An inorganic material modified organic thermal insulation material and preparation method thereof

By pre-embedding inorganic nanomaterials and hollow beads in organic foam insulation materials and adopting pretreatment and staged foaming processes, the problems of insufficient durability and fire resistance of organic insulation materials are solved, achieving an organic insulation material with Class A fire resistance and high durability while maintaining good insulation performance.

CN118085552BActive Publication Date: 2024-11-29PURUI ZHONGKE (SHANDONG) NEW MATERIAL TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410278515.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-12
Publication Date
2024-11-29
Estimated Expiration
2044-03-12

AI Technical Summary

Technical Problem

Existing organic thermal insulation materials have shortcomings in terms of durability, fire resistance, and waterproof performance, leading to increased building energy consumption and decreased comfort. Furthermore, inorganic nanomaterials are prone to agglomeration and segregation during the mixing process, which affects the performance improvement effect.

Method used

By pre-embedding inorganic nanomaterials and hollow beads in organic foam insulation materials, combined with pretreatment and staged foaming processes, the inorganic materials are ensured to be evenly distributed and form a flame-retardant and fireproof structure, thereby improving the durability and fire resistance of the materials. At the same time, the preparation method is optimized to maintain the insulation performance.

Benefits of technology

It achieves Class A fire resistance and high durability of organic thermal insulation materials, improves compressive, tensile, and flexural strength, prevents detachment and cracking, maintains sufficient thermal insulation performance, and makes reasonable use of the excellent properties of inorganic nanomaterials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004736730460000151
    Figure BDA0004736730460000151
  • Figure BDA0004736730460000161
    Figure BDA0004736730460000161
Patent Text Reader

Abstract

The present application provides an inorganic material modified organic thermal insulation material, comprising a foamed organic foam thermal insulation material matrix and an inorganic material, wherein the inorganic material is pre-embedded in the organic foam thermal insulation material matrix; the resin is polyurethane, phenolic resin or polystyrene resin; the inorganic material comprises nano-silicon dioxide, nano-aluminum oxide, nano-graphite, nano-aluminum hydroxide, nano-ferric oxide, nano-aerogel, nano-titanium dioxide, inorganic fiber, inorganic hollow beads, etc.; a preparation method of the inorganic material modified organic thermal insulation material is also provided, comprising foaming molding on a double-crawler laminator and foaming molding in a mold box; by adding the inorganic material, the organic thermal insulation material has thermal insulation performance that meets the standard, the thermal conductivity of the modified organic thermal insulation material is 0.022-0.028W / (m·K), and the fire protection grade is improved to Class A, the compressive strength, tensile strength, flexural strength and the like are increased, and the durability is extended.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of modified composite thermal insulation materials, in particular to an inorganic material modified organic thermal insulation material and a preparation method thereof. Background Art

[0002] Thermal insulation materials include inorganic thermal insulation materials and organic thermal insulation materials. Organic thermal insulation materials mainly include polyurethane rigid foam, EPS, XPS, phenolic foam, etc.

[0003] At present, with the economic and social development and scientific and technological progress, organic thermal insulation materials are required to have good thermal insulation performance, fire resistance closer to Class A (Class A includes Class A1 and Class A2), good waterproof performance, etc.

[0004] Assuming that the life of a building is designed to be 50 years, the corresponding insulation materials should also be extremely durable, and preferably have the same lifespan as the building; insulation materials with poor durability need to be replaced, and the environmental impact of the building will double; if they are not replaced, the building's energy loss will increase and the comfort level will decrease, which will obviously affect the overall environmental performance.

[0005] Therefore, how to optimize the formula and preparation method of organic thermal insulation materials so that the organic thermal insulation materials have higher thermal insulation performance and higher fire resistance, improve the durability, strength and other properties of organic thermal insulation materials, and prevent falling off, cracking, water seepage and other problems, is a technical problem that technical personnel in this field urgently need to solve. Summary of the invention

[0006] The object of the present invention is to provide an inorganic material modified organic thermal insulation material. Another object of the present invention is to provide a method for preparing an inorganic material modified organic thermal insulation material.

[0007] In order to solve the above technical problems, the technical solution provided by the present invention is:

[0008] An inorganic material-modified organic thermal insulation material, the organic thermal insulation material comprising a foamed organic foam thermal insulation material matrix and an inorganic material, wherein the inorganic material is pre-embedded in the organic foam thermal insulation material matrix;

[0009] The inorganic material comprises one or both of inorganic nanomaterials and inorganic hollow beads.

[0010] Preferably, the organic thermal insulation material is made by mixing and foaming a variety of raw materials including resin, inorganic material, foaming agent and auxiliary agent;

[0011] The resin is polyurethane, phenolic resin or polystyrene resin;

[0012] The organic foam insulation material matrix is ​​polyurethane rigid foam insulation material, phenolic foam insulation material or extruded polystyrene foam insulation material;

[0013] The inorganic nanomaterials include one, two or more of nano silicon dioxide powder, nano aluminum oxide powder, nano graphite powder, nano aluminum hydroxide powder, nano ferric oxide powder, nano aerogel powder, nano titanium dioxide powder and nano inorganic fiber;

[0014] The particle size of the inorganic nanomaterial is 1 nanometer to 150 nanometers;

[0015] The inorganic hollow beads include one or both of closed-pore vitrified microbeads and ceramic microbeads;

[0016] The mass percentage of the inorganic material to the mass percentage of the organic thermal insulation material is 5%-25%.

[0017] Preferably, a mesh is pre-embedded in the matrix of the organic foam thermal insulation material, the mesh is a metal mesh or an organic material mesh, and the mesh is a flat mesh or a mesh with tension bars.

[0018] Preferably, when the inorganic material only includes inorganic nanomaterials, the inorganic nanomaterials are pretreated before mixing the raw materials, specifically: different types of inorganic nanomaterials are stirred and mixed according to a ratio, then stirred and mixed while adding a binder, and then added into a ball making machine to make wet balls, the wet balls are spherical and have an outer diameter of 1cm-3cm, and then the wet balls are heated and dried. During the heating and drying process, the binder is solidified to bond and connect the nanoparticles of different types of inorganic nanomaterials together. After the heating and drying is completed, dry balls are obtained, and then the dry balls are crushed and ground. After the grinding is completed, inorganic material powder is obtained. The particle size of the inorganic material powder obtained by grinding is controlled to be 10 times to 20 times the particle size of the inorganic nanomaterial, and the particles of the inorganic material powder contain nanoparticles of different types of inorganic nanomaterials that are bonded and connected to each other.

