High-thermal-conductivity two-component silica gel and preparation method thereof
High thermal conductivity two-component silicone gel was prepared by mixing methyl ethylene silicone rubber, foaming agent, catalyst, flame retardant powder and graphene with isocyanate and hydrogen-containing silicone oil in proportion, which solved the problems of poor thermal conductivity and long curing time. , achieving efficient construction and cost reduction.
Patent Information
- Application Number
- CN202411346435.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing two-component thermal conductivity of silicone has poor thermal conductivity, and the under-air molding and complete curing time is too long, which affects construction efficiency and is low in density.
Component A and component B are mixed in proportion. Component A includes methyl ethylene silicone rubber, foaming agent, catalyst, flame retardant powder and graphene. Component B includes isocyanate and hydrogen-containing silicone oil, by controlling the pre-reaction and Under reaction conditions, high thermal conductivity two-component silica gel was prepared.
It significantly improves the thermal conductivity, mechanical properties and electrical insulation properties of silicone, shortens the forming and curing time, improves construction efficiency, and reduces production costs.
Smart Images

Figure BDA0005061100410000131 
Figure BDA0005061100410000141
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermal conductive silicone, in particular to a high thermal conductive two-component silicone and a manufacturing method thereof. Background Art
[0002] Thermally conductive silicone is produced with a special formula, using metal oxides with good thermal conductivity and insulation and organic siloxane. Many mature thermally conductive silicone products have excellent thermal conductivity, good electrical insulation, a wide operating temperature, good stability, low viscosity and good construction performance, and are non-toxic, non-corrosive, odorless, non-drying and insoluble. Its main uses are: 1. Used as a heat transfer medium for electronic components; 2. Filling gaps and heat conduction between CPU and radiator; 3. Filling the gaps between high-power triodes and aluminum and copper substrates; 4. Filling the gaps between thyristor diodes and aluminum and copper substrates; 5. Reducing the operating temperature of various heating elements.
[0003] However, the two-component thermally conductive silicone in the prior art, such as a two-component high thermal conductivity room temperature curing silicone potting glue with patent publication number CN105482774A, has a thermal conductivity of only 1 to 2 W / (m·k), which cannot meet people's demand for high thermal conductivity. In addition, the molding time and complete curing time in air are too long, which affects the construction efficiency, and this will also reduce the density of the silicone. Summary of the invention
[0004] In order to overcome the problems of poor thermal conductivity, long molding time in air and long complete curing time of existing two-component thermal conductive silicone, the present invention provides a high thermal conductive two-component silicone and a preparation method. The high thermal conductive two-component silicone has the advantages of short molding time in air, short complete curing time, high fire resistance, high density, high thermal conductivity, high mechanical properties and high electrical insulation performance, which effectively improves the construction efficiency.
[0005] The technical solution of the present invention is as follows:
[0006] In a first aspect, the present invention provides a high thermal conductivity two-component silicone rubber, which is prepared by filling component A and component B into a two-component tube in proportion.
[0007] The raw materials of component A include: methyl vinyl silicone rubber, foaming agent, catalyst, flame retardant powder, thermal conductive powder and graphene;
[0008] The raw materials of the B component include: isocyanate, hydrogen-containing silicone oil and toner.
[0009] As a preferred embodiment of the present invention, the mass ratio of the component A to the component B is 1:1.
[0010] As a preferred embodiment of the present invention, the mass percentage ratio of each raw material in the component A is:
[0011] Methyl vinyl silicone rubber: 20-40%;
[0012] Foaming agent: 10-20%;
[0013] Catalyst: 5-10%;
[0014] Flame retardant powder: 10-20%;
[0015] Thermal conductive powder: 15-30%;
[0016] Graphene: 5-10%.
[0017] As a preferred embodiment of the present invention, the mass percentage ratio of each raw material in the B component is:
[0018] Isocyanate: 35-65%;
[0019] Hydrogenated silicone oil: 30-60%;
[0020] Toner: 5-15%.
[0021] As a preferred embodiment of the present invention, the flame retardant powder is one or a mixture of at least two of aluminum hydroxide, magnesium hydroxide, decabromodiphenyl ether and antimony oxide.
[0022] As a preferred embodiment of the present invention, the thermally conductive powder is iron oxide.
[0023] As a preferred embodiment of the present invention, the isocyanate is one or a mixture of at least two of toluene diisocyanate, pure MDI, carbodiimide-modified MDI, MDI-50 and polymeric MDI I.
