Copper indium selenium / zinc sulfide core-shell quantum dot and preparation method and application thereof

By preparing copper indium selenide (CIGS)/zinc sulfide core-shell quantum dots, adjusting the stoichiometry, and doping with zinc ions, the emission wavelength and fluorescence efficiency issues of CIGS quantum dots in the near-infrared band were solved, achieving good matching with silicon detectors and improving the performance of near-infrared optical wireless communication.

CN118931540APending Publication Date: 2024-11-12SHANGHAI INST OF OPTICS & FINE MECHANICS CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410916568.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the existing technology, the emission wavelength of copper indium selenide quantum dots is difficult to control in the near-infrared band, resulting in decreased fluorescence efficiency and poor matching with silicon detectors, which limits their application in near-infrared optical wireless communication.

Method used

A copper indium selenide/zinc sulfide core-shell quantum dot structure is adopted. By adjusting the stoichiometry and doping with zinc ions, a core-shell structure is formed, optimizing the emission wavelength to around 800 nm. The core-shell structure is constructed with zinc sulfide cladding material to reduce surface defects and improve fluorescence efficiency.

Benefits of technology

Highly efficient fluorescence quantum yield of copper indium selenide/zinc sulfide core-shell quantum dots in the near-infrared band was achieved, which was well matched with silicon detectors, improving the detection efficiency and signal-to-noise ratio of the system and reducing the system cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931540A_ABST
    Figure CN118931540A_ABST
Patent Text Reader

Abstract

The invention discloses a copper indium selenium / zinc sulfide core-shell quantum dot as well as a preparation method and application thereof, and the preparation method comprises the following steps: mixing cuprous iodide, indium acetate, zinc stearate, octadecene and n-dodecyl mercaptan, violently stirring at 110-130 DEG C in an inert gas atmosphere, and then injecting oleylamine and oleic acid in sequence for continuous degassing. And injecting a selenium precursor solution at 215-225 DEG C in an inert gas atmosphere, carrying out heat preservation, finally dropwise adding a zinc sulfide shell solution at 230-240 DEG C, carrying out cladding and heat preservation, and then carrying out quenching and purification, thereby obtaining the selenium-rich zinc sulfide composite material. The copper indium selenium / zinc sulfide core-shell quantum dot material synthesized by the invention has efficient fluorescence quantum yield and large Stokes shift in near-infrared band of 800 nm, and shows huge application potential in near-infrared light wireless communication.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of optical wireless communication, and in particular relates to a copper indium selenide / zinc sulfide core-shell quantum dot and a preparation method and application thereof. Background Art

[0002] With the growing demand for data transmission and the development of semiconductor lighting technology, optical wireless communication is gradually being proposed as a communication technology with faster transmission rate and larger capacity. Compared with traditional radio frequency communication, optical wireless communication covers the entire band from visible light to near infrared, and is an ideal high-speed wireless communication method. Optical wireless communication technology mainly uses visible light and infrared light as transmission carriers to transmit information by modulating the properties of light waves (such as frequency, amplitude, phase, etc.). It can be applied to a variety of scenarios, including indoor communication and outdoor communication. It can also be used in special environments, such as underwater communication. After more than 20 years of development, visible light wireless communication has made great progress, but near-infrared light wireless communication still needs to be explored. Near-infrared light wireless communication has unique advantages such as lower optical loss, better penetration ability and higher security. It extends the spectral range to the near-infrared window, which not only broadens the link bandwidth but also paves the way for its integration into many applications using near-infrared radiation. Therefore, making up for the shortcomings of near-infrared light wireless communication is an important scientific issue.