[0019] Preferably, the modified organic thermal insulation material is a modified polyurethane rigid foam thermal insulation board, and the modified polyurethane mother liquor is prepared by uniformly mixing a plurality of raw materials, and the raw materials of the modified polyurethane mother liquor include 10-30 parts by mass of inorganic material, 40-80 parts by mass of polyether polyol, 5-25 parts by mass of foaming agent, 1-5 parts by mass of foam stabilizer, 0.5-5 parts by mass of catalyst, and 2-10 parts by mass of dispersant;

[0020] The raw materials of the modified polyurethane rigid foam insulation board include prepared modified polyurethane mother solution, 1-10 parts by weight of silicone oil, 120-200 parts by weight of isocyanate and 0.2-3 parts by weight of water.

[0021] Preferably, the modified organic thermal insulation material is a modified phenolic foam thermal insulation board, and the modified phenolic mother liquor is prepared by uniformly mixing a plurality of raw materials, wherein the raw materials of the modified phenolic mother liquor include 40-80 parts by mass of phenolic resin, 10-30 parts by mass of inorganic material, 5-15 parts by mass of curing agent, 1-5 parts by mass of zinc stearate, 5-15 parts by mass of phenolsulfonic acid, 2-5 parts by mass of lubricant, and 5-10 parts by mass of nitrile rubber;

[0022] The raw materials of the modified phenolic foam insulation board include modified phenolic mother liquor, 5-10 parts by weight of boric acid, 10-30 parts by weight of a foaming agent, and 0.5-5 parts by weight of a foam stabilizer, which are uniformly mixed.

[0023] The method for preparing an inorganic material-modified organic thermal insulation material as described in any one of the above comprises the following steps performed in sequence:

[0024] 1.1) Firstly prepare the ingredients, then stir and mix the raw materials evenly, and after the mixing is completed, a mixed slurry is obtained;

[0025] 1.2) The mixed slurry is sprayed by the nozzle of the foaming machine, and then foaming and laminating are performed on a double-crawler laminator, and then dried in a drying box, and then trimmed and cut in sequence to obtain a modified organic thermal insulation material.

[0026] The method for preparing an inorganic material-modified organic thermal insulation material as described in any one of the above comprises the following steps performed in sequence:

[0027] 2.1) Batching and mixing: first batch the ingredients, then stir and mix the raw materials evenly, and then obtain a mixed slurry;

[0028] 2.2) Mould box production: Use a foaming machine to inject the prepared mixed slurry into the mould box, then seal the mould box for foaming and curing, then let it rest, then demould, and then cut to obtain the modified organic thermal insulation material.

[0029] The method for preparing an inorganic material-modified organic thermal insulation material as described in any one of the above, when the inorganic material only includes inorganic nanomaterials, comprises the following steps performed in sequence:

[0030] 3.1) adding 10wt%-30wt% of the total resin and the total inorganic nanomaterials into a mold for open-cell foaming molding, and after completion, an open-cell foam material is obtained, so that all the inorganic nanomaterials are pre-embedded in the cell walls of the open-cell cells in the open-cell foam material;

[0031] 3.2) placing the prepared open-cell foam material into a mold box;

[0032] The remaining mass of resin, foaming agent and additives are stirred and mixed evenly to obtain a mixed slurry;

[0033] 3.3) Then, a foaming machine is used to pressurize the mixed slurry prepared in step 3.2) and inject it into a closed mold box. In the closed mold box, the mixed slurry is squeezed and flows into the cavities of the open-cell bubbles in the open-cell foam material. The mixed slurry fills all the cavities of the open-cell bubbles in the open-cell foam material. Then, the mixed slurry in the open-cell foam material is sequentially subjected to closed-cell foaming and curing. The mixed slurry in the cavities of the open-cell bubbles in the open-cell foam material is formed into hollow closed-cell bubbles through closed-cell foaming. After curing, the bubble walls of the open-cell bubbles located on the outside are formed to wrap the inner closed-cell bubbles. The structure of the hollow closed-cell bubbles on the side is then cured, demoulded, and cut. After completion, a modified organic thermal insulation material is obtained, so that the bubble wall containing inorganic nanomaterials in the open-cell bubbles on the outside forms a flame retardant and fireproof wall, and each open-cell bubble serves as a flame retardant and fireproof wall to wrap and cover the hollow closed-cell bubbles inside it. The flame retardant and fireproof wall provides flame retardant and fireproof protection to the hollow closed-cell bubbles inside it. The open-cell bubbles on the outside are used for flame retardancy and fire prevention, and the hollow closed-cell bubbles on the inside are used for heat preservation, forming a double-bubble superimposed and sheathed coating structure with flame retardancy and fire prevention on the outside and heat preservation on the inside.

[0034] Preferably, in step 3.3), the inner diameter of the cavity of the open-cell bubbles in the open-cell foam material is 500 μm to 5 mm.

[0035] The present application has achieved the following beneficial technical effects:

[0036] (1). The present application adds inorganic materials to organic resins such as polyurethane (PU) and phenolic resin (PF). Since the inorganic materials are inorganic flame retardant and fireproof materials, and the nanoparticles have excellent and unique nano properties, the modified organic thermal insulation material still has a qualified and sufficiently high thermal insulation performance, and the thermal insulation performance is not significantly reduced. The thermal conductivity of the modified organic thermal insulation material is 0.022-0.028W / (m·K), and the fire resistance level of the modified organic thermal insulation material is increased to Class A, and the compression, tensile, flexural and other strengths of the modified organic thermal insulation material are increased, and the durability of the modified organic thermal insulation material is improved;

[0037] (2) This application adds a mesh, and pre-buries a single mesh or a multi-layer mesh in the organic foam insulation material matrix, thereby improving the compression resistance, tensile strength, bending resistance, anti-falling, anti-cracking, and anti-water seepage properties of the modified organic insulation material. DETAILED DESCRIPTION

[0038] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only to further illustrate the features and advantages of the present invention, rather than to limit the claims of the present invention.