[0024] In a second aspect, the present invention provides a method for preparing a high thermal conductivity two-component silica gel as in any of the above schemes, comprising the following steps:
[0025] Step S1, preparing component A: putting the methyl vinyl silicone rubber, the flame retardant powder, the thermal conductive powder and the graphene into a reaction kettle according to a ratio for premixing, and after premixing for 10 to 12 hours, sequentially adding the catalyst and the foaming agent according to a ratio and mixing for 1 to 2 hours;
[0026] Step S2, preparing component B: putting the isocyanate, the hydrogen-containing silicone oil and the color powder into a reaction kettle according to a proportion and mixing them for 2 to 3 hours;
[0027] Step S3, filling the component A and the component B into a two-component tube in proportion to obtain a high thermal conductivity two-component silicone.
[0028] As a preferred solution of the present invention, during the premixing process of the component A, the rotation speed of the reactor is 120-150 r / min, and after the premixing is completed, the rotation speed of the reactor is 180-220 r / min.
[0029] As a preferred solution of the present invention, during the preparation of the component B, the rotation speed of the reactor is 150-200 r / min.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] The present invention controls the pre-reaction of component A and the raw material ratio and reaction conditions of each raw material in component A and component B, so that the prepared high thermal conductivity two-component silicone has the advantages of short molding time under air, short complete curing time, high fire resistance level, high density, high thermal conductivity, high mechanical properties and high electrical insulation performance, effectively improves the construction efficiency, reduces the production cost, and expands the application scope of the thermal conductive silicone. DETAILED DESCRIPTION
[0032] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below.
[0033] It should be noted that the terms "including" and "having" and any variations thereof in the specification and claims of the present invention are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device including a series of steps or units is not limited to the listed steps or units, but may optionally include steps or units not listed, or may optionally include other steps or units inherent to these processes, methods, products or devices.
[0034] Example 1
[0035] The present invention provides a method for preparing a high thermal conductivity two-component silica gel, comprising the following steps:
[0036] Step S1, preparing component A: putting methyl vinyl silicone rubber, flame retardant powder, thermal conductive powder and graphene into a reactor according to a ratio for premixing, adding a catalyst and a foaming agent in sequence according to a ratio for 10 hours and mixing for 1 hour. During the premixing process of component A, the speed of the reactor is 150 r / min, and the speed of the reactor after the premixing is completed is 220 r / min;
[0037] Step S2, preparing component B: putting isocyanate, hydrogen-containing silicone oil and toner into a reaction kettle according to the proportion and mixing them for 2 hours, and the rotation speed of the reaction kettle is 200 r / min;
[0038] Step S3, filling component A and component B into a two-component tube at a mass ratio of 1:1 to prepare a two-component polyurethane foaming agent.
[0039] Among them, the mass percentage ratio of each raw material in component A is:
[0040] Methyl vinyl silicone rubber: 20%;
[0041] Foaming agent: 10%;
[0042] Catalyst: 10%;
[0043] Flame retardant powder: 20%;
[0044] Thermal conductive powder: 30%;
[0045] Graphene: 10%.
[0046] Methyl vinyl silicone rubber is the basic elastomer material in component A, providing good elasticity and toughness for the entire silicone system. Methyl vinyl silicone rubber has good high temperature resistance and can maintain stable physical and chemical properties under high temperature environment. Methyl vinyl silicone rubber also has good weather resistance and has good resistance to environmental factors such as ultraviolet rays and ozone, which can extend the service life of silicone.
[0047] The foaming agent can produce bubbles during the curing process of silicone, thereby adjusting the density and hardness of silicone. An appropriate amount of foaming agent can improve the processing properties of silicone, making it easier to shape and process.
[0048] The catalyst can accelerate the curing reaction between component A and component B, shorten the molding time and the complete curing time, and shorten the curing time helps to improve production efficiency and reduce production costs.
[0049] The addition of flame retardant powder can significantly improve the fire resistance level of silica gel, reduce the risk of fire, and inhibit the spread of flames during combustion, buying time for escape and fire fighting. Some flame retardant powders such as aluminum hydroxide and magnesium hydroxide are environmentally friendly and meet environmental protection requirements. Flame retardant powder is a mixture of one or at least two of aluminum hydroxide, magnesium hydroxide, decabromodiphenyl ether and antimony oxide.
