Strong-adhesion conductive silica gel as well as preparation method and application thereof
By using 2-3μm silver-modified graphene oxide microcapsules and epoxy anchoring agent in electromagnetic shielding materials, combined with thixotropic agent, the problem of large amount of conductive material when the conductive properties and shielding efficiency is improved, and high Take into account both bonding strength and environmental protection.
Patent Information
- Application Number
- CN202411210137.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-12
AI Technical Summary
When existing electromagnetic shielding materials improve the conductivity and shielding performance, they use more conductive materials, which affects the adhesive strength and environmental protection of the materials.
The silver-modified graphene oxide microcapsules with particle size of 2-3μm and epoxy-containing bifunctional group anchoring agent are used to uniformly disperse the conductive microcapsules in the silicone system to reduce the amount of conductive material and improve the adhesion, while adding contact The variable agent adjusts the thixotropy of the glue to prevent collapse and separation of oil powder.
Without affecting the conductive performance and shielding performance, the amount of conductive material is reduced, the bonding strength and the shape retention force of the adhesive material are improved, and the adhesion to the substrate is enhanced. The shear strength of aluminum to aluminum reaches 4.5 MPa avoids oil powder separation.
Smart Images

Figure CN118931487A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of conductive adhesives, and in particular to a strong-bonding conductive silicone rubber and a preparation method and application thereof. Background Art
[0002] With the development of technology in the field of electronic communications, the development purpose of electronic equipment is to diversify, miniaturize and portability. Power modules are developing in the direction of miniaturization, density and increased power consumption. The large increase in components has put higher and higher requirements on electromagnetic shielding in electronic equipment. When electronic equipment is working, it does not want to be interfered by external electromagnetic waves, nor does it want its own radiation to affect other electronic equipment and cause radiation damage to the human body. This has brought huge challenges to electromagnetic shielding materials. Electromagnetic shielding materials are also developing in the direction of higher shielding efficiency, wider shielding frequency and excellent comprehensive performance.
[0003] According to different types of base glue, traditional electromagnetic shielding materials mainly include epoxy, acrylic and silicone systems. The epoxy system has outstanding bonding performance, but poor heat resistance and weather resistance; acrylic glue has high strength, but poor reliability, and usually contains a large amount of solvents, which is not environmentally friendly; the silicone system is soft, the elastomer has good heat resistance and good environmental protection, but the bonding strength is poor. Patent CN112898945B discloses a two-component conductive silicone rubber and its preparation method and application. 107 glue is used as the main raw material to prepare A glue and B glue respectively, and nickel-coated graphite / carbon fiber is used as the conductive material. The particle size of nickel-coated graphite / carbon fiber is 30-50μm, and the dosage is large.
[0004] Therefore, it is very important to provide a conductive silicone that uses less conductive material and does not affect the conductive performance and shielding effectiveness. Summary of the invention
[0005] The embodiment of the present application provides a strong bonding conductive silicone to solve the problem of using more conductive materials in order to improve the conductive performance and shielding effectiveness in the related art.
[0006] In the first aspect, the present application provides a strongly bonding conductive silicone, comprising the following raw materials in parts by weight: 6 to 20 parts of vinyl silicone oil, 2-5 parts of vinyl silicone resin, 2 to 5 parts of hydrogenated silicone oil, 1 to 3 parts of anchoring agent, 1 to 3 parts of thixotropic agent, 0.1 to 1 part of catalyst, 0.05 to 0.5 part of inhibitor, 5 to 10 parts of solvent, and 20 to 40 parts of conductive microcapsules, wherein the shell material of the conductive microcapsules is silver and the core material is modified graphene oxide.
[0007] In some embodiments, the conductive microcapsules include the following raw materials, measured by mass: 5 to 20 parts of graphene oxide, 2 to 5 parts of 3-aminopropyltrimethoxysilane, 15 to 30 parts of silver nitrate, 10 to 20 parts of anhydrous ethanol, 10 to 20 parts of sodium citrate, 1 to 5 parts of sodium dodecylbenzene sulfonate, and 1 to 5 parts of polyvinyl alcohol.
[0008] In some embodiments, the vinyl silicone oil is a vinyl-terminated silicone oil with a vinyl content of 0.5%-1.2% and a viscosity of 500-5000 mPa·s.
[0009] In some embodiments, the vinyl silicone resin is a vinyl MQ resin having a viscosity of 5000-50000 mPa·s.
[0010] In some embodiments, the hydrogen-containing silicone oil is a partially hydrogen-containing silicone oil having a hydrogen content of 0.2-1.2% and a viscosity of 30-70 mPa·s.
[0011] In some embodiments, the structural formula of the anchoring agent is:
[0012] In the formula, R is -CH3, R1 is -CH2CH3, and a=0 or 1.