[0039] The present application provides an inorganic material-modified organic thermal insulation material, the organic thermal insulation material comprising a foamed organic foam thermal insulation material matrix and an inorganic material, wherein the inorganic material is pre-embedded in the organic foam thermal insulation material matrix;

[0040] The inorganic material comprises one or both of inorganic nanomaterials and inorganic hollow beads.

[0041] In one embodiment of the present application, the organic thermal insulation material is prepared by mixing and foaming a variety of raw materials including resin, inorganic material, foaming agent and auxiliary agent;

[0042] The resin is polyurethane, phenolic resin or polystyrene resin;

[0043] The organic foam insulation material matrix is ​​polyurethane rigid foam insulation material, phenolic foam insulation material or extruded polystyrene foam insulation material;

[0044] The inorganic nanomaterials include one, two or more of nano silicon dioxide powder, nano aluminum oxide powder, nano graphite powder, nano aluminum hydroxide powder, nano ferric oxide powder, nano aerogel powder, nano titanium dioxide powder and nano inorganic fiber;

[0045] The particle size of the inorganic nanomaterial is 1 nanometer to 150 nanometers;

[0046] The inorganic hollow beads include one or both of closed-pore vitrified microbeads and ceramic microbeads;

[0047] The mass percentage of the inorganic material to the mass percentage of the organic thermal insulation material is 5%-25%; preferably, all different kinds of inorganic materials are evenly distributed in the organic thermal insulation material, and the mass percentage of the inorganic material as a raw material is 5%-25%.

[0048] In one embodiment of the present application, a mesh is pre-embedded in the matrix of the organic foam thermal insulation material, the mesh is a metal mesh or an organic material mesh, and the mesh is a flat mesh or a mesh with tension bars.

[0049] In the present application, the addition of inorganic nanomaterials is mainly used to improve flame retardant and fireproof properties. Therefore, the inorganic nanomaterials are preferably not a single variety, but it is more reasonable to select multiple varieties (more than 3 varieties) for mixing. Multiple varieties of inorganic nanomaterials mixed in proportion will form a complementary and strong combination effect, thereby more significantly improving the above-mentioned flame retardant and fireproof properties;

[0050] However, there is a problem in actual production: currently, inorganic nanomaterials are directly mixed with other raw materials in proportion and then foamed. Although multiple inorganic nanomaterials are mixed according to the ratio at the macro level, and the ratio is correct and constant, at the micro level, after mixing, there may not be other nanoparticles or several nanoparticles near a certain nanoparticle, that is, at the micro level, all kinds of nanoparticles are unlikely to be grouped together according to the ratio, that is, at the micro level, there is a high probability that there is no ratio relationship between a certain nanoparticle and its neighboring nanoparticles as designed by the process. This results in a large deviation between the performance data of actual production and the theoretical design. The theoretical effect of multiple types of inorganic nanomaterials mixed in proportion to form a complementary and strong combination is weakened, which ultimately leads to a small increase in flame retardancy and fire resistance and other properties, which does not meet the expectations of the theoretical design.

[0051] To this end, in one embodiment of the present application, when the inorganic material includes and only includes inorganic nanomaterials, the inorganic nanomaterials are pretreated before mixing the raw materials, specifically: different types of inorganic nanomaterials are stirred and mixed according to a ratio, and then stirred and mixed while adding a binder, and then added into a ball making machine to make wet balls, the wet balls are spherical and have an outer diameter of 1cm-3cm, and then the wet balls are heated and dried (dried at a low temperature of 50°C-70°C), and the binder is solidified during the heating and drying process to bond and connect nanoparticles of different types of inorganic nanomaterials together, and dry balls are obtained after the heating and drying is completed, and then the dry balls are crushed and ground, and inorganic material powder is obtained after the grinding is completed, and the particle size of the inorganic material powder obtained by grinding is controlled to be 10 times to 20 times the particle size of the inorganic nanomaterial, and the particles of the inorganic material powder contain nanoparticles of different types of inorganic nanomaterials bonded to each other;

[0052] Here, preferably, the particle size of the large-particle inorganic material powder obtained by pretreatment is 500 nanometers to 2500 nanometers;

[0053] Here, the binder is preferably a liquid resin binder corresponding to the resin raw material, for example, when the resin in the organic thermal insulation material is polyurethane, the binder is a polyurethane adhesive, and when the resin in the organic thermal insulation material is phenolic resin, the binder is a phenolic adhesive;

[0054] Here, the pelletizing machine is preferably a disc pelletizing machine or a cylinder pelletizing machine;

[0055] Here, the pretreatment includes dry mixing, wet mixing, and ball-forming mixing in sequence, and since dry mixing is only stirring and mixing inorganic nanomaterials, and since the inorganic nanomaterials in wet mixing and ball-forming mixing are in large quantities while the binder is in small quantities, therefore, these three mixings obviously mix the different types of inorganic nanomaterials very evenly both macroscopically and microscopically according to the proportions, that is, at the microscopic level, all types of nanoparticles are likely to be clustered together according to the proportions, that is, at the microscopic level, a certain nanoparticle and its nearby nanoparticles are likely to form the proportion relationship designed by the above process, and then the nanoparticles are bonded to the nanoparticles nearby with the binder. The inorganic material powder is connected together, and then crushed and ground after drying to obtain large particles of 10-20 times the particle size. Due to the previous multiple mixing and bonding with a binder, most of the large particles of 10-20 times the particle size contain all kinds of nanoparticles that meet the proportion, that is, most of the large particles are a complete minimum unit at the microscopic level, so that multiple kinds of inorganic nanomaterials in the organic thermal insulation material are mixed in proportion at the macroscopic and microscopic levels, and the effect of complementary and strong combination is stronger and more obvious, thereby more significantly improving the flame retardant and fireproof properties;

[0056] The pretreatment also has an outstanding advantage: after the pretreated inorganic material powder is mixed with the resin and foamed to form the organic thermal insulation material, since the resin binder used in the pretreatment process is the same resin as the resin raw material in the organic thermal insulation material, the resin adhesive layer wrapped on the nanoparticles and the resin matrix in the organic thermal insulation material are similar substances of the same type, and therefore, there is no interface barrier problem between the resin adhesive layer wrapped on the nanoparticles and the resin matrix in the organic thermal insulation material when different materials are compounded. The resin adhesive layer and the resin matrix form a whole during the curing process, and there is no interface between the two. It is easier to form a whole and indistinguishable from each other, and finally significantly improves the strength, flame retardancy, fire resistance, durability and other properties of the inorganic material modified organic thermal insulation material;

[0057] Here, although the inorganic material powder obtained after pretreatment is large-particle with 10-20 times the particle size, which is not necessarily nanoparticle, the resin binder and the resin raw material are the same substance and are solidified into one, so the nanoparticles of the inorganic nanomaterial in the organic thermal insulation material are still in their original appearance, that is, nanoparticles. Therefore, the mixed foaming with the large particles after pretreatment does not weaken the excellent nano properties of the nanoparticles of the inorganic nanomaterial. The nanoparticles of the pretreated inorganic nanomaterial still maintain the original excellent nano properties, thereby continuing to improve the performance of the organic thermal insulation material with excellent nano properties.