[0050] Thermally conductive powder is iron oxide. As an inorganic thermally conductive filler, iron oxide has good thermal conductivity. Adding an appropriate amount of iron oxide to silica gel can form an effective thermal conductive network, allowing heat to be transferred more quickly, thereby improving the overall thermal conductivity of silica gel. Graphene is a material with extremely high thermal conductivity, and its thermal conductivity is much higher than that of traditional materials. Adding graphene to silica gel can further enhance the thermal conductive network, making the transfer of heat in silica gel more efficient, thereby significantly improving the thermal conductivity of silica gel. Iron oxide and graphene not only play a thermal conductive role in silica gel, but also have a synergistic effect between them. The high thermal conductivity of graphene can drive the heat transfer around the iron oxide particles, while the iron oxide particles can fix the graphene to a certain extent and prevent it from agglomerating, thereby maintaining the stability and continuity of the thermal conductive network. In addition to improving thermal conductivity, the addition of thermal conductive powder and graphene also has a positive effect on other properties of silica gel, such as mechanical properties and electrical insulation properties. This is because the addition of thermally conductive fillers can strengthen the skeleton structure of silicone and improve its mechanical properties such as tensile strength and compression resistance; at the same time, since the thermally conductive fillers themselves have good insulation properties, they can also improve the electrical insulation properties of silicone.
[0051] In addition, although aluminum oxide has higher thermal conductivity, iron oxide can also show good thermal conductivity under certain conditions. Especially when working in synergy with high-performance thermal conductive materials such as graphene, iron oxide can effectively improve the overall thermal conductivity of silicone. Compared with aluminum oxide, iron oxide may be more economical in the market, so using iron oxide as thermal conductive powder in the manufacturing process can reduce production costs and improve the market competitiveness of products.
[0052] Among them, the mass percentage ratio of each raw material in component B is:
[0053] Isocyanate: 35%;
[0054] Hydrogenated silicone oil: 60%;
[0055] Color powder: 5%.
[0056] Isocyanate is the main crosslinking agent in component B, which can react chemically with the silicone rubber in component A to form a crosslinked network structure. The formation of the crosslinked network can significantly enhance the mechanical properties and heat resistance of the silicone. Among them, the isocyanate is one or a mixture of at least two of toluene diisocyanate, pure MDI, carbodiimide modified MDI, MDI-50 and polymerized MDI I.
[0057] Hydrogenated silicone oil can adjust the curing speed of silicone, making it more controllable, and can improve the fluidity of silicone, making it easier to mix and shape.
[0058] Color powder is used to color silicone to meet different color requirements. When components A and B are mixed, the color powder can provide obvious color contrast to help determine whether the mixture is uniform.
[0059] Example 2
[0060] The present invention provides a method for preparing a high thermal conductivity two-component silica gel, comprising the following steps:
[0061] Step S1, preparing component A: putting methyl vinyl silicone rubber, flame retardant powder, thermal conductive powder and graphene into a reactor according to a ratio for premixing, adding a catalyst and a foaming agent in sequence according to a ratio for 10 to 12 hours after premixing, and mixing for 1 to 2 hours. During the premixing process of component A, the speed of the reactor is 120 to 150 r / min, and the speed of the reactor after the premixing is 180 to 220 r / min;
[0062] Step S2, preparing component B: putting isocyanate, hydrogen-containing silicone oil and toner into a reaction kettle according to a proportion and mixing them for 2 to 3 hours, and the rotation speed of the reaction kettle is 150 to 200 r / min;
[0063] Step S3, filling component A and component B into a two-component tube at a mass ratio of 1:1 to prepare a two-component polyurethane foaming agent.
[0064] Among them, the mass percentage ratio of each raw material in component A is:
[0065] Methyl vinyl silicone rubber: 40%;
[0066] Foaming agent: 20%;
[0067] Catalyst: 10%;
[0068] Flame retardant powder: 10%;
[0069] Thermal conductive powder: 15%;
[0070] Graphene: 5%.
[0071] Furthermore, the flame retardant powder is one or a mixture of at least two of aluminum hydroxide, magnesium hydroxide, decabromodiphenyl ether and antimony oxide.