[0013] In some embodiments, the anchoring agent is prepared by the following process:
[0014] Allyl alcohol, tetrabutylammonium bromide and liquid alkali are reacted at 60°C in a mass ratio of 6:4:1 for 1 hour, allyl chloride is slowly added dropwise, refluxed for 6 hours, cooled, filtered and distilled to obtain diallyl ether; the prepared diallyl ether and Speier catalyst are activated at 70°C for 20 minutes in a mass ratio of 8:1, chlorosilane is added dropwise, and after the addition, the mixture is kept at 75°C for 2 hours, cooled and distilled to obtain 3-allyloxypropyl chlorosilane; the synthesized 3-allyloxypropyl chlorosilane is esterified with ethanol in a mass ratio of 3:1 to obtain 3-allyloxypropyl triethoxysilane; 3-allyloxypropyl triethoxysilane, butyraldehyde and Ni(bpy)2Cl2 are stirred and mixed evenly in a mass ratio of 10:2:3, reacted at 50°C for 4 hours under continuous oxygen flow, and distilled under reduced pressure to obtain an anchoring agent.
[0015] In some embodiments, the thixotropic agent is at least one of fumed silica, polyethylene wax, and organic bentonite.
[0016] In some embodiments, the catalyst is a platinum catalyst having a platinum content of 3000 to 5000 ppm.
[0017] In some embodiments, the inhibitor is at least one of 3-methyl-1-butyn-3-ol, 1-ethynylcyclohexanol, and 3,5-dimethyl-1-hexyn-3-ol.
[0018] In some embodiments, the solvent is at least one of silicone oil, PGMEA, anhydrous ethanol, ethylene glycol, ethyl ether, ethyl acetate, and low molecular weight silane.
[0019] In some embodiments, the particle size of the conductive microcapsules is 2-3 μm.
[0020] In a second aspect, the present application also provides a method for preparing the above-mentioned strong bonding conductive silicone, comprising the following steps:
[0021] S101, mixing vinyl silicone oil, vinyl silicone resin, anchoring agent, thixotropic agent and solvent in a kneader, setting the temperature at 130-150° C. for 2-4 hours, mixing evenly, and grinding with a three-roll mill after cooling to obtain a pre-dispersed liquid;
[0022] S102, adding conductive microcapsules to the pre-dispersion liquid, setting the temperature at 120° C., kneading time for 2 hours, cooling to room temperature, then adding hydrogenated silicone oil, mixing and dispersing in a double planetary mixer, wherein the stirring speed is 100 rpm / min, the dispersing speed is 800 rpm, and the stirring and dispersing time is 30 minutes, then adding an inhibitor, stirring speed is 100 rpm / min, the dispersing speed is 800 rpm, and the stirring and dispersing time is 30 minutes, to obtain a mixed rubber material;
[0023] S103, adding a catalyst to the mixed rubber material, mixing and dispersing in a double planetary mixer, with a stirring speed of 100 rpm / min and a dispersing speed of 800 rpm, vacuum treatment, with a vacuum degree lower than -0.095 MPa, for 30 minutes, vacuum filling the mixed rubber material into a rubber barrel, dispensing with a glue dispenser, curing at a high temperature of 150°C for 0.5-1h, and obtaining a strong bonding conductive silicone rubber.
[0024] In some embodiments, the conductive microcapsules are prepared by the following process:
[0025] 3-aminopropyltrimethoxysilane is added to deionized water, and after stirring evenly, graphene oxide powder is added, stirring is continued until a uniform suspension is formed, and then modified graphene oxide is obtained by centrifugal separation;
[0026] Adding silver nitrate into anhydrous ethanol and dissolving it to obtain an ethanol solution of silver nitrate;
[0027] The modified graphene oxide is dispersed in deionized water, sodium dodecylbenzene sulfonate and polyvinyl alcohol are added, and then an ethanol solution of silver nitrate is added, and sodium citrate is slowly added while stirring, and the reaction mixture is freeze-dried to obtain conductive microcapsules.
[0028] On the third aspect, the present application also provides the application of the above-mentioned strong bonding conductive silicone in conductive bonding in industries such as liquid crystal displays, 5G communications, and electronic appliances.
[0029] The beneficial effects of the technical solution provided by this application include:
[0030] 1. The present application uses conductive microcapsules with a core-shell structure and a particle size of 2-3 μm. The anchoring agent containing epoxy and alkoxy bifunctional groups can treat the surface of the conductive microcapsules, so that the conductive microcapsules are evenly dispersed in the silica gel system, and the amount of conductive microcapsules is reduced without affecting the conductive performance and shielding effectiveness. On the other hand, the presence of epoxy groups greatly increases the adhesion of the rubber to the substrate after curing, and the shear strength of aluminum to aluminum can reach 4.5 MPa.