[0003] Optical wireless communication systems are mainly composed of transmitting devices, intermediate optical conversion materials and receiving devices. Quantum dots have a place in optical conversion materials because they can easily adjust emission by controlling size and composition, have high fluorescence quantum yield and high chemical stability. In the past, II-VI (CdSe, CdTe) and IV-VI (PbS, PbSe) were typical near-infrared fluorescent quantum dots, but their further development and commercial application were limited because they contained toxic heavy metals such as cadmium and lead. At present, I-III-VI environmentally friendly quantum dots are effective alternatives, mainly including copper indium sulfide and copper indium selenide, but copper indium sulfide has a wide band gap and is not suitable for use in the infrared band. Copper indium selenide has far-reaching application prospects in the infrared band due to its narrow band gap and excellent optical properties. The reason why near-infrared quantum dots have developed slowly in optical wireless communication is mainly because the fluorescence efficiency will drop significantly as the wavelength gradually redshifts. At present, it is still a huge challenge to synthesize copper indium selenide quantum dots with high fluorescence quantum yield at an emission wavelength near 800nm. The emission wavelength is set at 800nm ​​to match the silicon detector, which is beneficial to improve the overall performance and reduce the system cost.

[0004] Adjusting the precursor molar ratio and doping can adjust the emission wavelength, and encapsulation treatment can improve the fluorescence efficiency. Therefore, reasonable design of the stoichiometric ratio and doping elements is an effective way to synthesize high-efficiency fluorescence near-infrared quantum dots, and ultimately realize environmentally friendly quantum dots that are expected to be used in the field of near-infrared light wireless communications. Summary of the invention

[0005] In view of the above-mentioned prior art, the present invention provides a copper indium selenide / zinc sulfide core-shell quantum dot and a preparation method and application thereof to solve the problems of controlling the emission wavelength in the near-infrared band, a significant decrease in fluorescence efficiency, and poor matching with silicon detectors.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is: to provide a method for preparing copper indium selenide / zinc sulfide core-shell quantum dots, comprising the following steps:

[0007] After mixing cuprous iodide, indium acetate, zinc stearate, octadecene and n-dodecyl mercaptan, stir vigorously at 110°C to 130°C for 20min to 30min under an inert gas atmosphere, then add oleic acid and oleylamine successively and continue degassing for 20min to 30min.

[0008] In an inert gas atmosphere, the temperature is heated to 215°C to 225°C, and the selenium precursor solution is rapidly injected and kept warm for 20min to 30min to obtain a copper indium selenium quantum dot solution.

[0009] The copper indium selenide quantum dot solution is continued to be heated to 230° C. to 240° C., and then the zinc sulfide shelling solution is added dropwise and kept warm for 60 min to 70 min to form a core-shell structure, followed by quenching and purification to obtain the product.

[0010] Among various environmentally friendly quantum dots, copper indium selenide quantum dots have the characteristics of high absorption and narrow band gap. By doping zinc ions and changing the stoichiometric ratio, the emission wavelength can be controlled in the near-infrared region of about 800nm, improving the compatibility with silicon detectors and facilitating the integration of the entire system. Using zinc sulfide to coat copper indium selenide core quantum dots to form a core-shell structure can effectively reduce surface defect states and greatly improve the fluorescence quantum yield, thereby realizing high-performance quantum dots that can be used in the field of near-infrared optical wireless communications.

[0011] On the basis of the above technical solution, the present invention can also be improved as follows:

[0012] Furthermore, in step 1, the usage ratio of cuprous iodide, indium acetate, zinc stearate, octadecene, n-dodecyl mercaptan, oleic acid and oleylamine is 0.1mmol-0.2mmol:0.1mmol-0.2mmol:0.1mmol-0.2mmol:9-11ml:0.5-1.5ml:0.4-0.6ml:0.4-0.6ml. The optimal ratio is 0.18mmol:0.2mmol:0.14mmol:10ml:1ml:0.5ml:0.5ml.

[0013] Further, the selenium powder is dissolved in a mixed solution of oleylamine and n-dodecyl mercaptan, and stirred to fully dissolve, to obtain the selenium powder, oleylamine, n-dodecyl mercaptan and the mixture obtained in step 1. The dosage ratio is 0.3-0.5 mmol: 0.6-0.8 ml: 0.2-0.4 ml: 10-13 ml.