[0072] Furthermore, the thermally conductive powder is iron oxide. Iron oxide, as an inorganic thermally conductive filler, has good thermal conductivity. Adding an appropriate amount of iron oxide to silica gel can form an effective thermal conductive network, so that heat can be transferred more quickly, thereby improving the overall thermal conductivity of silica gel. Graphene is a material with extremely high thermal conductivity, and its thermal conductivity is much higher than that of traditional materials. Adding graphene to silica gel can further enhance the thermal conductive network, making the transfer of heat in silica gel more efficient, thereby significantly improving the thermal conductivity of silica gel. Iron oxide and graphene not only play a thermal conductive role in silica gel, but also have a synergistic effect between them. The high thermal conductivity of graphene can drive the heat transfer around the iron oxide particles, while the iron oxide particles can fix the graphene to a certain extent and prevent it from agglomerating, thereby maintaining the stability and continuity of the thermal conductive network. In addition to improving thermal conductivity, the addition of thermally conductive powder and graphene also has a positive effect on other properties of silica gel, such as mechanical properties and electrical insulation properties. This is because the addition of thermally conductive fillers can strengthen the skeleton structure of silicone and improve its mechanical properties such as tensile strength and compression resistance; at the same time, since the thermally conductive fillers themselves have good insulation properties, they can also improve the electrical insulation properties of silicone.
[0073] In addition, although aluminum oxide has higher thermal conductivity, iron oxide can also show good thermal conductivity under certain conditions. Especially when working in synergy with high-performance thermal conductive materials such as graphene, iron oxide can effectively improve the overall thermal conductivity of silicone. Compared with aluminum oxide, iron oxide may be more economical in the market, so using iron oxide as thermal conductive powder in the manufacturing process can reduce production costs and improve the market competitiveness of products.
[0074] Among them, the mass percentage ratio of each raw material in component B is:
[0075] Isocyanate: 65%;
[0076] Hydrogenated silicone oil: 30%;
[0077] Color powder: 5%.
[0078] Furthermore, the isocyanate is one or a mixture of at least two of toluene diisocyanate, pure MDI, carbodiimide-modified MDI, MDI-50 and polymerized MDI I.
[0079] Example 3
[0080] The present invention provides a method for preparing a high thermal conductivity two-component silica gel, comprising the following steps:
[0081] Step S1, preparing component A: putting methyl vinyl silicone rubber, flame retardant powder, thermal conductive powder and graphene into a reactor according to a ratio for premixing, adding a catalyst and a foaming agent in sequence according to a ratio for 10 to 12 hours after premixing, and mixing for 1 to 2 hours. During the premixing process of component A, the speed of the reactor is 120 to 150 r / min, and the speed of the reactor after the premixing is 180 to 220 r / min;
[0082] Step S2, preparing component B: putting isocyanate, hydrogen-containing silicone oil and toner into a reaction kettle according to a proportion and mixing them for 2 to 3 hours, and the rotation speed of the reaction kettle is 150 to 200 r / min;
[0083] Step S3, filling component A and component B into a two-component tube at a mass ratio of 1:1 to prepare a two-component polyurethane foaming agent.
[0084] Among them, the mass percentage ratio of each raw material in component A is:
[0085] Methyl vinyl silicone rubber: 30%;
[0086] Foaming agent: 15%;
[0087] Catalyst: 8%;
[0088] Flame retardant powder: 15%;
[0089] Thermal conductive powder: 25%;
[0090] Graphene: 7%.
[0091] Furthermore, the flame retardant powder is one or a mixture of at least two of aluminum hydroxide, magnesium hydroxide, decabromodiphenyl ether and antimony oxide.
[0092] Furthermore, the thermally conductive powder is iron oxide. Iron oxide, as an inorganic thermally conductive filler, has good thermal conductivity. Adding an appropriate amount of iron oxide to silica gel can form an effective thermal conductive network, so that heat can be transferred more quickly, thereby improving the overall thermal conductivity of silica gel. Graphene is a material with extremely high thermal conductivity, and its thermal conductivity is much higher than that of traditional materials. Adding graphene to silica gel can further enhance the thermal conductive network, making the transfer of heat in silica gel more efficient, thereby significantly improving the thermal conductivity of silica gel. Iron oxide and graphene not only play a thermal conductive role in silica gel, but also have a synergistic effect between them. The high thermal conductivity of graphene can drive the heat transfer around the iron oxide particles, while the iron oxide particles can fix the graphene to a certain extent and prevent it from agglomerating, thereby maintaining the stability and continuity of the thermal conductive network. In addition to improving thermal conductivity, the addition of thermally conductive powder and graphene also has a positive effect on other properties of silica gel, such as mechanical properties and electrical insulation properties. This is because the addition of thermally conductive fillers can strengthen the skeleton structure of silicone and improve its mechanical properties such as tensile strength and compression resistance; at the same time, since the thermally conductive fillers themselves have good insulation properties, they can also improve the electrical insulation properties of silicone.
