Broadband excitation orange red fluorescent powder with high external quantum efficiency as well as preparation method and application thereof

Through the chemical formula of La2-xO3:xEu2+/Eu3+ and one-step calcination reduction method, orange-red phosphor with strong absorption and high stability in the near-ultraviolet region was prepared, which solved the problems of narrow excitation peaks and poor stability of phosphors in the prior art. , achieves high external quantum efficiency and broadband excitation effects, and is suitable for a variety of lighting and display applications.

CN118931536APending Publication Date: 2024-11-12HENAN POLYTECHNIC UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410987580.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing Y2O3:Eu3+ and Y2O2S:Eu3+ phosphors have narrow excitation peaks and poor stability in the near-ultraviolet region, which limits their application, and the problem of developing high external quantum efficiency and broadband excitation of orange-red phosphors has not yet been solved.

Method used

The chemical formula of La2-xO3:xEu2+/Eu3+ is adopted to prepare orange-red phosphor by mixing Eu2+/Eu3+ activator in the valence state, and a one-step calcination reduction method is used to ensure strong absorption, high stability and high quantum efficiency in the near-ultraviolet region.

Benefits of technology

A broadband excitation peak in the range of 260-400nm is achieved, with a narrow band of emission spectrum of 537nm, 585nm and 624nm, with high external quantum yield and good optical thermal stability. It is suitable for traditional fluorescent lamps, LED lighting and display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931536A_ABST
    Figure CN118931536A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of luminescent materials, and discloses high external quantum efficiency broadband excitation orange red fluorescent powder as well as a preparation method and application thereof, and the general formula of the orange red fluorescent powder is La2-xO3: xEu < 2 + > / Eu < 3 + >, x is the mole number of Eu atoms, and x is larger than or equal to 0.02 and smaller than or equal to 0.10. Calculating and weighing a La source and an Eu source according to the stoichiometric ratio of the general formula; grinding and mixing the weighed La source and Eu source to obtain a mixture; calcining the mixture, and cooling to room temperature after calcining to obtain a calcined product; and grinding the calcined product to obtain the orange red fluorescent powder La (2-x) O3: xEu < 2 + > / Eu < 3 + >. The orange red fluorescent powder provided by the invention greatly improves the energy utilization rate, and has important commercial value; the quantum dot has the light-emitting characteristics of strong absorption in a near ultraviolet region, high stability, high quantum efficiency and the like, and has great application potential in the fields of illumination, display, signal lamps, indicator lamps, sensors and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of luminescent materials, and in particular to high external quantum efficiency broadband excitation orange-red phosphor and a preparation method and application thereof. Background Art

[0002] In recent years, Y2O3:Eu 3+ Phosphors have attracted widespread attention due to their applications in cathode ray tubes (CRTs), liquid crystal displays (LCDs), field emission displays (FEDs), plasma displays (PDPs), temperature sensors, solid-state lasers, and traditional fluorescent lamps. Recently, this material has also been used in biomedical fields such as biomarkers, bioimaging probes, and medical diagnosis. This material has extremely high commercial value, but because it only has a broadband excitation peak in the range of 240-300nm and only a sharp excitation peak in the near-ultraviolet region of 300-400nm, its application does have certain limitations.

[0003] Y2O2S:Eu 3+ It has broadband absorption in the near-ultraviolet region, but contains S components, has poor stability and is easily contaminated. Therefore, it is urgent to develop alternative high-efficiency phosphors to improve the above problems. The raw materials for development are easy to obtain, the preparation is simple, the economic benefits are high, it has a broadband excitation peak, a high external quantum yield, and it also has Eu 3+ The material with characteristic sharp emission peak is the core technical problem to be overcome in order to realize industrial production.

[0004] Therefore, there is an urgent need for high external quantum efficiency broadband excitation orange-red phosphors and their preparation methods and applications to solve the above technical problems. Summary of the invention

[0005] The purpose of the present invention is to overcome the existing Y2O3:Eu 3+ and Y2O2S:Eu 3+ The shortcomings of phosphors are overcome, and an orange-red luminescent material is provided which has simple preparation, strong absorption in the near-ultraviolet region, high stability and high quantum efficiency.