[0014] Further, zinc stearate, n-dodecyl mercaptan and octadecene are mixed, heated to 180-200° C. in an inert gas atmosphere to dissolve, and the amount ratio of zinc stearate, n-dodecyl mercaptan, octadecene and copper indium selenide quantum dot solution is 1.5-1.7 mmol: 0.3-0.5 ml: 1.5-1.7 ml: 10-13 ml.

[0015] Furthermore, the speed of dropwise addition in step 2 should be controlled at about 0.9 to 1.1 ml / min.

[0016] Furthermore, the purification includes the following steps: mixing the copper indium selenide / zinc sulfide core-shell quantum dot solution with ethanol and toluene in a volume ratio of 14:7:12, and then centrifuging at a speed of 11300 rpm for 7 minutes to obtain a primary precipitate, adding appropriate ethanol and toluene to the primary precipitate, mixing at a volume ratio of 1:1 between ethanol and toluene, and then centrifuging at a speed of 11500 rpm for 7 minutes to obtain a secondary precipitate, adding appropriate ethanol and toluene to the secondary precipitate, mixing at a volume ratio of 1:1 between ethanol and toluene, and then centrifuging at a speed of 12000 rpm for 7 minutes to obtain a tertiary precipitate, and dissolving in a toluene solution for storage.

[0017] The present invention also provides copper indium selenide / zinc sulfide core-shell quantum dots prepared by the preparation method.

[0018] The present invention also provides the application of the copper indium selenide / zinc sulfide core-shell quantum dots in the field of optical wireless communications.

[0019] The beneficial effects of the present invention are:

[0020] 1. The copper indium selenide / zinc sulfide core-shell structure quantum dot material prepared by the present invention is an environmentally friendly semiconductor quantum dot material. Compared with traditional near-infrared quantum dots, it does not contain toxic heavy metal elements such as cadmium and lead, is environmentally friendly, and its performance is comparable to that of toxic quantum dots.

[0021] 2. In the process of preparing copper indium selenide quantum dots, the present invention changes the stoichiometric ratio so that the emission wavelength of the copper indium selenide core is sufficiently red-shifted, and then zinc ions are doped to avoid subsequent cation exchange between zinc ions and copper ions and indium ions, making the core smaller and significantly blue-shifted, effectively solving the previous problem of the contradiction between the red shift of the emission wavelength and the high fluorescence efficiency.

[0022] 3. The present invention uses zinc sulfide shell material to construct a core-shell structure. Compared with the common zinc selenide shell material, it has better light transmittance and is more suitable for use in optoelectronic devices. Combined with zinc ion doping, it reduces the lattice mismatch between the core and shell, effectively passivates surface defects, and greatly improves the fluorescence efficiency.

[0023] 4. The copper indium selenide / zinc sulfide core-shell structure quantum dots synthesized by the present invention maintain a high fluorescence quantum yield at a wavelength near 800nm, which matches well with commercial silicon photodetectors, can achieve higher detection efficiency and higher signal-to-noise ratio, is conducive to integration, and reduces system costs. Because the contradiction between emission wavelength and fluorescence efficiency is effectively solved, environmentally friendly quantum dots that can be used in the field of near-infrared optical wireless communications are synthesized. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a TEM characterization image of the copper indium selenide / zinc sulfide core-shell quantum dots in Example 1 of the present invention.

[0025] Figure 2 1 is the light absorption and emission spectra of the copper indium selenide / zinc sulfide core-shell quantum dots in Example 1 of the present invention.

[0026] Figure 3 Schematic diagram of the indoor near-infrared wireless communication test system.