[0093] In addition, although aluminum oxide has higher thermal conductivity, iron oxide can also show good thermal conductivity under certain conditions. Especially when working in synergy with high-performance thermal conductive materials such as graphene, iron oxide can effectively improve the overall thermal conductivity of silicone. Compared with aluminum oxide, iron oxide may be more economical in the market, so using iron oxide as thermal conductive powder in the manufacturing process can reduce production costs and improve the market competitiveness of products.
[0094] Among them, the mass percentage ratio of each raw material in component B is:
[0095] Isocyanate: 50%;
[0096] Hydrogenated silicone oil: 35%;
[0097] Color powder: 15%.
[0098] Furthermore, the flame retardant powder is one or a mixture of at least two of aluminum hydroxide, magnesium hydroxide, decabromodiphenyl ether and antimony oxide.
[0099] Example 4
[0100] The present invention provides a method for preparing a high thermal conductivity two-component silica gel, comprising the following steps:
[0101] Step S1, preparing component A: putting methyl vinyl silicone rubber, flame retardant powder, thermal conductive powder and graphene into a reactor according to a ratio for premixing, adding a catalyst and a foaming agent in sequence according to a ratio for 10 to 12 hours after premixing, and mixing for 1 to 2 hours. During the premixing process of component A, the speed of the reactor is 120 to 150 r / min, and the speed of the reactor after the premixing is 180 to 220 r / min;
[0102] Step S2, preparing component B: putting isocyanate, hydrogen-containing silicone oil and toner into a reaction kettle according to a proportion and mixing them for 2 to 3 hours, and the rotation speed of the reaction kettle is 150 to 200 r / min;
[0103] Step S3, filling component A and component B into a two-component tube at a mass ratio of 1:1 to prepare a two-component polyurethane foaming agent.
[0104] Among them, the mass percentage ratio of each raw material in component A is:
[0105] Methyl vinyl silicone rubber: 30%;
[0106] Foaming agent: 10%;
[0107] Catalyst: 5%;
[0108] Flame retardant powder: 20%;
[0109] Thermal conductive powder: 30%;
[0110] Graphene: 5%.
[0111] Furthermore, the flame retardant powder is one or a mixture of at least two of aluminum hydroxide, magnesium hydroxide, decabromodiphenyl ether and antimony oxide.
[0112] Furthermore, the thermally conductive powder is iron oxide. Iron oxide, as an inorganic thermally conductive filler, has good thermal conductivity. Adding an appropriate amount of iron oxide to silica gel can form an effective thermal conductive network, so that heat can be transferred more quickly, thereby improving the overall thermal conductivity of silica gel. Graphene is a material with extremely high thermal conductivity, and its thermal conductivity is much higher than that of traditional materials. Adding graphene to silica gel can further enhance the thermal conductive network, making the transfer of heat in silica gel more efficient, thereby significantly improving the thermal conductivity of silica gel. Iron oxide and graphene not only play a thermal conductive role in silica gel, but also have a synergistic effect between them. The high thermal conductivity of graphene can drive the heat transfer around the iron oxide particles, while the iron oxide particles can fix the graphene to a certain extent and prevent it from agglomerating, thereby maintaining the stability and continuity of the thermal conductive network. In addition to improving thermal conductivity, the addition of thermally conductive powder and graphene also has a positive effect on other properties of silica gel, such as mechanical properties and electrical insulation properties. This is because the addition of thermally conductive fillers can strengthen the skeleton structure of silicone and improve its mechanical properties such as tensile strength and compression resistance; at the same time, since the thermally conductive fillers themselves have good insulation properties, they can also improve the electrical insulation properties of silicone.
[0113] In addition, although aluminum oxide has higher thermal conductivity, iron oxide can also show good thermal conductivity under certain conditions. Especially when working in synergy with high-performance thermal conductive materials such as graphene, iron oxide can effectively improve the overall thermal conductivity of silicone. Compared with aluminum oxide, iron oxide may be more economical in the market, so using iron oxide as thermal conductive powder in the manufacturing process can reduce production costs and improve the market competitiveness of products.