[0006] To achieve the above object, the present invention is implemented according to the following technical solutions:

[0007] High external quantum efficiency broadband excitation orange-red phosphor, the general formula of orange-red phosphor is La 2-x O3:xEu 2+ / Eu 3+ ; Wherein x is the molar number of Eu atoms, 0.02≤x≤0.10.

[0008] The orange-red phosphor La of the present invention 2-x O3:xEu 2+ / Eu 3+Abbreviated as La2O3:Eu 2+ / Eu 3+ .

[0009] The orange-red phosphor La of the present invention 2-x O3:xEu 2+ / Eu 3+ In the phosphor, the activator Eu element coexists in a mixed valence state of +2 and +3, and it is a europium-activated lanthanum oxide orange-red phosphor.

[0010] The principle of the coexistence of Eu elements in +2 and +3 mixed valence states is that the Eu element in the raw material Eu2O3 is +3 valence, which is partially reduced to Eu under high temperature calcination and in the presence of a reducing atmosphere. 2+ , the rest is still Eu 3+ , the reason is that Eu 3+ Occupies La in the base material 3+ The lattice position and charge balance make it difficult to be completely reduced to Eu even in the presence of a reducing atmosphere. 2+ . .

[0011] Specifically, x includes but is not limited to any one of 0.02, 0.04, 0.06, 0.08, and 0.10, or a range of values ​​between any two of them. Further, when x=0.04, La 2-x O3:xEu 2+ / Eu 3+ Highest luminous efficiency.

[0012] A method for preparing a high external quantum efficiency broadband excitation orange-red phosphor comprises the following steps:

[0013] S1, according to the general formula La 2-x O3:xEu 2+ / Eu 3+ Calculate and weigh the La source and Eu source according to the stoichiometric ratio;

[0014] S2, weighing the La source and Eu source, grinding and mixing them to obtain a mixture;

[0015] S3, pre-calcining the mixture obtained in step S2 and then calcining it, cooling it to room temperature after the calcination to obtain a calcined product; grinding the calcined product to obtain an orange-red phosphor La 2-x O3:xEu 2+ / Eu 3+ .

[0016] Preferably, in step S1, the La source is at least one of La2O3, La(OH)3, and La2(CO3)3·xH2O; and the Eu source is at least one of Eu2O3 and Eu(OH)3.

[0017] Preferably, in step S3, the process of pre-sintering and then calcining is: pre-sintering the mixture, cooling it, grinding it and then calcining it; the pre-sintering temperature is 400°C, and the pre-sintering time is 10 hours; the calcining temperature is 1100-1700°C, and the calcining time is 6-48 hours.

[0018] The calcination temperature is 1100-1700℃. The temperature will affect some properties of the material, but will have little effect on the overall effect.

[0019] Preferably, in step S3, the pre-firing atmosphere is air, and the calcining atmosphere is a reducing atmosphere.

[0020] Preferably, in step S3, the reducing atmosphere is at least one of H2, NH3, CO, H2S, SO2, SO, CH4, C2H6, C2H4, C2H2, CH3OH, C2H5OH, a mixture of H2 and N2, a mixture of H2 and Ar, a mixture of H2 and CO, and water gas.

[0021] Preferably, in step S3, the mixture is placed in a crucible and calcined in a high-temperature furnace.

[0022] The mixture is placed in the crucible in a loose manner.

[0023] Specifically, the preparation method comprises the following steps:

[0024] S1, according to the general formula La 2-x O3:xEu 2+ / Eu 3 (where 0.02≤x≤0.10), calculate and weigh La2O3 and Eu2O3;

[0025] S2, weighing La2O3 and Eu2O3, mixing them in an agate mortar or grinding them in a ball mill for 10 to 20 minutes to prepare a mixture;

[0026] S3, the above mixture is put into an alumina crucible, placed in a furnace, and heated to 1100-1700°C in a reducing atmosphere, calcined for 6-48 hours, and after the reaction is completed, cooled to room temperature and ground again to obtain La 2- x O3:xEu 2+ / Eu 3+ .