[0027] Figure 4 In order to use the copper indium selenide / zinc sulfide core-shell quantum dots prepared in Example 1 of the present invention as optical conversion materials, a modulation bandwidth diagram in the near-infrared band was tested. DETAILED DESCRIPTION

[0028] The specific implementation modes of the present invention are described in detail below with reference to the accompanying drawings.

[0029] Example 1

[0030] A copper indium selenide / zinc sulfide core-shell quantum dot material, the preparation method of which comprises the following steps:

[0031] 0.18 mmol of cuprous iodide, 0.2 mmol of indium acetate, 0.14 mmol of zinc stearate, 10 ml of octadecene and 1 ml of n-dodecyl mercaptan were mixed, and stirred vigorously at 120°C for 30 min under an inert gas atmosphere. Then, 0.5 ml of oleic acid and 0.5 ml of oleylamine were added successively, and degassing was continued for 30 min.

[0032] In an inert gas atmosphere, the mixture was heated to 220°C, and the selenium precursor solution was rapidly injected and kept warm for 20 minutes to obtain a copper indium selenium quantum dot solution. The preparation method of the selenium precursor solution is as follows: 0.4 mmol of selenium powder was dissolved in 0.7 ml of oleylamine and 0.3 ml of n-dodecyl mercaptan, and stirred to fully dissolve.

[0033] The copper indium selenide quantum dot solution is further heated to 230°C, and then the zinc sulfide shell solution is added dropwise, and the temperature is kept for 60 minutes to form a core-shell structure, and then quenched to obtain. The speed of dropwise addition should be controlled at about 1 ml / min. The zinc sulfide shell solution is formed by mixing zinc stearate, n-dodecyl mercaptan and octadecene, and heated to 190°C under an inert gas atmosphere to dissolve. The amount ratio of zinc stearate, n-dodecyl mercaptan, octadecene and copper indium selenide quantum dot solution is 1.6 mmol: 0.4 ml: 1.6 ml: 12 ml.

[0034] The copper indium selenide / zinc sulfide core-shell quantum dot solution was mixed with ethanol and toluene in a volume ratio of 14:7:12, and then centrifuged at 11300 rpm for 7 min to obtain a primary precipitate, appropriate ethanol and toluene were added to the primary precipitate, and the mixture was mixed in a volume ratio of 1:1 to ethanol and toluene, and then centrifuged at 11500 rpm for 7 min to obtain a secondary precipitate, and appropriate ethanol and toluene were added to the secondary precipitate, and the mixture was mixed in a volume ratio of 1:1 to ethanol and toluene, and then centrifuged at 12000 rpm for 7 min to obtain a tertiary precipitate, which was dissolved in a toluene solution for storage.

[0035] Example 2

[0036] A copper indium selenide / zinc sulfide core-shell quantum dot material, the preparation method of which comprises the following steps:

[0037] 0.2 mmol of cuprous iodide, 0.15 mmol of indium acetate, 0.2 mmol of zinc stearate, 11 ml of octadecene and 0.5 ml of n-dodecyl mercaptan were mixed, stirred vigorously at 110°C for 25 min under an inert gas atmosphere, and then 0.4 ml of oleic acid and 0.6 ml of oleylamine were added successively and degassing was continued for 25 min.

[0038] In an inert gas atmosphere, the mixture was heated to 215°C, and the selenium precursor solution was rapidly injected and kept warm for 25 minutes to obtain a copper indium selenium quantum dot solution. The preparation method of the selenium precursor solution is as follows: 0.3 mmol of selenium powder was dissolved in 0.6 ml of oleylamine and 0.2 ml of n-dodecyl mercaptan, and stirred to fully dissolve.

[0039] The copper indium selenide quantum dot solution is further heated to 235°C, and then the zinc sulfide shell solution is added dropwise, and the temperature is kept for 65 minutes to form a core-shell structure, and then quenched to obtain. The speed of dropwise addition should be controlled at about 0.9 ml / min. The zinc sulfide shell solution is mixed with zinc stearate, n-dodecyl mercaptan and octadecene, and is heated to 180°C under an inert gas atmosphere to dissolve and form. The amount ratio of zinc stearate, n-dodecyl mercaptan, octadecene and copper indium selenide quantum dot solution is 1.5 mmol: 0.3 ml: 1.5 ml: 12 ml.