[0031] 2. The present application adjusts the thixotropy of the rubber by adding a thixotropic agent, so that the rubber does not collapse after being dispensed from the rubber barrel and has good shape retention; at the same time, the thixotropy prevents oil-powder separation from occurring during storage of the rubber. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0033] Figure 1 This is a schematic diagram of a process for preparing a strong bonding conductive silicone rubber according to the present application. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0035] The embodiment of the present application provides a strong bonding conductive silicone, which can solve the problem of using more conductive materials in order to improve the conductive performance and shielding effectiveness in the related art.
[0036] refer to Figure 1 This embodiment provides a method for preparing a strong bonding conductive silicone rubber, comprising the following steps:
[0037] Step S101, by weight, 6 to 20 parts of vinyl silicone oil, 2 to 5 parts of vinyl silicone resin, 1 to 3 parts of anchoring agent, 1 to 3 parts of thixotropic agent and 5 to 10 parts of solvent are stirred and mixed in a kneader, the temperature is set at 130-150° C., the kneading time is 2 to 4 hours, the mixture is mixed evenly, and after cooling, the mixture is ground with a three-roll mill to obtain a pre-dispersed liquid;
[0038] Step S102, adding 20 to 40 parts of conductive microcapsules to the pre-dispersion liquid, setting the temperature at 120° C., kneading time for 2 hours, cooling to room temperature, then adding 2 to 5 parts of hydrogenated silicone oil, mixing and dispersing in a double planetary mixer, wherein the stirring speed is 100 rpm / min, the dispersing speed is 800 rpm, the stirring and dispersing time is 30 minutes, then adding 0.05 to 0.5 parts of inhibitor, stirring speed is 100 rpm / min, the dispersing speed is 800 rpm, and the stirring and dispersing time is 30 minutes, to obtain a mixed rubber material;
[0039] Step S103, add 0.1 to 1 parts of catalyst to the mixed rubber material, mix and disperse it in a double planetary mixer, the stirring speed is 100 rpm / min, the dispersion speed is 800 rpm, vacuum treatment, the vacuum degree is lower than -0.095Mpa, the time is 30 minutes, the mixed rubber material is vacuum filled in a rubber barrel, and glue is dispensed by a glue dispenser, and cured at a high temperature of 150°C for 0.5-1h to obtain a strong bonding conductive silicone.
[0040] The conductive microcapsules are prepared by the following process: adding 2 to 5 parts of 3-aminopropyltrimethoxysilane to deionized water by mass, stirring evenly, adding 5 to 20 parts of graphene oxide powder, continuing to stir until a uniform suspension is formed, and then obtaining modified graphene oxide by centrifugation; adding 15 to 30 parts of silver nitrate to anhydrous ethanol, dissolving, and obtaining an ethanol solution of silver nitrate; dispersing the modified graphene oxide in deionized water, adding 1 to 5 parts of sodium dodecylbenzene sulfonate and 1 to 5 parts of polyvinyl alcohol, and then adding the ethanol solution of silver nitrate, slowly adding 10 to 20 parts of sodium citrate while stirring, and freeze-drying the mixture obtained by the reaction at -20 to -45°C to obtain conductive microcapsules.
[0041] The strong bonding conductive silicone rubber and the preparation method thereof provided by the present application are described in detail below in combination with embodiments and comparative examples.
[0042] In the following examples, the anchoring agent is prepared by the following process:
[0043] Allyl alcohol, tetrabutylammonium bromide and liquid caustic soda are reacted at 60°C for 1 hour in a mass ratio of 6:4:1, allyl chloride is slowly added dropwise, refluxed for 6 hours, cooled, filtered and distilled to obtain diallyl ether; the prepared diallyl ether and Speier catalyst are activated at 70°C for 20 minutes in a mass ratio of 8:1, chlorosilane is added dropwise, and after the addition, the mixture is kept at 75°C for 2 hours, cooled and distilled to obtain 3-allyloxypropyl chlorosilane; the synthesized 3-allyloxypropyl chlorosilane is esterified with ethanol in a mass ratio of 3:1 to obtain 3-allyloxypropyl triethoxysilane; 3-allyloxypropyl triethoxysilane, butyraldehyde and Ni(bpy)2Cl2 are stirred and mixed uniformly in a mass ratio of 10:2:3, reacted at 50°C for 4 hours under continuous oxygen flow, and distilled under reduced pressure to obtain an anchoring agent In the formula, R is -CH3, R1 is -CH2CH3, and a=1.