[0027] The reducing atmosphere is cheap and readily available substances such as H2, NH3, CO, H2S, SO2, SO, CH4, C2H6, C2H4, C2H2, CH3OH, C2H5OH, etc., or a mixture of H2+N2, H2+Ar, H2+CO, water gas, etc.; the mixture is placed in the alumina crucible in a loose manner.

[0028] The preparation method of the invention is a one-step calcination reduction method.

[0029] The invention also includes the application of orange-red fluorescent powder in lighting and display.

[0030] Specifically, the orange-red phosphor of the present invention can be used in the fields of traditional fluorescent lamps, LED lighting, displays, signal lamps, indicator lights, sensors, etc.

[0031] The orange-red phosphor of the present invention can be applied to various technical fields, especially in traditional fluorescent lamps, and can replace the traditional red phosphor Y2O3:Eu 3+ or Y2O2S:Eu 3+ It can also be used in general lighting systems, white light lighting systems based on white light LEDs, signal lights, indicator lights, etc., as well as display backlights, plasma display panels, and display panels based on LEDs.

[0032] The orange-red fluorescent powder La prepared by the present invention 2-x O3:xEu 2+ / Eu 3+ It has a broadband excitation peak in the range of 260-400nm, with a peak value of 360nm; the emission spectrum is mainly a sharp narrow emission band with peak values ​​of 537nm, 585nm, and 624nm.

[0033] The orange-red phosphor La2O3:Eu prepared by the present invention 2+ / Eu 3+ The mechanism of high quantum yield emission under near-ultraviolet light (300-400nm) is that Eu 2+ As sensitizer, Eu 3+ As the luminescence center, first Eu 2+ The ion absorbs radiation energy, excites the 4f electron to jump to its 5d orbital, and then transfers the excitation energy to Eu through energy transfer. 3+ The related orbits of the ions, after a series of processes, finally produce Eu 3+ A series of luminescence processes.

[0034] The orange-red phosphor La2O3:Eu prepared by the present invention 2+ / Eu 3+ , where Eu 2+ With Eu 3+The energy transfer efficiency is almost 100%.

[0035] The orange-red phosphor La with a europium concentration of 0.04 prepared by the present invention 1.96 O3:0.04Eu 2+ / Eu 3+ , has good optical thermal stability, and the emission integrated intensity at 425K still maintains 79% of that at 300K.

[0036] The orange-red phosphor La with a europium concentration of 0.04 prepared by the present invention 1.96 O3:0.04Eu 2+ / Eu 3+ , which is higher than single Eu in the whole excitation band. 3+ Activated La2O3 red phosphor La2O3:Eu 3+ The external quantum yield.

[0037] The orange-red phosphor La with a europium concentration of 0.04 prepared by the present invention 1.96 O3:0.04Eu 2+ / Eu 3+ , exposed to air at 300℃ for more than 1 hour, the luminous intensity did not change, and no Eu 2+ The phenomenon of oxidation shows its good chemical stability.

[0038] Working principle:

[0039] The present invention uses La2O3 as the substrate and Eu 2+ / Eu 3+ As a co-activator, a new type of highly efficient orange-red phosphor with high external quantum efficiency and ultra-narrow band emission was prepared. The preparation process is simple, the raw materials are readily available, and the cost is low. It is suitable for the manufacture of fluorescent conversion lighting and display devices. 2-x O3:xEu 2+ / Eu 3+ , which represents the material composition, abbreviated as La2O3:Eu 2 + / Eu 3+ , where x is the molar number of Eu atoms, 0.02≤x≤0.10.