[0040] The copper indium selenide / zinc sulfide core-shell quantum dot solution was mixed with ethanol and toluene in a volume ratio of 14:7:12, and then centrifuged at 11300 rpm for 7 min to obtain a primary precipitate, appropriate ethanol and toluene were added to the primary precipitate, and the mixture was mixed in a volume ratio of 1:1 to ethanol and toluene, and then centrifuged at 11500 rpm for 7 min to obtain a secondary precipitate, and appropriate ethanol and toluene were added to the secondary precipitate, and the mixture was mixed in a volume ratio of 1:1 to ethanol and toluene, and then centrifuged at 12000 rpm for 7 min to obtain a tertiary precipitate, which was dissolved in a toluene solution for storage.

[0041] Example 3

[0042] A copper indium selenide / zinc sulfide core-shell quantum dot material, the preparation method of which comprises the following steps:

[0043] 0.18 mmol of cuprous iodide, 0.2 mmol of indium acetate, 0.1 mmol of zinc stearate, 9 ml of octadecene and 1 ml of n-dodecyl mercaptan were mixed, and stirred vigorously at 130°C for 20 min under an inert gas atmosphere. Then, 0.6 ml of oleic acid and 0.4 ml of oleylamine were added successively, and degassing was continued for 30 min.

[0044] In an inert gas atmosphere, the mixture was heated to 225°C, and the selenium precursor solution was rapidly injected and kept warm for 30 minutes to obtain a copper indium selenium quantum dot solution. The preparation method of the selenium precursor solution is as follows: 0.5 mmol of selenium powder was dissolved in 0.8 ml of oleylamine and 0.4 ml of n-dodecyl mercaptan, and stirred to fully dissolve.

[0045] The copper indium selenide quantum dot solution is further heated to 230°C, and then the zinc sulfide shell solution is added dropwise, and the temperature is kept for 70 minutes to form a core-shell structure, and then quenched to obtain. The speed of dropwise addition should be controlled at about 1.1 ml / min. The zinc sulfide shell solution is mixed with zinc stearate, n-dodecyl mercaptan and octadecene, and is heated to 200°C under an inert gas atmosphere to dissolve and form. The amount ratio of zinc stearate, n-dodecyl mercaptan, octadecene and copper indium selenide quantum dot solution is 1.7 mmol: 0.5 ml: 1.7 ml: 12 ml.

[0046] The copper indium selenide / zinc sulfide core-shell quantum dot solution was mixed with ethanol and toluene in a volume ratio of 14:7:12, and then centrifuged at 11300 rpm for 7 min to obtain a primary precipitate, appropriate ethanol and toluene were added to the primary precipitate, and the mixture was mixed in a volume ratio of 1:1 to ethanol and toluene, and then centrifuged at 11500 rpm for 7 min to obtain a secondary precipitate, and appropriate ethanol and toluene were added to the secondary precipitate, and the mixture was mixed in a volume ratio of 1:1 to ethanol and toluene, and then centrifuged at 12000 rpm for 7 min to obtain a tertiary precipitate, which was dissolved in a toluene solution for storage.

[0047] Example 4

[0048] A copper indium selenide / zinc sulfide core-shell quantum dot material, the preparation method of which comprises the following steps:

[0049] 0.1 mmol of cuprous iodide, 0.1 mmol of indium acetate, 0.2 mmol of zinc stearate, 10 ml of octadecene and 1.5 ml of n-dodecyl mercaptan were mixed, stirred vigorously at 120°C for 30 min under an inert gas atmosphere, and then 0.5 ml of oleic acid and 0.5 ml of oleylamine were added successively and degassing was continued for 20 min.