[0044] Embodiment 1:
[0045] (1) Add 15 parts by mass of vinyl silicone oil with a vinyl content of 0.8% and a viscosity of 1500 mPa·s, 3 parts of vinyl silicone resin with a viscosity of 20000 mPa·s, 1 part of anchoring agent, 2 parts of fumed silica and 6 parts of anhydrous ethanol to a kneader, knead and disperse at room temperature, turn on heating after the color is uniform, set the temperature at 150° C., knead for 3 hours, mix evenly, and grind with a three-roll mill after cooling to obtain a pre-dispersion liquid;
[0046] (2) Add 22 parts by mass of conductive microcapsules to the pre-dispersion liquid, set the temperature at 120° C., evacuate the mixture, and make the vacuum degree lower than −0.095 MPa. Knead the mixture for 2 h. Cool the mixture to room temperature, then add 3 parts of hydrogenated silicone oil with a hydrogen content of 0.6% and a viscosity of 60 mPa·s, and mix and disperse the mixture in a double planetary mixer at a stirring speed of 100 rpm / min, a dispersing speed of 800 rpm, and a stirring and dispersing time of 30 min. Then, add 0.1 parts of 3-methyl-1-butyn-3-ol, stir at a stirring speed of 100 rpm / min, a dispersing speed of 800 rpm, and a stirring and dispersing time of 30 min to obtain a mixed rubber material.
[0047] (3) Add 0.4 parts of platinum catalyst to the mixed rubber material by weight, mix and disperse it in a double planetary mixer at a stirring speed of 100 rpm / min and a dispersion speed of 800 rpm. Vacuum treatment is performed with a vacuum degree lower than -0.095 MPa for 30 minutes. The dispersed rubber material is placed in a vacuum filling glue barrel for a dispensing test.
[0048] In Example 1, the conductive microcapsules were prepared by the following process:
[0049] By mass, 2.5 parts of 3-aminopropyltrimethoxysilane are added to deionized water, and after stirring evenly, 10 parts of graphene oxide powder are added, and stirring is continued until a uniform suspension is formed, and then modified graphene oxide is obtained by centrifugal separation; 18 parts of silver nitrate are added to anhydrous ethanol, dissolved, and an ethanol solution of silver nitrate is obtained; the modified graphene oxide is dispersed in deionized water, 1.5 parts of sodium dodecylbenzene sulfonate and 2 parts of polyvinyl alcohol are added, and then the ethanol solution of silver nitrate is added, and 18 parts of sodium citrate are slowly added while stirring, and the mixture obtained by the reaction is freeze-dried at -45°C to obtain conductive microcapsules.
[0050] Embodiment 2:
[0051] (1) Add 8 parts by mass of vinyl silicone oil with a vinyl content of 1.0% and a viscosity of 2000 mPa·s, 4 parts of vinyl silicone resin with a viscosity of 30000 mPa·s, 2 parts of anchoring agent and 1.5 parts of polyethylene wax, and 7 parts of ethylene glycol to a kneader and knead and disperse at room temperature until the color is uniform. Turn on the heating, set the temperature at 140° C., knead for 3 hours, mix evenly, and grind with a three-roll mill after cooling to obtain a pre-dispersion liquid;
[0052] (2) Add 25 parts by weight of conductive microcapsules to the pre-dispersion liquid, set the temperature at 120° C., evacuate the mixture, and knead it for 2 hours. Cool the mixture to room temperature, then add 3 parts of hydrogenated silicone oil with a hydrogen content of 0.5% and a viscosity of 60 mPa·s, and mix and disperse the mixture in a double planetary mixer at a stirring speed of 100 rpm / min, a dispersing speed of 800 rpm, and a stirring and dispersing time of 30 minutes. Then add 0.1 parts of 1-ethynylcyclohexanol, stir at a speed of 100 rpm / min, a dispersing speed of 800 rpm, and a stirring and dispersing time of 30 minutes to obtain a mixed rubber material.
[0053] (3) Add 0.2 parts of platinum catalyst to the mixed rubber material by weight, mix and disperse it in a double planetary mixer, with a stirring speed of 100 rpm / min and a dispersion speed of 800 rpm. Vacuum treatment is carried out with a vacuum degree lower than -0.095 MPa for 30 minutes. The dispersed rubber material is placed in a vacuum filling glue barrel for a dispensing test.