[0058] In one embodiment of the present application, the modified organic thermal insulation material is a modified polyurethane rigid foam thermal insulation board, and the modified polyurethane mother liquor is prepared by uniformly mixing a plurality of raw materials, and the raw materials of the modified polyurethane mother liquor include 10-30 parts by mass of inorganic material, 40-80 parts by mass of polyether polyol, 5-25 parts by mass of foaming agent, 1-5 parts by mass of foam stabilizer, 0.5-5 parts by mass of catalyst, and 2-10 parts by mass of dispersant;

[0059] The raw materials of the modified polyurethane rigid foam insulation board include prepared modified polyurethane mother solution, 1-10 parts by weight of silicone oil, 120-200 parts by weight of isocyanate and 0.2-3 parts by weight of water.

[0060] In one embodiment of the present application, the modified organic thermal insulation material is a modified phenolic foam thermal insulation board, and the modified phenolic mother liquor is prepared by uniformly mixing a plurality of raw materials, and the raw materials of the modified phenolic mother liquor include 40-80 parts by mass of phenolic resin, 10-30 parts by mass of inorganic material, 5-15 parts by mass of curing agent, 1-5 parts by mass of zinc stearate, 5-15 parts by mass of phenol sulfonic acid, 2-5 parts by mass of lubricant, and 5-10 parts by mass of nitrile rubber;

[0061] The raw materials of the modified phenolic foam insulation board include modified phenolic mother liquor, 5-10 parts by weight of boric acid, 10-30 parts by weight of a foaming agent, and 0.5-5 parts by weight of a foam stabilizer, which are uniformly mixed.

[0062] In the present application, two mother liquors, a modified polyurethane mother liquor and a modified phenolic mother liquor, are provided. The main reason is that the particle size of the inorganic nanomaterial is too small and the amount added is too small, which leads to the problem that small and few nanoparticles are easily agglomerated, segregated, and unevenly mixed in a large amount of matrix material; here, the provision of the mother liquor is essentially to pre-mix the inorganic nanomaterial in a part of the liquid raw materials, which is a premix. The raw materials of the mother liquor are selected after theoretical design and experimental verification. The raw materials of the mother liquor themselves make it easier to mix with the nanoparticles, and then the mother liquor is stirred and mixed with the remaining raw materials, thereby improving the mixing uniformity of the inorganic nanomaterial in the entire matrix.

[0063] The present application also provides a method for preparing the above-mentioned inorganic material-modified organic thermal insulation material, comprising the following steps performed in sequence:

[0064] 1.1) Firstly prepare the ingredients, then stir and mix the raw materials evenly, and after the mixing is completed, a mixed slurry is obtained;

[0065] 1.2) The mixed slurry is sprayed by the nozzle of a foaming machine (including a single-component foaming machine or a two-component foaming machine), and then foaming and laminating are performed on a double-crawler laminator, and then dried in a drying box, and then trimmed and cut in sequence to obtain a modified organic thermal insulation material.

[0066] The present application also provides a method for preparing the above-mentioned inorganic material-modified organic thermal insulation material, comprising the following steps performed in sequence:

[0067] 2.1) Batching and mixing: first batch the ingredients, then stir and mix the raw materials evenly, and then obtain a mixed slurry;

[0068] 2.2) Mould box production: Use a foaming machine (including a single-component foaming machine or a two-component foaming machine) to inject the prepared mixed slurry into the mould box, then seal the mould box for foaming and curing, then let it rest (static storage and curing), then demould, then cut, and after completion, a modified organic thermal insulation material is obtained.

[0069] In the present application, an inorganic material-modified organic thermal insulation material is provided. Therefore, the main body is still an organic foam thermal insulation material matrix, the organic foam thermal insulation material matrix is ​​still in large quantity, and the inorganic nanomaterial is in small quantity. The inorganic nanomaterial is added because the nanoparticles have many excellent and unique nano properties. However, there is also a problem that has always existed: because the particle size of the nanoparticles is too small and the amount added is relatively small, the small and small nanoparticles are prone to agglomeration, segregation, and uneven mixing in a large amount of matrix materials. It is not that the inorganic nanomaterials are added and then stirred and mixed for a period of time, and the mixture can be mixed evenly. It is difficult to achieve uniform mixing in actual production, and the mixing uniformity in actual production is low.

[0070] Furthermore, although adding inorganic nanomaterials will improve the fireproof level, it will significantly reduce the thermal insulation performance at the same time. Therefore, this is a contradiction. Therefore, in order to give priority to keeping the basic thermal insulation performance of organic thermal insulation materials up to standard and not reduced, and because the production of inorganic nanomaterials is complicated and the price is very high, the amount of inorganic nanomaterials added is limited and cannot be added too much. The current production method of mixing inorganic nanomaterials with other raw materials and then foaming and pouring them into shape is similar to the more water-scarce and wasteful flooding of the land for a small amount of precious inorganic nanomaterials, and it causes "dispersion of troops and lack of concentration of troops", similar to 1,000 soldiers defending the area of ​​a province, 1,000 soldiers are dispersed in 50 cities, and each city is assigned 10-30 soldiers to station. The number of soldiers in each city is too small to effectively defend the city, and the defense effect is weak, that is, the limited and precious inorganic nanomaterial resources are wasted, not reasonably utilized, and not really play their role. Technical problems;

[0071] To this end, in the present application, a method for preparing an inorganic material-modified organic thermal insulation material, when the inorganic material includes and only includes an inorganic nanomaterial, comprises the following steps performed in sequence:

[0072] 3.1) adding 10wt%-30wt% of the total resin, the total inorganic nanomaterials, the foaming agent, the cell-opening agent and the remaining types of additives into a mold for open-cell foaming molding, and after completion, an open-cell foam material is obtained, so that all the inorganic nanomaterials are pre-embedded in the cell walls of the open-cell cells in the open-cell foam material;

[0073] 3.2) placing the prepared open-cell foam material into a mold box;

[0074] The remaining mass of resin, foaming agent and additives are stirred and mixed evenly to obtain a mixed slurry;

[0075] 3.3) Then, a foaming machine is used to pressurize and inject the mixed slurry prepared in step 3.2) into a closed mold box, in which the mixed slurry is squeezed and flows into the cavities of the open-cell bubbles in the open-cell foam material, and the mixed slurry fills all the cavities of the open-cell bubbles in the open-cell foam material, and then the mixed slurry in the open-cell foam material is sequentially subjected to closed-cell foaming and curing, and the mixed slurry in the cavities of the open-cell bubbles in the open-cell foam material is formed into hollow closed-cell bubbles by closed-cell foaming, and after curing, a structure is formed in which the bubble walls of the open-cell bubbles located on the outside wrap around the outer bubbles of the hollow closed-cell bubbles located on the inside, and the outer bubbles wrap around the inner bubbles, and then the mixture is allowed to rest, demolded, and cut, and after completion, a modified organic thermal insulation material is obtained;

[0076] Preferably, in step 3.3), the inner diameter of the cavity of the open-cell bubble in the open-cell foam material (the cavity inside each open-cell bubble) is 500 μm to 5 mm, preferably 1 mm to 5 mm;

[0077] Here, the present application carries out foaming molding twice in total, the former is open-cell foaming molding, and the latter is closed-cell foaming molding. The open-cell foam material formed by the open-cell foaming molding has its cell walls pre-embedded with all inorganic nanomaterials, while the closed-cell foam material formed by the closed-cell foaming molding does not contain any inorganic nanomaterials in its closed-cell cell walls, so that the cell walls of the open-cell bubbles formed later on the outside wrap around the hollow closed-cell bubbles on the inside. The cell walls of the open-cell bubbles on the outside contain all the inorganic nanomaterials to form a flame-retardant fireproof wall, which wraps and covers the hollow closed-cell bubbles therein, thereby the flame-retardant fireproof wall protects the hollow closed-cell bubbles inside. The open-cell foam is flame-retardant and fire-proofed, just like a flame-retardant and fire-proof protective cover is put on the outside of the hollow closed-cell foam used for heat preservation, that is, each open-cell foam is used as a flame-retardant and fire-proof wall to protect one, two or more hollow closed-cell foams. The open-cell foam located on the outside is mainly used for flame-retardant and fire-proofing and has relatively low heat preservation performance, and the hollow closed-cell foam located on the inside is mainly used for high heat preservation, forming a double-bubble superimposed and sheathed coating structure with outer main flame-retardant and fireproofing and inner main heat preservation, thereby optimizing the internal structure and preparation method of the organic heat preservation material, ensuring that the organic heat preservation material has a sufficiently high heat preservation performance that meets the standard, and the heat preservation performance is not reduced, and the fireproof performance is significantly improved to Class A fireproof performance;

[0078] Furthermore, the present application only selects 10wt%-30wt% (mass percentage) of the resin and all the inorganic nanomaterials from the whole resin to manufacture the open-cell foam material. For the nanoparticles with too small particle size and too little addition, the mass of the resin here is obviously much less. At this time, the resin and the inorganic nanomaterial are stirred and mixed. Since the mass of the resin is obviously much less, the resin and the inorganic nanomaterial can be stirred and mixed more easily to achieve a higher mixing uniformity. It has been verified in actual production that the mixing uniformity has been significantly improved.

[0079] Furthermore, all the inorganic nanomaterials in the present application are distributed in the cell walls of the open-cell foam material, and all the inorganic nanomaterials are not distributed in the entire organic thermal insulation material as described above, that is, the inorganic nanomaterials used for flame retardancy and fire prevention are all concentrated in the cell walls of the open-cell foam used as a flame retardant and fireproof cover, realizing "special materials for special purposes", "good steel is used on the blade", and "concentrating troops to prevent troops from being dispersed", similar to the water-saving drip irrigation technology in arid areas, making full and reasonable use of a small amount of water resources to concentrate water only on the roots of plants, instead of using limited water resources for large-scale flooding, thus achieving limited and precious inorganic nanomaterial resources are no longer wasted, are reasonably utilized, and truly play the role of flame retardancy and fire prevention.

[0080] The present application provides an inorganic material modified organic thermal insulation material, which is made by mixing and foaming a variety of raw materials, the raw materials including 40-200 parts by mass of resin, 10-30 parts by mass of inorganic material, 5-30 parts by mass of foaming agent, 5-40 parts by mass of auxiliary agents (auxiliary agents include 3-20 parts by mass of curing agent, 0.5-5 parts by mass of foam stabilizer, etc.).

[0081] In the present application, the resin is an organic resin such as polyurethane, phenolic resin or polystyrene resin;

[0082] The organic foam insulation material matrix is ​​a polyurethane rigid foam insulation material, a phenolic foam insulation material or an extruded polystyrene foam insulation material. The formula and preparation method of the polyurethane rigid foam insulation material, the phenolic foam insulation material or the extruded polystyrene foam insulation material are well known to those skilled in the art and will not be described in detail here.

[0083] The excellent and unique nano properties of inorganic nanomaterials are: it has volume effect, surface effect, small size effect and macro quantum tunneling effect, etc. When the macroscopic object is subdivided into ultrafine particles (nanoscale), it will show many unique characteristics, that is, its optical, thermal, electrical, magnetic, mechanical and chemical properties will be significantly different from those of large solids. For example, nano silicon dioxide is an inorganic chemical material, commonly known as white carbon black. Because it is ultrafine nanoscale with a size range of 1-100nm, it has many unique properties, such as optical properties against ultraviolet rays, and can improve the material's anti-aging, strength and chemical resistance, etc.