[0050] In an inert gas atmosphere, the mixture was heated to 220°C, and the selenium precursor solution was rapidly injected and kept warm for 20 minutes to obtain a copper indium selenium quantum dot solution. The preparation method of the selenium precursor solution is as follows: 0.4 mmol of selenium powder was dissolved in 0.7 ml of oleylamine and 0.3 ml of n-dodecyl mercaptan, and stirred to fully dissolve.

[0051] The copper indium selenide quantum dot solution is further heated to 240°C, and then the zinc sulfide shell solution is added dropwise, and the temperature is kept for 60 minutes to form a core-shell structure, and then quenched to obtain. The speed of dropwise addition should be controlled at about 1 ml / min. The zinc sulfide shell solution is mixed with zinc stearate, n-dodecyl mercaptan and octadecene, and is heated to 190°C under an inert gas atmosphere to dissolve and form. The amount ratio of zinc stearate, n-dodecyl mercaptan, octadecene and copper indium selenide quantum dot solution is 1.6 mmol: 0.4 ml: 1.6 ml: 12 ml.

[0052] The copper indium selenide / zinc sulfide core-shell quantum dot solution was mixed with ethanol and toluene in a volume ratio of 14:7:12, and then centrifuged at 11300 rpm for 7 min to obtain a primary precipitate, appropriate ethanol and toluene were added to the primary precipitate, and the mixture was mixed in a volume ratio of 1:1 to ethanol and toluene, and then centrifuged at 11500 rpm for 7 min to obtain a secondary precipitate, and appropriate ethanol and toluene were added to the secondary precipitate, and the mixture was mixed in a volume ratio of 1:1 to ethanol and toluene, and then centrifuged at 12000 rpm for 7 min to obtain a tertiary precipitate, which was dissolved in a toluene solution for storage.

[0053] Comparative Example 5

[0054] A copper indium selenide / zinc sulfide core-shell quantum dot material, the preparation method of which comprises the following steps:

[0055] 0.18 mmol of cuprous iodide, 0.2 mmol of indium acetate, 10 ml of octadecene and 1 ml of n-dodecyl mercaptan were mixed, and stirred vigorously at 120°C for 30 min under an inert gas atmosphere. Then, 0.5 ml of oleic acid and 0.5 ml of oleylamine were added successively, and degassing was continued for 30 min.

[0056] In an inert gas atmosphere, the mixture was heated to 220°C, and the selenium precursor solution was rapidly injected and kept warm for 20 minutes to obtain a copper indium selenium quantum dot solution. The preparation method of the selenium precursor solution is as follows: 0.4 mmol of selenium powder was dissolved in 0.7 ml of oleylamine and 0.3 ml of n-dodecyl mercaptan, and stirred to fully dissolve.

[0057] The copper indium selenide quantum dot solution is further heated to 230°C, and then the zinc sulfide shell solution is added dropwise, and the temperature is kept for 60 minutes to form a core-shell structure, and then quenched to obtain. The speed of dropwise addition should be controlled at about 1 ml / min. The zinc sulfide shell solution is formed by mixing zinc stearate, n-dodecyl mercaptan and octadecene, and heated to 190°C under an inert gas atmosphere to dissolve. The amount ratio of zinc stearate, n-dodecyl mercaptan, octadecene and copper indium selenide quantum dot solution is 1.6 mmol: 0.4 ml: 1.6 ml: 12 ml.

[0058] The copper indium selenide / zinc sulfide core-shell quantum dot solution was mixed with ethanol and toluene in a volume ratio of 14:7:12, and then centrifuged at 11300 rpm for 7 min to obtain a primary precipitate, appropriate ethanol and toluene were added to the primary precipitate, and the mixture was mixed in a volume ratio of 1:1 to ethanol and toluene, and then centrifuged at 11500 rpm for 7 min to obtain a secondary precipitate, and appropriate ethanol and toluene were added to the secondary precipitate, and the mixture was mixed in a volume ratio of 1:1 to ethanol and toluene, and then centrifuged at 12000 rpm for 7 min to obtain a tertiary precipitate, which was dissolved in a toluene solution for storage.