[0040] Phosphor has Eu 2+ Characteristic broadband excitation (300-400nm), which is consistent with the near-ultraviolet LED chip, and its emission light is mainly Eu 3+ The red phosphor used in traditional fluorescent lamps (i.e. low-pressure mercury lamps and fluorescent lamps) is mainly Y2O3:Eu 3+ or Y2O2S:Eu3+ , Y2O3:Eu 3+ It can only absorb light in the 254nm band of the mercury vapor spectrum, and cannot absorb light in the other 300-400nm band. 2+ / Eu 3+ The material has a broadband excitation peak in the 260-400nm band, and its emission spectrum contains not only orange-red light in the 585nm and 624nm bands, but also green light in the 537nm band. 2+ / Eu 3+ The material is simply prepared, and the quantum efficiency of the emission spectrum under the excitation of light in the 300-370nm band reaches more than 50%, which is much better than Y2O3:Eu 3+ . With Y2O2S:Eu 3+ Compared with La2O3:Eu 2+ / Eu 3+ It is simple to make, low in cost, stable in nature, pollution-free and not easy to deteriorate. 2+ / Eu 3+ Can be used in traditional fluorescent lamps to replace Y2O3:Eu 3+ and Y2O2S:Eu 3+ , and can be used in the manufacture of LED lighting and display devices, and has important commercial value.

[0041] Beneficial effects:

[0042] The orange-red phosphor La2O3:Eu of the present invention 2+ / Eu 3+ , where the activator Eu element coexists in a mixed valence state of +2 / +3. 2+ As a sensitizer, Eu 2+ The highly efficient 260-400nm range has a broadband absorption peak, which is very similar to the traditional red phosphor Y2O3:Eu 3+ Compared with traditional methods, it greatly improves the energy utilization rate and has important commercial value.

[0043] The orange-red phosphor La2O3:Eu of the present invention 2+ / Eu 3+ It has luminescence characteristics such as strong absorption in the near-ultraviolet region, high stability, and high quantum efficiency, and has great application potential in the fields of lighting, display, signal lights, indicator lights, sensors, etc.

[0044] The orange-red phosphor La2O3:Eu of the present invention 2+ / Eu 3+ , which can well solve the current Y2O3:Eu 3+ The problems faced are poor absorption in the near-ultraviolet band, low energy utilization, and poor matching with LED chips.

[0045] The orange-red phosphor La2O3:Eu of the present invention 2+ / Eu 3+ , simple to make, low cost, solves the problem of Y2O2S:Eu 3+ The disadvantages are poor stability and easy contamination due to S content. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 The XRD spectra of the orange-red phosphors prepared in Examples 1 to 5 of the present invention;

[0047] Figure 2 The La prepared in Example 2 of the present invention 1.96 O3:0.04Eu 2+ / Eu 3+ Fluorescence excitation emission spectrum of

[0048] Figure 3 The La prepared in Example 2 of the present invention 1.96 O3:0.04Eu 2+ / Eu 3+ Compared with the pure Eu prepared in Comparative Example 1 3+ Activation material La 1.96 O3:0.04Eu 3+ Comparison bar graph of external quantum yield at different excitation light wavelengths;

[0049] Figure 4 The La prepared in Example 2 of the present invention 1.96 O3:0.04Eu 2+ / Eu 3+ Thermal stability diagram. DETAILED DESCRIPTION

[0050] The present invention is further described below with reference to specific embodiments. The illustrative embodiments and descriptions of the present invention are used to explain the present invention but are not intended to limit the present invention.

[0051] All raw materials of the present invention have no particular limitation on their sources, and can be purchased from the market or prepared according to conventional methods known to those skilled in the art.

[0052] There is no particular limitation on the purity of all raw materials in the present invention, and the present invention preferably adopts the conventional purity used in the art.

[0053] The devices used in the present invention are not particularly limited and can be any of the commonly used devices in the art.