[0114] Among them, the mass percentage ratio of each raw material in component B is:
[0115] Isocyanate: 40%;
[0116] Hydrogenated silicone oil: 50%;
[0117] Color powder: 10%.
[0118] Furthermore, the isocyanate is one or a mixture of at least two of toluene diisocyanate, pure MDI, carbodiimide-modified MDI, MDI-50 and polymerized MDI I.
[0119] Furthermore, the flame retardant powder is one or a mixture of at least two of aluminum hydroxide, magnesium hydroxide, decabromodiphenyl ether and antimony oxide.
[0120] Example 5
[0121] The present invention provides a method for preparing a high thermal conductivity two-component silica gel, comprising the following steps:
[0122] Step S1, preparing component A: putting methyl vinyl silicone rubber, flame retardant powder, thermal conductive powder and graphene into a reactor according to a ratio for premixing, adding a catalyst and a foaming agent in sequence according to a ratio for 10 to 12 hours after premixing, and mixing for 1 to 2 hours. During the premixing process of component A, the speed of the reactor is 120 to 150 r / min, and the speed of the reactor after the premixing is 180 to 220 r / min;
[0123] Step S2, preparing component B: putting isocyanate, hydrogen-containing silicone oil and toner into a reaction kettle according to a proportion and mixing them for 2 to 3 hours, and the rotation speed of the reaction kettle is 150 to 200 r / min;
[0124] Step S3, filling component A and component B into a two-component tube at a mass ratio of 1:1 to prepare a two-component polyurethane foaming agent.
[0125] Among them, the mass percentage ratio of each raw material in component A is:
[0126] Methyl vinyl silicone rubber: 35%;
[0127] Foaming agent: 15%;
[0128] Catalyst: 10%;
[0129] Flame retardant powder: 15%;
[0130] Thermal conductive powder: 20%;
[0131] Graphene: 5%.
[0132] Furthermore, the flame retardant powder is one or a mixture of at least two of aluminum hydroxide, magnesium hydroxide, decabromodiphenyl ether and antimony oxide.
[0133] Furthermore, the thermally conductive powder is iron oxide. Iron oxide, as an inorganic thermally conductive filler, has good thermal conductivity. Adding an appropriate amount of iron oxide to silica gel can form an effective thermal conductive network, so that heat can be transferred more quickly, thereby improving the overall thermal conductivity of silica gel. Graphene is a material with extremely high thermal conductivity, and its thermal conductivity is much higher than that of traditional materials. Adding graphene to silica gel can further enhance the thermal conductive network, making the transfer of heat in silica gel more efficient, thereby significantly improving the thermal conductivity of silica gel. Iron oxide and graphene not only play a thermal conductive role in silica gel, but also have a synergistic effect between them. The high thermal conductivity of graphene can drive the heat transfer around the iron oxide particles, while the iron oxide particles can fix the graphene to a certain extent and prevent it from agglomerating, thereby maintaining the stability and continuity of the thermal conductive network. In addition to improving thermal conductivity, the addition of thermally conductive powder and graphene also has a positive effect on other properties of silica gel, such as mechanical properties and electrical insulation properties. This is because the addition of thermally conductive fillers can strengthen the skeleton structure of silicone and improve its mechanical properties such as tensile strength and compression resistance; at the same time, since the thermally conductive fillers themselves have good insulation properties, they can also improve the electrical insulation properties of silicone.
[0134] In addition, although aluminum oxide has higher thermal conductivity, iron oxide can also show good thermal conductivity under certain conditions. Especially when working in synergy with high-performance thermal conductive materials such as graphene, iron oxide can effectively improve the overall thermal conductivity of silicone. Compared with aluminum oxide, iron oxide may be more economical in the market, so using iron oxide as thermal conductive powder in the manufacturing process can reduce production costs and improve the market competitiveness of products.
[0135] Among them, the mass percentage ratio of each raw material in component B is:
[0136] Isocyanate: 50%;
[0137] Hydrogenated silicone oil: 40%;
[0138] Color powder: 10%.
[0139] Furthermore, the flame retardant powder is one or a mixture of at least two of aluminum hydroxide, magnesium hydroxide, decabromodiphenyl ether and antimony oxide.