[0054] In Example 2, the conductive microcapsules were prepared by the following process:
[0055] By mass, 4 parts of 3-aminopropyltrimethoxysilane are added to deionized water, and after stirring evenly, 15 parts of graphene oxide powder are added, and stirring is continued until a uniform suspension is formed, and then modified graphene oxide is obtained by centrifugal separation; 18 parts of silver nitrate are added to anhydrous ethanol, dissolved, and an ethanol solution of silver nitrate is obtained; the modified graphene oxide is dispersed in deionized water, 2 parts of sodium dodecylbenzene sulfonate and 1.5 parts of polyvinyl alcohol are added, and then the ethanol solution of silver nitrate is added, and 12 parts of sodium citrate are slowly added while stirring, and the mixture obtained by the reaction is freeze-dried at -30°C to obtain conductive microcapsules.
[0056] Embodiment 3:
[0057] (1) Add 18 parts by mass of vinyl silicone oil with a vinyl content of 1.0% and a viscosity of 2000 mPa·s, 5 parts of vinyl silicone resin with a viscosity of 20000 mPa·s, 1 part of anchoring agent, 3 parts of organic bentonite, and 7 parts of ether to a kneader and knead and disperse at room temperature until the color is uniform. Turn on the heating, set the temperature at 150° C., knead for 3 hours, mix evenly, and grind with a three-roll mill after cooling to obtain a pre-dispersion liquid;
[0058] (2) Add 30 parts by mass of conductive microcapsules to the pre-dispersion liquid, set the temperature at 120° C., evacuate the mixture, and make the vacuum degree lower than −0.095 MPa. Knead for 2 h. Cool the mixture to room temperature, then add 3 parts of hydrogenated silicone oil with a hydrogen content of 0.4% and a viscosity of 50 mPa·s, and mix and disperse the mixture in a double planetary mixer at a stirring speed of 100 rpm / min, a dispersing speed of 800 rpm, and a stirring and dispersing time of 30 min. Then, add 0.2 parts of 3,5-dimethyl-1-hexyn-3-ol, stir at a stirring speed of 100 rpm / min, a dispersing speed of 800 rpm, and a stirring and dispersing time of 30 min to obtain a mixed rubber material.
[0059] (3) Add 0.6 parts of platinum catalyst by weight to the mixed rubber material, mix and disperse it in a double planetary mixer, with a stirring speed of 100 rpm / min and a dispersion speed of 800 rpm. Vacuum treatment is carried out with a vacuum degree lower than -0.095 MPa for 30 minutes. The dispersed rubber material is placed in a vacuum filling glue barrel for a dispensing test.
[0060] In Example 3, the conductive microcapsules were prepared by the following process:
[0061] By mass, 4.5 parts of 3-aminopropyltrimethoxysilane are added to deionized water, and after stirring evenly, 20 parts of graphene oxide powder are added, and stirring is continued until a uniform suspension is formed, and then modified graphene oxide is obtained by centrifugal separation; 25 parts of silver nitrate are added to anhydrous ethanol and dissolved to obtain an ethanol solution of silver nitrate; the modified graphene oxide is dispersed in deionized water, 3 parts of sodium dodecylbenzene sulfonate and 2 parts of polyvinyl alcohol are added, and then the ethanol solution of silver nitrate is added, and 12 parts of sodium citrate are slowly added while stirring, and the mixture obtained by the reaction is freeze-dried at -40°C to obtain conductive microcapsules.
[0062] Embodiment 4:
[0063] (1) Add 20 parts by mass of vinyl silicone oil with a vinyl content of 1.0% and a viscosity of 1500 mPa·s, 3 parts of vinyl silicone resin with a viscosity of 15000 mPa·s, 2 parts of anchoring agent and 3 parts of polyethylene wax, and 6 parts of ethyl acetate to a kneader and knead and disperse at room temperature until the color is uniform. Turn on the heating, set the temperature at 150° C., knead for 3 hours, mix evenly, and grind with a three-roll mill after cooling to obtain a pre-dispersion liquid;
[0064] (2) Add 40 parts by weight of conductive microcapsules to the pre-dispersion liquid, set the temperature at 120° C., evacuate the mixture, and make the vacuum degree lower than −0.095 MPa. Knead the mixture for 2 h. Cool the mixture to room temperature, then add 3 parts of hydrogenated silicone oil with a hydrogen content of 0.8% and a viscosity of 60 mPa·s, and mix and disperse the mixture in a double planetary mixer at a stirring speed of 100 rpm / min, a dispersing speed of 800 rpm, and a stirring and dispersing time of 30 min. Then, add 0.3 parts of 3-methyl-1-butyn-3-ol, stir at a stirring speed of 100 rpm / min, a dispersing speed of 800 rpm, and a stirring and dispersing time of 30 min to obtain a mixed rubber material.
[0065] (3) Add 0.6 parts of platinum catalyst by weight to the mixed rubber material, mix and disperse it in a double planetary mixer, with a stirring speed of 100 rpm / min and a dispersion speed of 800 rpm. Vacuum treatment is carried out with a vacuum degree lower than -0.095 MPa for 30 minutes. The dispersed rubber material is placed in a vacuum filling glue barrel for a dispensing test.