[0054] Embodiment 1:

[0055] A method for preparing a high external quantum efficiency broadband excitation orange-red phosphor comprises the following steps:

[0056] Preparation of La 1.98 O3:0.02Eu 2+ / Eu 3+ Phosphor: According to the chemical formula La 1.98 Eu 0.02 O3, weigh 3.000g of lanthanum oxide (La2O3) and 0.0327g of europium oxide (Eu2O3), grind them in an agate mortar for half an hour to make them evenly mixed, put them in a muffle furnace, heat them to 400℃ and keep them constant in air for 10 hours. Then cool and take out the crucible, pour out the sample, grind it evenly again, put it into the corundum crucible again, and calcine it at 1450℃ for 24 hours in a flowing H2 (10% volume) + N2 (90% volume) mixed atmosphere in a muffle furnace with a gas flow rate of 40ml / min, and turn off the power of the muffle furnace. After cooling, take out the crucible to obtain a white powder sample, which is the compound La 1.98 O3:0.02Eu 2+ / Eu 3+ of pure powder.

[0057] Embodiment 2:

[0058] The preparation method of the high external quantum efficiency broadband excitation orange-red phosphor comprises the following steps:

[0059] Preparation of La 1.96 O3:0.04Eu 2+ / Eu 3+ Phosphor, according to the chemical formula La 1.96 Eu 0.04 O3, weigh 3.000g of lanthanum oxide (La2O3) and 0.0661g of europium oxide (Eu2O3), grind them in an agate mortar for half an hour to make them evenly mixed, put them in a muffle furnace, heat them to 400℃ and keep them constant in air for 10 hours. Then cool and take out the crucible, pour out the sample, grind it again and put it into the corundum crucible again, and calcine it at 1450℃ for 24 hours in a flowing H2 (10% volume) + N2 (90% volume) mixed atmosphere with a gas flow rate of 40ml / min in the muffle furnace. Turn off the power of the muffle furnace. After cooling, take out the crucible to obtain a white powder sample, which is the compound La 1.96 O3:0.04Eu 2+ / Eu 3+ of pure powder.

[0060] Embodiment 3:

[0061] The preparation method of the high external quantum efficiency broadband excitation orange-red phosphor comprises the following steps:

[0062] Preparation of La 1.94 O3:0.06Eu 2+ / Eu 3+ Phosphor, according to the chemical formula La 1.94 Eu 0.06 O3, weigh 3.000g of lanthanum oxide (La2O3) and 0.100g of europium oxide (Eu2O3), grind them in an agate mortar for half an hour to make them evenly mixed, put them in a muffle furnace, heat them to 400℃ and keep them constant in air for 10 hours. Then cool and take out the crucible, pour out the sample, grind it evenly again, put it into the corundum crucible again, and calcine it at 1450℃ for 24 hours in a flowing H2 (10% volume) + N2 (90% volume) mixed atmosphere in a muffle furnace with a gas flow rate of 40ml / min, and turn off the power of the muffle furnace. After cooling, take out the crucible to obtain a white powder sample, which is the compound La 1.94 O3:0.06Eu 2+ / Eu 3+ of pure powder.

[0063] Embodiment 4:

[0064] The preparation method of the high external quantum efficiency broadband excitation orange-red phosphor comprises the following steps:

[0065] Preparation of La 1.92 O3:0.08Eu 2+ / Eu 3+ Phosphor, according to the chemical formula La 1.92 Eu 0.08 O3, weigh 3.000g of lanthanum oxide (La2O3) and 0.135g of europium oxide (Eu2O3), grind them in an agate mortar for half an hour to make them evenly mixed, put them in a muffle furnace, heat them to 400℃ and keep them constant in air for 10 hours. Then cool and take out the crucible, pour out the sample, grind it evenly again, put it into the corundum crucible again, and calcine it at 1450℃ for 24 hours in a flowing H2 (10% volume) + N2 (90% volume) mixed atmosphere in a muffle furnace with a gas flow rate of 40ml / min, and turn off the power of the muffle furnace. After cooling, take out the crucible to obtain a white powder sample, which is the compound La 1.92 O3:0.08Eu 2+ / Eu 3+ of pure powder.