[0140] Test case performance test
[0141] The high thermal conductivity two-component silicone rubber prepared in Examples 1-5 of the present invention was compared with the existing two-component thermal conductive silicone rubber in terms of performance test. The results are shown in Table 1.
[0142] Table 1 Performance test results
[0143]
[0144]
[0145] It can be seen from the above table that the high thermal conductivity two-component silicone rubber prepared in Examples 1-5 of the present invention has short molding time under air, short complete curing time, high fire resistance, high density, high thermal conductivity, high mechanical properties and high electrical insulation performance compared with the existing two-component polyurethane foaming agent, which effectively improves the construction efficiency, reduces the production cost, and expands the application scope of the thermal conductive silicone rubber, and is an ideal heat dissipation sealing material suitable for high-power components.
[0146] It should be understood that those skilled in the art can make improvements or changes based on the above description, and all these improvements and changes should fall within the scope of protection of the appended claims of the present invention.
[0147] The above is an exemplary description of the present invention. Obviously, the implementation of the present invention is not limited to the above method. As long as various improvements are made using the method concept and technical solution of the present invention, or the concept and technical solution of the present invention are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.
Claims
1. A high thermal conductivity two-component silicone, which is made by filling component A and component B into a two-component tube in proportion, characterized in that: The raw materials of component A include: methyl vinyl silicone rubber, foaming agent, catalyst, flame retardant powder, thermal conductive powder and graphene; The raw materials of the B component include: isocyanate, hydrogen-containing silicone oil and toner.
2. The high thermal conductivity two-component silicone according to claim 1, characterized in that: The mass ratio of the component A to the component B is 1:
1.
3. The high thermal conductivity two-component silicone according to claim 1, characterized in that: The mass percentage ratio of each raw material in the A component is: Methyl vinyl silicone rubber: 20-40%; Foaming agent: 10-20%; Catalyst: 5-10%; Flame retardant powder: 10-20%; Thermal conductive powder: 15-30%; Graphene: 5-10%.
4. The high thermal conductivity two-component silicone according to claim 3, characterized in that: The mass percentage ratio of each raw material in the B component is: Isocyanate: 35-65%; Hydrogenated silicone oil: 30-60%; Toner: 5-15%.
5. The high thermal conductivity two-component silicone according to claim 1, characterized in that: The flame retardant powder is one or a mixture of at least two of aluminum hydroxide, magnesium hydroxide, decabromodiphenyl ether and antimony oxide.
6. The high thermal conductivity two-component silicone rubber according to claim 1, characterized in that: The thermally conductive powder is iron oxide.
7. The high thermal conductivity two-component silicone rubber according to claim 1, characterized in that: The isocyanate is one or a mixture of at least two of toluene diisocyanate, pure MDI, carbodiimide-modified MDI, MDI-50 and polymerized MDI I.
8. A method for preparing the high thermal conductivity two-component silica gel according to any one of claims 1 to 7, characterized in that: The following steps are involved: Step S1, preparing component A: putting the methyl vinyl silicone rubber, the flame retardant powder, the thermal conductive powder and the graphene into a reaction kettle according to a ratio for premixing, and after premixing for 10 to 12 hours, sequentially adding the catalyst and the foaming agent according to a ratio and mixing for 1 to 2 hours; Step S2, preparing component B: putting isocyanate, hydrogen-containing silicone oil and color powder into a reaction kettle according to the proportion and mixing them for 2 to 3 hours; Step S3, filling the component A and the component B into a two-component tube in proportion to obtain a high thermal conductivity two-component silicone.
9. The method for preparing the high thermal conductivity two-component silica gel according to claim 8, characterized in that: During the premixing of the component A, the rotation speed of the reactor is 120-150 r / min, and after the premixing is completed, the rotation speed of the reactor is 180-220 r / min.
10. The method for preparing the high thermal conductivity two-component silica gel according to claim 8, characterized in that: During the preparation of the component B, the rotation speed of the reactor is 150-200 r / min.
Citation Information
Patent Citations
Double-component high-heat-conductivity room-curing organic silicon potting adhesive
CN105482774A
Graphene reinforced organic silicon heat-conductive material and preparation method thereof
CN104530706A
High thermal conductivity and high strength silicone rubber / graphene composite material and preparation method thereof
CN109651820A
High-thermal-conductivity two-component organic silicon pouring sealant and preparation method thereof
CN116622332A
Liquid-state bi-component fireproof flame-retardant sealing foaming agent and preparation method thereof
CN116813866A