[0084] In the present application, because the thermal conductivity of inorganic materials is relatively low and the combustion grade is Class A, the role of inorganic materials is mainly to keep the thermal conductivity of organic thermal insulation materials from increasing, so that it can achieve sufficient thermal insulation performance, and at the same time improve the fire resistance grade of organic thermal insulation materials to Class A (A2); and because the particle size of inorganic materials is small enough, the nanoparticles have many special properties in terms of structure, physics and chemical properties.

[0085] The main innovations of this application are: (1) The organic resin raw material is a low thermal conductivity resin material such as polyurethane (PU), phenolic resin (PF) or polystyrene resin;

[0086] (2) The added inorganic materials include: nano-aerogel powder, nano-silicon dioxide powder, nano-graphene powder, glass microspheres, inorganic hollow beads, nano-titanium dioxide powder, nano-inorganic fibers and other low thermal conductivity inorganic materials;

[0087] (3) The mesh includes: single flat mesh, mesh with ribs or multi-layer mesh, made of metal and organic material mesh, metal mesh (metal mesh with anti-corrosion treatment such as hot-dip galvanizing, cold-dip galvanizing, carbon black, fluorocarbon, etc.) and organic material mesh (PVC, PC, PE, ABS, PET or PS mesh, etc.);

[0088] (4) Lay cement-based cloth or alkali-resistant mesh cloth on the two length and width surfaces of the modified organic insulation material plate;

[0089] (5) Spreading inorganic slurry or composite inorganic sheet on the two length and width surfaces of the modified organic insulation material sheet;

[0090] (6). Preparation method 1: double-track heated double-track curing laminator → laying cement-based cloth (or alkali-resistant mesh cloth) → laying mesh → spraying mixed slurry by foaming machine → laying cement-based cloth (or alkali-resistant mesh cloth) → foaming → foaming and curing by double-track curing laminator → entering high-temperature channel (adjustable temperature drying box) → band saw cutting → trimming → automatic palletizing → finished product packaging → storage; (In this preparation method: using release agent instead of cement-based cloth or alkali-resistant mesh cloth, it is possible to directly produce panels with or without mesh);

[0091] (7). Preparation method 2: mold box production process, after placing the mesh in the mold box, add the prepared mixed slurry, then seal and solidify, and cut and package according to design requirements; mesh placed in the mold box - inject mixed slurry into the mold box - seal and solidify - let stand (can be heated) - demoulding - cutting - packaging - storage; mold box size: width 400-1250mm, length 1200-3100mm, height 600-1500mm, the mold box size can be adjusted at will; mesh: multi-layer mesh is tied in advance according to design requirements; product size: cut according to design requirements.

[0092] In the present application, the organic thermal insulation material is usually a foam material, also known as microporous plastic, which is a plastic that is covered with countless interconnected or unconnected micropores to significantly reduce the apparent density. It has the advantages of light weight, heat insulation, sound absorption, shock resistance, moisture resistance, corrosion resistance, etc.; according to its pore structure, it can be divided into closed-cell, open-cell and reticulated foam plastics. All the pores in closed-cell foam plastics are almost unconnected, and all the pores in open-cell foam plastics are almost connected. Foam plastics with almost no cell walls are called reticulated foam plastics; according to the density of foam plastics, it can be divided into low-foaming, medium-foaming and high-foaming foam plastics, and the density is greater than 0.4g / cm 3 It is low foaming plastic with a density of 0.1-0.4g / cm 3 The foam is medium foam plastic with a density less than 0.1g / cm 3The most common ones are high-foaming foam plastics; common traditional foam plastics include polyurethane (PUR), polystyrene (PS), polyvinyl chloride (PVC), polyethylene (PE), phenolic resin (PF) and other varieties.

[0093] In this application, polyurethane rigid foam insulation material is a rigid foam plastic with waterproof and thermal insulation functions formed by the foaming reaction of component A and component B, which is called polyurethane rigid foam, or polyurethane rigid foam for short; component A refers to a combination of polyols (combined polyethers or polyesters) and additives such as foaming agents, commonly known as white materials; component B refers to a raw material whose main component is isocyanate, commonly known as black material. In this application, isocyanate is preferably polyphenyl polymethylene polyisocyanate, or PAPI for short, or crude MDI.

[0094] In the present application, the phenolic foam insulation material is referred to as phenolic foam for short, which is a closed-cell rigid foam plastic made by mixing and foaming a variety of substances such as phenolic resin and flame retardants, smoke suppressants, curing agents, foaming agents and other additives.

[0095] In the present application, a foaming agent and a cell opening agent are required in the open-cell foaming molding, wherein the cell opening agent is a special type of surfactant, generally containing hydrophobic and hydrophilic chain segments as groups, and its function is to reduce the surface tension of the foam, promote the rupture of the cells, and increase the open-cell foaming rate of the foam plastic; the formula and preparation method of the open-cell foaming molding here are well known to technicians in this field and will not be repeated here.

[0096] The present invention has no limitation on the processing equipment and process parameters not mentioned in the above method, and the processing equipment and process parameters well known to those skilled in the art can be used.

[0097] In order to further understand the present invention, an inorganic material-modified organic thermal insulation material and a preparation method thereof provided by the present invention are described in detail below in conjunction with embodiments. The protection scope of the present invention is not limited by the following embodiments.

[0098] Example 1

[0099] An inorganic material-modified organic thermal insulation material, wherein the modified organic thermal insulation material is a modified polyurethane rigid foam thermal insulation board, wherein the modified polyurethane mother liquor is prepared by uniformly mixing a plurality of raw materials, wherein the raw materials of the modified polyurethane mother liquor include 20 parts by mass of an inorganic material, 60 parts by mass of a polyether polyol, 14 parts by mass of a foaming agent, 2 parts by mass of a foam stabilizer, 1 part by mass of a catalyst, and 3 parts by mass of a dispersant;

[0100] The raw materials of the modified polyurethane rigid foam insulation board include the modified polyurethane mother solution uniformly mixed as above, 3 parts by mass of silicone oil, 140 parts by mass of isocyanate, 5 parts by mass of curing agent (triethanolamine), and 1 part by mass of water;

[0101] The inorganic materials include nano silicon dioxide powder, nano aluminum oxide powder, nano aluminum hydroxide powder, nano silicon dioxide aerogel powder and nano titanium dioxide powder; all different kinds of inorganic materials are evenly distributed in the organic thermal insulation material in terms of the mass fraction of the inorganic material; the particle size of the inorganic material is 50 nanometers to 90 nanometers.