[0066] Embodiment 5:

[0067] The preparation method of the high external quantum efficiency broadband excitation orange-red phosphor comprises the following steps:

[0068] Preparation of La 1.90 O3:0.10Eu 2+ / Eu3+ Phosphor, according to the chemical formula La 1.90 Eu 0.10 O3, weigh 3.000g of lanthanum oxide (La2O3) and 0.171g of europium oxide (Eu2O3), grind them in an agate mortar for half an hour to make them evenly mixed, put them in a muffle furnace, heat them to 400℃ and keep them constant in air for 10 hours. Then cool and take out the crucible, pour out the sample, grind it again and put it into the corundum crucible again, and calcine it at 1450℃ for 24 hours in a flowing H2 (10% volume) + N2 (90% volume) mixed atmosphere with a gas flow rate of 40ml / min in the muffle furnace. Turn off the power of the muffle furnace. After cooling, take out the crucible to obtain a white powder sample, which is the compound La 1.90 O3:0.10Eu 2+ / Eu 3+ of pure powder.

[0069] Comparative Example 1:

[0070] Pure Eu 3+ Activation material La 1.96 O3:0.04Eu 3+ Preparation: According to the chemical formula La 1.96 Eu 0.04 O3, weigh 3.000g of lanthanum oxide (La2O3) and 0.0661g of europium oxide (Eu2O3), grind them in an agate mortar for half an hour to make them evenly mixed, put them in a muffle furnace, heat them to 400℃ and keep them constant in air for 10 hours, then cool them down and take out the crucible, pour out the sample, grind it evenly again, put it into a corundum crucible again, heat it to 1450℃ in a muffle furnace and keep it constant in air for 24 hours to obtain pure Eu 3+ Activation material La 1.96 O3:0.04Eu 3+ .

[0071] like Figure 1 The figure shows the XRD spectra of the orange-red phosphors prepared in Examples 1 to 5 of the present invention. In the figure, x=0.00 refers to the raw material La2O3 used in the examples; x=0.02 refers to the La2O3 prepared in Example 1. 1.98 O3:0.02Eu 2+ / Eu 3+ ; x = 0.04 refers to the La prepared in Example 2 1.96 O3:0.04Eu 2+ / Eu 3+ ; x = 0.06 refers to the La prepared in Example 3 1.94 O3:0.06Eu 2+ / Eu 3+; x = 0.08 refers to the La prepared in Example 4 1.92 O3:0.08Eu 2+ / Eu 3+ ; x = 0.10 refers to the La prepared in Example 5 1.90 O3:0.10Eu 2+ / Eu 3+ ; X-ray diffraction test was performed on each of the above powders.

[0072] Depend on Figure 1 It can be seen that the obtained spectrum is completely consistent with the X-ray diffraction spectrum obtained by crystal structure fitting, indicating that the prepared sample is a compound with high purity; the peak positions of each spectrum are the same, proving that the prepared material is a pure phase material.

[0073] like Figure 2 As shown, this is the La prepared in Example 2 of the present invention. 1.96 O3:0.04Eu 2+ / Eu 3+ Fluorescence excitation emission spectra.

[0074] In other embodiments, materials with different concentrations only differ in emission intensity, and the peak types and positions are basically the same.

[0075] exist Figure 2 The left side of the middle is the excitation spectrum of monitoring 585nm emission, which is mainly a broadband peak in the range of 260-400nm, attributed to Eu 2+ The ion's 4f→5d transition absorption peak; the luminescence spectrum obtained by excitation with ultraviolet light at 360nm on the right, the main central luminescence wavelength is mainly composed of three linear spectra, located near 537nm (green light), 585nm (yellow light), and 623nm (red light), respectively corresponding to Eu 3+ ion 5 D1→ 7 F1, 5 D1→ 7 F3, 5 D0→ 7 F2 transition peak, the emission peak at 585nm is the strongest peak. At the same time, through CIE calculation, it is known that its coordinates are x=0.512y=0.460, which falls in the orange-red area, and can be used as orange-red phosphor in the field of white light LED lighting. In addition, the material La 1.96 O3:0.04Eu 2+ / Eu 3+ It can simultaneously generate narrow-band green, yellow and red light emissions and can be used in the field of LED displays.