[0066] In Example 4, the conductive microcapsules were prepared by the following process:
[0067] By mass, 5 parts of 3-aminopropyltrimethoxysilane are added to deionized water, and after stirring evenly, 18.5 parts of graphene oxide powder are added, and stirring is continued until a uniform suspension is formed, and then modified graphene oxide is obtained by centrifugal separation; 25 parts of silver nitrate are added to anhydrous ethanol and dissolved to obtain an ethanol solution of silver nitrate; the modified graphene oxide is dispersed in deionized water, 4 parts of sodium dodecylbenzene sulfonate and 1.5 parts of polyvinyl alcohol are added, and then the ethanol solution of silver nitrate is added, and 18 parts of sodium citrate are slowly added while stirring, and the mixture obtained by the reaction is freeze-dried at -35°C to obtain conductive microcapsules.
[0068] Embodiment 5:
[0069] (1) Add 8 parts by mass of vinyl silicone oil with a vinyl content of 0.8% and a viscosity of 1000 mPa·s, 2.5 parts of vinyl silicone resin with a viscosity of 10000 mPa·s, 1.5 parts of anchoring agent and 2.5 parts of organic bentonite, and 7 parts of ether to a kneader, knead and disperse at room temperature, turn on the heating after the color is uniform, set the temperature at 150° C., knead for 3 hours, mix evenly, and grind with a three-roll mill after cooling to obtain a pre-dispersion liquid;
[0070] (2) Add 35 parts of conductive microcapsules to the pre-dispersion liquid by weight, set the temperature at 120° C., evacuate the mixture, and make the vacuum degree lower than −0.095 MPa. Knead the mixture for 2 h. Cool the mixture to room temperature, then add 3 parts of hydrogenated silicone oil with a hydrogen content of 0.6% and a viscosity of 40 mPa·s, and mix and disperse the mixture in a double planetary mixer at a stirring speed of 100 rpm / min, a dispersing speed of 800 rpm, and a stirring and dispersing time of 30 min. Then, add 0.4 parts of 3-methyl-1-butyn-3-ol, stir at a stirring speed of 100 rpm / min, a dispersing speed of 800 rpm, and a stirring and dispersing time of 30 min to obtain a mixed rubber material.
[0071] (3) Add 0.6 parts of platinum catalyst by weight to the mixed rubber material, mix and disperse it in a double planetary mixer, with a stirring speed of 100 rpm / min and a dispersion speed of 800 rpm. Vacuum treatment is carried out with a vacuum degree lower than -0.095 MPa for 30 minutes. The dispersed rubber material is placed in a vacuum filling glue barrel for a dispensing test.
[0072] In Example 5, the conductive microcapsules were prepared by the following process:
[0073] By mass, 3 parts of 3-aminopropyltrimethoxysilane are added to deionized water, and after stirring evenly, 16.5 parts of graphene oxide powder are added, and stirring is continued until a uniform suspension is formed, and then modified graphene oxide is obtained by centrifugal separation; 21 parts of silver nitrate are added to anhydrous ethanol and dissolved to obtain an ethanol solution of silver nitrate; the modified graphene oxide is dispersed in deionized water, 2.5 parts of sodium dodecylbenzene sulfonate and 1.5 parts of polyvinyl alcohol are added, and then the ethanol solution of silver nitrate is added, and 15 parts of sodium citrate are slowly added while stirring, and the mixture obtained by the reaction is freeze-dried at -35°C to obtain conductive microcapsules.
[0074] Comparative Example 1:
[0075] (1) Add 15 parts by mass of vinyl silicone oil with a vinyl content of 0.8% and a viscosity of 1500 mPa·s, 3 parts of vinyl silicone resin with a viscosity of 20000 mPa·s, 2 parts of fumed silica and 6 parts of anhydrous ethanol to a kneader and knead and disperse at room temperature until the color is uniform. Turn on the heating, set the temperature at 150° C., knead for 3 hours, mix evenly, and grind with a three-roll mill after cooling to obtain a pre-dispersion liquid;
[0076] (2) Add 22 parts by mass of conductive microcapsules to the pre-dispersion liquid, set the temperature at 120° C., evacuate the mixture, and make the vacuum degree lower than −0.095 MPa. Knead the mixture for 2 h. Cool the mixture to room temperature, then add 3 parts of hydrogenated silicone oil with a hydrogen content of 0.6% and a viscosity of 60 mPa·s, and mix and disperse the mixture in a double planetary mixer at a stirring speed of 100 rpm / min, a dispersing speed of 800 rpm, and a stirring and dispersing time of 30 min. Then, add 0.1 parts of 3-methyl-1-butyn-3-ol, stir at a stirring speed of 100 rpm / min, a dispersing speed of 800 rpm, and a stirring and dispersing time of 30 min to obtain a mixed rubber material.
