for 4 h to mix evenly after the addition is completed, and cooling to 25° C. to obtain mixture 2;
[0068] S3, uniformly mixing the remaining components with the mixture 2 to obtain.
[0069] Performance Testing Methods
[0070] The fixing glue prepared in the embodiment and the comparative example was subjected to performance tests, and the test data are listed in Table 2.
[0071] 1. Elongation at break:
[0072] Prepare dog bone samples with an average thickness of 1 mm, treat them under pure thermosetting conditions, and perform mechanical tensile tests at a gauge length of 25 mm and a tensile speed of 10 mm / min. Take the average value for a group of 3 samples.
[0073] 2. Determination of bonding strength:
[0074] Glass, anodized aluminum 4*4mm glass and substrate bonding, UV + thermosetting conditions, average thickness of the adhesive layer 35m, shear force tested at a speed of 10mm / min. A group of 7 samples, take the average value.
[0075] 3. Test of body strength:
[0076] Prepare dog bone samples with an average thickness of 1 mm, treat them under pure thermosetting conditions, and perform mechanical tensile tests at a gauge length of 25 mm and a tensile speed of 10 mm / min. Take the average value for a group of 3 samples.
[0077] 4. High temperature and high humidity aging test:
[0078] 85℃, 85%RH1700h, other test methods are equivalent to the test of elongation at break and bulk strength.
[0079] Performance test data
[0080] Table 2
[0081]
Claims
1. A high elongation precision coupling fixing adhesive, characterized in that: Calculated by weight, the components include: 5-15 parts of polyurethane acrylic resin, 2-6 parts of acrylic reactive diluent, 6-15 parts of epoxy resin, 5-12 parts of epoxy reactive diluent, 2-12 parts of alicyclic primary amine, 4-8 parts of initiator, and 0.5-4 parts of antioxidant.
2. The high elongation precision coupling fixing adhesive according to claim 1, characterized in that: The acrylic acid reactive diluent includes a monofunctional acrylic acid reactive diluent and a trifunctional acrylic acid reactive diluent, and the weight ratio of the trifunctional acrylic acid reactive diluent to the monofunctional acrylic acid reactive diluent is (0.3-3):
1.
3. The high elongation precision coupling fixing adhesive according to claim 2, characterized in that: The epoxy resin includes a difunctional epoxy resin and a tetrafunctional epoxy resin.
4. The high elongation precision coupling fixing adhesive according to claim 3, characterized in that: The epoxy reactive diluent includes a monofunctional epoxy reactive diluent and a difunctional epoxy reactive diluent.
5. The high elongation precision coupling fixing adhesive according to claim 4, characterized in that: The initiator includes a free radical photoinitiator and an imidazole thermal initiator.
6. The high elongation precision coupling fixing adhesive according to claim 5, characterized in that: The viscosity of the polyurethane acrylic resin at 60° C. is 6000-30000 mPa·s.
7. The high elongation precision coupling fixing adhesive according to claim 5, characterized in that: The tetrafunctional epoxy resin contains a naphthalene ring in its structure.
8. A method for preparing the high elongation precision coupling fixing adhesive according to any one of claims 5 to 7, characterized in that: The following steps are involved: S1, adding a monofunctional epoxy reactive diluent dropwise to an alicyclic primary amine for reaction to obtain a mixture 1; S2, adding mixture 1 to the tetrafunctional epoxy resin in 5-10 batches, stirring evenly after the addition is completed, and cooling to 20-35° C. to obtain mixture 2; S3, uniformly mixing the remaining components with the mixture 2 to obtain.
9. The method for preparing the high elongation precision coupling fixing adhesive according to claim 8, characterized in that: The steps The interval time for each batch of S2 is 0.5-1h, and the temperature is maintained at 80-120℃ during the addition process.
10. The method for preparing the high elongation precision coupling fixing adhesive according to claim 9, characterized in that: The stirring time is 2-6h.