[0076] like Figure 3 As shown, this is the La prepared in Example 2 of the present invention.1.96 O3:0.04Eu 2+ / Eu 3+ Compared with the pure Eu prepared in Comparative Example 1 3+ Activation material La 1.96 O3:0.04Eu 3+ Comparison bar graph of external quantum yield at different excitation light wavelengths.

[0077] Depend on Figure 3 It can be seen that La 1.96 O3:0.04Eu 2+ / Eu 3+ It shows that it has high luminous efficiency in the 260-400nm band, and its highest external quantum efficiency is located at 330nm, reaching 74%, ensuring its practical value.

[0078] like Figure 4 As shown, this is the La prepared in Example 2 of the present invention. 1.96 O3:0.04Eu 2+ / Eu 3+ Thermal stability diagram.

[0079] Depend on Figure 4 It can be seen that La 1.96 O3:0.04Eu 2+ / Eu 3+ It has good optical thermal stability, and the emission integrated intensity at 425K still maintains 79% of that at 300K.

[0080] The technical solution of the present invention is not limited to the above-mentioned specific embodiments. All technical variations made according to the technical solution of the present invention fall within the protection scope of the present invention.

Claims

1. High external quantum efficiency broadband excitation orange-red phosphor, characterized by: The general formula of orange-red phosphor is La 2-x O3:xEu 2+ / Eu 3+ ; Wherein x is the molar number of Eu atoms, 0.02≤x≤0.

10.

2. A method for preparing the high external quantum efficiency broadband excitation orange-red phosphor according to claim 1, characterized in that: The following steps are involved: S1, according to the general formula La 2-x O3:xEu 2+ / Eu 3+ Calculate and weigh the La source and Eu source according to the stoichiometric ratio; S2, weighing the La source and Eu source, grinding and mixing them to obtain a mixture; S3, pre-calcining the mixture obtained in step S2 and then calcining it, cooling it to room temperature after the calcination to obtain a calcined product; grinding the calcined product to obtain an orange-red phosphor La 2-x O3:xEu 2+ / Eu 3+ .

3. The method for preparing the high external quantum efficiency broadband excitation orange-red phosphor according to claim 2, characterized in that: In step S1, the La source is at least one of La2O3, La(OH)3, and La2(CO3)3·xH2O; the Eu source is at least one of Eu2O3 and Eu(OH)3.

4. The method for preparing the high external quantum efficiency broadband excitation orange-red phosphor according to claim 2, characterized in that: In step S3, the process of pre-sintering and then calcining is as follows: pre-sintering the mixture, cooling it, grinding it and then calcining it; the pre-sintering temperature is 400° C., and the pre-sintering time is 10 hours; the calcining temperature is 1100-1700° C., and the calcining time is 6-48 hours.

5. The method for preparing the high external quantum efficiency broadband excitation orange-red phosphor according to claim 2, characterized in that: In the step S3, the atmosphere for pre-firing is air, and the atmosphere for calcining is a reducing atmosphere.

6. The method for preparing the high external quantum efficiency broadband excitation orange-red phosphor according to claim 5, characterized in that: In step S3, the reducing atmosphere is at least one of H2, NH3, CO, H2S, SO2, SO, CH4, C2H6, C2H4, C2H2, CH3OH, C2H5OH, a mixture of H2 and N2, a mixture of H2 and Ar, a mixture of H2 and CO, and water gas.

7. The method for preparing the high external quantum efficiency broadband excitation orange-red phosphor according to claim 2, characterized in that: In step S3, the mixture is placed in a crucible and calcined in a high-temperature furnace.

8. Use of the orange-red phosphor according to claim 1 or the orange-red phosphor prepared by the preparation method according to any one of claims 2 to 7 in lighting and display.

Citation Information

Patent Citations

  • Eu&lt;2+&gt; / Eu&lt;3+&gt; coexisting (Y0.9La0.1)2O3 powder and preparation method and application of powder as well as preparation method of transparent ceramic

    CN104478435A