[0077] (3) Add 0.4 parts of platinum catalyst by weight to the mixed rubber material, mix and disperse it in a double planetary mixer, where the stirring speed is 100 rpm / min, the dispersion speed is 800 rpm, and the vacuum treatment is carried out with a vacuum degree lower than -0.095 MPa for 30 minutes. The dispersed rubber material is placed in a vacuum filling glue barrel and a dispensing test is carried out.
[0078] The preparation process of the conductive microcapsules used in Comparative Example 1 is the same as that of Example 1.
[0079] Comparative Example 2:
[0080] (1) Add 15 parts by mass of vinyl silicone oil with a vinyl content of 0.8% and a viscosity of 1500 mPa·s, 3 parts of vinyl silicone resin with a viscosity of 20000 mPa·s, 3 parts of anchoring agent, and 6 parts of anhydrous ethanol to a kneader and knead and disperse at room temperature until the color is uniform. Turn on the heating, set the temperature at 150° C., knead for 3 hours, mix evenly, and grind with a three-roll mill after cooling to obtain a pre-dispersion liquid;
[0081] (2) Add 22 parts by mass of conductive microcapsules to the pre-dispersion liquid, set the temperature at 120° C., evacuate the mixture, and make the vacuum degree lower than −0.095 MPa. Knead the mixture for 2 h. Cool the mixture to room temperature, then add 3 parts of hydrogenated silicone oil with a hydrogen content of 0.6% and a viscosity of 60 mPa·s, and mix and disperse the mixture in a double planetary mixer at a stirring speed of 100 rpm / min, a dispersing speed of 800 rpm, and a stirring and dispersing time of 30 min. Then, add 0.1 parts of 3-methyl-1-butyn-3-ol, stir at a stirring speed of 100 rpm / min, a dispersing speed of 800 rpm, and a stirring and dispersing time of 30 min to obtain a mixed rubber material.
[0082] (3) Add 0.4 parts of platinum catalyst to the mixed rubber material by weight, mix and disperse it in a double planetary mixer at a stirring speed of 100 rpm / min and a dispersion speed of 800 rpm. Vacuum treatment is performed with a vacuum degree lower than -0.095 MPa for 30 minutes. The dispersed rubber material is placed in a vacuum filling glue barrel for a dispensing test.
[0083] The preparation process of the conductive microcapsules used in Comparative Example 2 is the same as that of Example 1.
[0084] Comparative Example 3:
[0085] (1) Add 15 parts by mass of vinyl silicone oil with a vinyl content of 0.8% and a viscosity of 1500 mPa·s, 3 parts of vinyl silicone resin with a viscosity of 20000 mPa·s, 1 part of anchoring agent, 2 parts of fumed silica and 6 parts of anhydrous ethanol to a kneader, knead and disperse at room temperature, turn on heating after the color is uniform, set the temperature at 150° C., knead for 3 hours, mix evenly, and grind with a three-roll mill after cooling to obtain a pre-dispersion liquid;
[0086] (2) Add 22 parts of silver carbon powder to the pre-dispersion liquid by weight, set the temperature at 120° C., evacuate the mixture, and make the vacuum degree lower than −0.095 MPa. The kneading time is 2 h. Cool the mixture to room temperature, then add 3 parts of hydrogen-containing silicone oil with a hydrogen content of 0.6% and a viscosity of 60 mPa·s, and mix and disperse the mixture in a double planetary mixer at a stirring speed of 100 rpm / min, a dispersing speed of 800 rpm, and a stirring and dispersing time of 30 min. Then, add 0.1 parts of 3-methyl-1-butyn-3-ol, stir at a speed of 100 rpm / min, a dispersing speed of 800 rpm, and a stirring and dispersing time of 30 min to obtain a mixed rubber material.
[0087] (3) Add 0.4 parts of platinum catalyst to the mixed rubber material by weight, mix and disperse it in a double planetary mixer at a stirring speed of 100 rpm / min and a dispersion speed of 800 rpm. Vacuum treatment is performed with a vacuum degree lower than -0.095 MPa for 30 minutes. The dispersed rubber material is placed in a vacuum filling glue barrel for a dispensing test.
[0088] The performance test results of the conductive silica gel obtained in Examples 1-5 and Comparative Examples 1-3 are shown in Table 1.