[0102] The method for preparing an inorganic material-modified organic thermal insulation material in the above embodiment 1 comprises the following steps performed in sequence:

[0103] 1.1) Batching and mixing: first batch the ingredients, then stir and mix the raw materials evenly, and then obtain a mixed slurry;

[0104] 1.2) The mixed slurry is sprayed by the nozzle of a two-component foaming machine, and then foaming and laminating are performed on a double-crawler laminator, and then dried in a drying box, and then trimmed and cut in sequence to obtain a modified organic thermal insulation material.

[0105] Table 1 Performance test data of modified polyurethane rigid foam insulation board prepared in Example 1

[0106] project unit Performance Indicators density <![CDATA[kg / m 3 ]]> 105 Tensile strength perpendicular to the board surface MPa 0.15 Compressive strength MPa 0.20 Thermal conductivity W / (m·K) 0.026 Water absorption % ≤3 Combustion performance grade A2

[0107] Example 2

[0108] An inorganic material-modified organic thermal insulation material, wherein the modified organic thermal insulation material is a modified phenolic foam thermal insulation board, wherein the modified phenolic mother liquor is prepared by uniformly mixing a plurality of raw materials, wherein the raw materials of the modified phenolic mother liquor include 65 parts by mass of phenolic resin, 15 parts by mass of inorganic material, 5 parts by mass of a curing agent (hexamethylenetetramine), 2 parts by mass of zinc stearate, 5 parts by mass of phenolsulfonic acid, 3 parts by mass of a lubricant, and 5 parts by mass of nitrile rubber;

[0109] The raw materials of the modified phenolic foam insulation board include the modified phenolic mother solution prepared by uniformly mixing the above, 5 parts by mass of boric acid, 15 parts by mass of a foaming agent, and 2 parts by mass of a silicone foam stabilizer;

[0110] The inorganic materials include nano silicon dioxide powder, nano aluminum oxide powder, nano silicon dioxide aerogel powder and nano titanium dioxide powder. All different kinds of inorganic materials are evenly distributed in the organic thermal insulation material in terms of the mass fraction of the inorganic material. The particle size of the inorganic material is 50 to 90 nanometers.

[0111] The method for preparing an inorganic material-modified organic thermal insulation material of the above embodiment 2 comprises the following steps performed in sequence:

[0112] 3.1) The inorganic nanomaterials are pretreated before the raw materials are mixed, specifically: different types of inorganic nanomaterials are stirred and mixed according to a ratio, and then a binder is added while stirring and mixing, and then the materials are added into a pelletizer to make wet balls, the wet balls are spherical and have an outer diameter of 2cm-3cm, and then the wet balls are heated and dried, and the binder is solidified during the heating and drying process to bond and connect the nanoparticles of different types of inorganic nanomaterials together, and dry balls are obtained after the heating and drying, and then the dry balls are crushed and ground, and inorganic material powder is obtained after the grinding, and the particle size of the inorganic material powder obtained by the grinding is controlled to be 12 times to 16 times the particle size of the inorganic nanomaterial, and the particles of the inorganic material powder contain nanoparticles of different types of inorganic nanomaterials bonded to each other;

[0113] Then, 25wt% of the whole phenolic resin, all the pretreated inorganic material powders, a foaming agent, a cell-opening agent and the remaining types of auxiliary agents are added into a mold for open-cell foaming molding, and an open-cell foam material is obtained after curing, so that all the inorganic material powders are pre-embedded in the cell walls of the open-cell cells in the open-cell foam material;

[0114] 3.2) placing the prepared open-cell foam material into a mold box;

[0115] The remaining mass of phenolic resin, foaming agent and auxiliary agent are stirred and mixed uniformly to obtain a mixed slurry;

[0116] 3.3) Then, a foaming machine is used to pressurize and inject the mixed slurry prepared in step 3.2) into a closed mold box, in which the mixed slurry is squeezed and flows into the cavities of the open-cell bubbles in the open-cell foam material, and the mixed slurry fills all the cavities of the open-cell bubbles in the open-cell foam material, and then the mixed slurry in the open-cell foam material is sequentially subjected to closed-cell foaming and curing, and the mixed slurry in the cavities of the open-cell bubbles in the open-cell foam material is formed into hollow closed-cell bubbles by closed-cell foaming, and after curing, a structure is formed in which the bubble walls of the open-cell bubbles located on the outside wrap around the hollow closed-cell bubbles located on the inside, and then the mixture is allowed to rest, then demolded, and then cut, and after completion, a modified organic thermal insulation material is obtained;

[0117] In step 3.3), the inner diameter of the cavity of the open-cell bubbles in the open-cell foam material is 4 mm to 5 mm.

[0118] Table 2 Performance test data of modified phenolic foam insulation board prepared in Example 2

[0119]

[0120]

[0121] The above embodiments are only used to help understand the method and core idea of ​​the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

Claims

1. An inorganic material modified organic thermal insulation material, characterized in that: The organic thermal insulation material comprises a foamed organic foam thermal insulation material matrix and an inorganic material, wherein the inorganic material is pre-embedded in the organic foam thermal insulation material matrix; The inorganic material is an inorganic nanomaterial; The inorganic nanomaterials include nano silicon dioxide powder, nano aluminum oxide powder, nano graphite powder, nano aluminum hydroxide powder, nano ferric oxide powder, nano aerogel powder, nano titanium dioxide powder, and nano inorganic fiber. The particle size of the inorganic nanomaterial is 1 nanometer to 150 nanometers; The mass of the inorganic material accounts for 5%-25% of the mass of the organic thermal insulation material; Before mixing the raw materials, the inorganic nanomaterials are pretreated, specifically: different types of inorganic nanomaterials are stirred and mixed according to a ratio, then a binder is added while stirring and mixing, and then the materials are added into a ball-making machine to make wet balls, the wet balls are spherical and have an outer diameter of 1cm-3cm, and then the wet balls are heated and dried. During the heating and drying process, the binder is solidified to bond and connect the nanoparticles of different types of inorganic nanomaterials together. After the heating and drying is completed, dry balls are obtained, and then the dry balls are crushed and ground. After the grinding is completed, inorganic material powder is obtained. The particle size of the inorganic material powder obtained by grinding is controlled to be 10 times to 20 times the particle size of the inorganic nanomaterial, and the particles of the inorganic material powder contain nanoparticles of different types of inorganic nanomaterials that are bonded and connected to each other.

2. The inorganic material-modified organic thermal insulation material according to claim 1, characterized in that: The organic thermal insulation material is made by mixing and foaming a variety of raw materials including resin, inorganic material, foaming agent and auxiliary agent; The resin is polyurethane, phenolic resin or polystyrene resin; The organic foam thermal insulation material matrix is ​​polyurethane rigid foam thermal insulation material, phenolic foam thermal insulation material or extruded polystyrene foam thermal insulation material.

3. The inorganic material-modified organic thermal insulation material according to claim 1, characterized in that: A mesh is pre-buried in the matrix of the organic foam thermal insulation material. The mesh is a metal mesh or an organic material mesh. The mesh is a flat mesh or a mesh with tension bars.

4. The inorganic material-modified organic thermal insulation material according to claim 1, characterized in that: The modified organic thermal insulation material is a modified polyurethane rigid foam thermal insulation board, and the raw materials of the modified polyurethane rigid foam thermal insulation board include a prepared modified polyurethane mother solution, 1-10 parts by weight of silicone oil, 120-200 parts by weight of isocyanate, and 0.2-3 parts by weight of water; The modified polyurethane mother liquor is prepared by uniformly mixing a variety of raw materials, and the raw materials of the modified polyurethane mother liquor include 10-30 parts by mass of inorganic materials, 40-80 parts by mass of polyether polyols, 5-25 parts by mass of foaming agents, 1-5 parts by mass of foam stabilizers, 0.5-5 parts by mass of catalysts, and 2-10 parts by mass of dispersants.

5. The inorganic material-modified organic thermal insulation material according to claim 1, characterized in that: The modified organic thermal insulation material is a modified phenolic foam thermal insulation board, and the raw materials of the modified phenolic foam thermal insulation board include a modified phenolic mother liquid, 5-10 parts by weight of boric acid, 10-30 parts by weight of a foaming agent, and 0.5-5 parts by weight of a foam stabilizer prepared by mixing uniformly; The modified phenolic mother liquor is prepared by uniformly mixing a plurality of raw materials, wherein the raw materials of the modified phenolic mother liquor include 40-80 parts by weight of phenolic resin, 10-30 parts by weight of inorganic material, 5-15 parts by weight of curing agent, 1-5 parts by weight of zinc stearate, 5-15 parts by weight of phenol sulfonic acid, 2-5 parts by weight of lubricant and 5-10 parts by weight of nitrile rubber.

6. The method for preparing an inorganic material-modified organic thermal insulation material according to any one of claims 1 to 5, characterized in that: The method includes the following steps: 1.1) Firstly, the ingredients are prepared, and then the raw materials are stirred and mixed evenly, and after the mixing is completed, a mixed slurry is obtained; 1.2) The mixed slurry is sprayed by the nozzle of the foaming machine, and then foaming and laminating are performed on a double-crawler laminator, and then dried in a drying box, and then trimmed and cut in sequence to obtain a modified organic thermal insulation material.

7. The method for preparing an inorganic material-modified organic thermal insulation material according to any one of claims 1 to 5, characterized in that: The method includes the following steps: 2.1) Batching and mixing: first batch the ingredients, then stir and mix the raw materials evenly, and then prepare a mixed slurry; 2.2) Mould box production: Use a foaming machine to inject the prepared mixed slurry into the mould box, then seal the mould box for foaming and curing, then let it rest, then demould, and then cut to obtain the modified organic thermal insulation material.

8. The method for preparing an inorganic material-modified organic thermal insulation material according to claim 2, characterized in that: The method includes the following steps: 3.1) adding 10wt%-30wt% of the total resin and the total inorganic nanomaterials into a mold for open-cell foaming molding, and after completion, an open-cell foam material is obtained, so that all the inorganic nanomaterials are pre-embedded in the cell walls of the open-cell cells in the open-cell foam material; 3.2) placing the prepared open-cell foam material into a mold box; The remaining mass of resin, foaming agent and additives are stirred and mixed evenly to obtain a mixed slurry; 3.3) Then, a foaming machine is used to pressurize the mixed slurry prepared in step 3.2) and inject it into a closed mold box. In the closed mold box, the mixed slurry is squeezed and flows into the cavities of the open-cell bubbles in the open-cell foam material. The mixed slurry fills all the cavities of the open-cell bubbles in the open-cell foam material. Then, the mixed slurry in the open-cell foam material is sequentially subjected to closed-cell foaming and curing. The mixed slurry in the cavities of the open-cell bubbles in the open-cell foam material is formed into hollow closed-cell bubbles through closed-cell foaming. After curing, the bubble walls of the open-cell bubbles located on the outside are formed to wrap the inner closed-cell bubbles. The structure of the hollow closed-cell bubble is then cured, demoulded, and cut to obtain a modified organic thermal insulation material, so that the bubble wall containing inorganic nanomaterials in the open-cell bubble on the outside forms a flame retardant and fireproof wall, and each open-cell bubble is wrapped and covered with the hollow closed-cell bubble inside as a flame retardant and fireproof wall, and the flame retardant and fireproof wall provides flame retardant and fireproof protection to the hollow closed-cell bubbles inside, the open-cell bubbles on the outside are used for flame retardancy and fire prevention, and the hollow closed-cell bubbles on the inside are used for heat preservation, forming a double-bubble superimposed and sheathed coating structure with flame retardancy and fire prevention on the outside and heat preservation on the inside.

9. The method for preparing an inorganic material-modified organic thermal insulation material according to claim 8, characterized in that: In step 3.3), the inner diameter of the cavity of the open-cell bubbles in the open-cell foam material is 500 μm to 5 mm.

Citation Information

Patent Citations

  • A process for the treatment of waste tyres

    CA3207816A1

  • Polyurethane composite thermal insulation board, manufacturing method and application of the same

    CN101220614A

  • Corrosion-resistant propping agent

    CN101768432A

  • Composite ceramsite prepared from bentonite, perlite and zeolite serving as main raw materials and preparation method of composite ceramsite

    CN102247800A

  • Rigid polyurethane foam thermal insulation material, composite rock wool thermal insulation board and preparation method thereof

    CN112300567A