[0089] Table 1: Performance test results of conductive silica gel obtained in Examples 1-5 and Comparative Examples 1-3
[0090]
[0091]
[0092] As can be seen from Table 1, the conductive silicone without the addition of anchoring agent cracked under the conditions of 125°C and 1000h, and the bonding strength was low; the conductive silicone without the addition of fumed silica showed the phenomenon of rubber collapse and oil-powder separation; the self-prepared conductive microcapsules had lower volume resistivity and better shielding effectiveness than silver carbon powder.
[0093] In the description of this specification, the description with reference to the terms "one embodiment / method", "some embodiments / methods", "example", "specific example" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment / method or example are included in at least one embodiment / method or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment / method or example. Moreover, the specific features, structures, materials or characteristics described may be combined in a suitable manner in any one or more embodiments / methods or examples. In addition, those skilled in the art may combine and combine the different embodiments / methods or examples described in this specification and the features of the different embodiments / methods or examples, unless they are contradictory.
[0094] It should be noted that, in the present application, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of more restrictions, the elements defined by the sentence "comprise one..." do not exclude the existence of other identical elements in the process, method, article or equipment including the elements. In the present application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically stipulated.
[0095] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A strong bonding conductive silicone, characterized in that: The invention comprises the following raw materials in parts by weight: 6 to 20 parts of vinyl silicone oil, 2 to 5 parts of vinyl silicone resin, 2 to 5 parts of hydrogenated silicone oil, 1 to 3 parts of anchoring agent, 1 to 3 parts of thixotropic agent, 0.1 to 1 part of catalyst, 0.05 to 0.5 part of inhibitor, 5 to 10 parts of solvent and 20 to 40 parts of conductive microcapsules; wherein the shell material of the conductive microcapsules is silver and the core material is modified graphene oxide.
2. The strong bonding conductive silicone according to claim 1, characterized in that: The conductive microcapsules include the following raw materials in parts by mass: 5 to 20 parts of graphene oxide, 2 to 5 parts of 3-aminopropyltrimethoxysilane, 15 to 30 parts of silver nitrate, 10 to 20 parts of anhydrous ethanol, 10 to 20 parts of sodium citrate, 1 to 5 parts of sodium dodecylbenzene sulfonate, and 1 to 5 parts of polyvinyl alcohol.
3. The strong bonding conductive silicone according to claim 1, characterized in that: The structural formula of the anchoring agent is: In the formula, R is -CH3, R1 is -CH2CH3, and a=0 or 1.
4. The strong bonding conductive silicone according to claim 1, characterized in that: The thixotropic agent is at least one of fumed silica, polyethylene wax and organic bentonite.
5. The strong bonding conductive silicone according to claim 1, characterized in that: The catalyst is a platinum catalyst with a platinum content of 3000 to 5000 ppm.
6. The strong bonding conductive silicone according to claim 1, characterized in that: The inhibitor is at least one of 3-methyl-1-butyn-3-ol, 1-ethynylcyclohexanol, and 3,5-dimethyl-1-hexyn-3-ol.
7. The strong bonding conductive silicone according to claim 1, characterized in that: The solvent is at least one of silicone oil, PGMEA, anhydrous ethanol, ethylene glycol, ethyl ether, ethyl acetate, and low molecular weight silane.
8. The method for preparing the strong bonding conductive silicone according to any one of claims 1 to 7, characterized in that: The following steps are involved: S101, mixing vinyl silicone oil, vinyl silicone resin, anchoring agent, thixotropic agent and solvent to obtain a pre-dispersion liquid; S102, adding conductive microcapsules to the pre-dispersed liquid and mixing, and then sequentially adding hydrogenated silicone oil and an inhibitor and mixing evenly to obtain a mixed rubber material; S103, adding a catalyst to the mixed rubber material, stirring, vacuuming, filling, dispensing, and curing to obtain a strong bonding conductive silicone rubber.
9. The method for preparing the strong bonding conductive silicone according to claim 8, characterized in that: The conductive microcapsules are prepared by the following process: 3-aminopropyltrimethoxysilane is added to deionized water, and after stirring evenly, graphene oxide powder is added, stirring is continued until a uniform suspension is formed, and then modified graphene oxide is obtained by centrifugal separation; Adding silver nitrate into anhydrous ethanol and dissolving it to obtain an ethanol solution of silver nitrate; The modified graphene oxide is dispersed in deionized water, sodium dodecylbenzene sulfonate and polyvinyl alcohol are added, and then an ethanol solution of silver nitrate is added, and sodium citrate is slowly added while stirring, and the reaction mixture is freeze-dried to obtain conductive microcapsules.
10. The strong bonding conductive silicone described in any one of claims 1 to 7 or the strong bonding conductive silicone obtained by the method described in claims 8 to 9 is used for conductive bonding of liquid crystal displays, 5G communications, and electronic appliances.