[0059] Through Comparative Example 5, it is found that the fluorescence efficiency of copper indium selenide quantum dots not doped with zinc ions is greatly reduced, and the copper indium selenide core quantum dots not doped with zinc ions will undergo a larger blue shift after being encapsulated, resulting in an emission wavelength below the near-infrared range of 800nm.

[0060] An indoor near-infrared optical wireless communication test system is designed. Signals are generated based on different modulation methods through an arbitrary waveform generator, loaded onto a laser diode through a microcircuit, and converged through a lens onto the sample of Example 1 encapsulated in a 1 mm thick quartz cuvette. After being focused by the lens and filtered out by a filter, the light is received by a photodetector. Finally, an oscilloscope is used to demodulate the digital signal to obtain an eye diagram and a target signal waveform, and the bit error rate is calculated.

[0061] from Figure 1 It can be seen that the quantum dot TEM images are mostly triangles and quadrilaterals. This is because the quantum dots we synthesized have a pyramid shape.

[0062] from Figure 2 It can be seen that the quantum dots we synthesized have broad and extensive absorption and efficient fluorescence quantum yield in the near-infrared band.

[0063] Figure 3 It is a schematic diagram of a system for testing the performance of near-infrared light wireless communication.

[0064] from Figure 4 It can be seen that a wider -3db modulation bandwidth was tested using synthesized high-efficiency copper indium selenide / zinc sulfide quantum dots.

[0065] Although the specific implementation of the present invention is described in detail in conjunction with the drawings, it should not be understood as limiting the scope of protection of this patent. Within the scope described in the claims, various modifications and variations that can be made by those skilled in the art without creative work still fall within the scope of protection of this patent.

Claims

1. A method for preparing copper indium selenide / zinc sulfide core-shell quantum dots, characterized in that: The following steps are involved: S1. After mixing cuprous iodide, indium acetate, zinc stearate, octadecene and n-dodecyl mercaptan, the mixture was heated to 110°C to 130°C under an inert gas atmosphere and stirred vigorously, and then oleic acid and oleylamine were added successively to continue degassing; S2. The mixture obtained in step S1 is heated to 215°C to 225°C, and a selenium precursor solution is rapidly injected thereinto and kept warm to obtain a copper indium selenium quantum dot solution; S3. The copper indium selenide quantum dot solution obtained in step S2 is further heated to 230°C to 240°C, and then the zinc sulfide shelling solution is added dropwise and kept warm. After the core-shell structure is formed, the solution is quenched and purified to obtain the product.

2. The method for preparing copper indium selenide / zinc sulfide core-shell quantum dots according to claim 1, characterized in that: In step S1, the usage ratio of cuprous iodide, indium acetate, zinc stearate, octadecene, n-dodecyl mercaptan, oleic acid and oleylamine is 0.1mmol~0.2mmol:0.1mmol~0.2mmol:0.1mmol~0.2mmol:9~11ml:0.5~1.5ml:0.4~0.6ml:0.4~0.6ml.

3. The method for preparing copper indium selenide / zinc sulfide core-shell quantum dots according to claim 2, characterized in that: In step S1, the usage ratio of cuprous iodide, indium acetate, zinc stearate, octadecene, n-dodecyl mercaptan, oleic acid and oleylamine is 0.18 mmol: 0.2 mmol: 0.14 mmol: 10 ml: 1 ml: 0.5 ml: 0.5 ml.

4. The method for preparing copper indium selenide / zinc sulfide core-shell quantum dots according to claim 1, characterized in that: In step S1, the stirring time is 20 to 30 minutes, and the degassing time is 20 to 30 minutes.

5. The method for preparing copper indium selenide / zinc sulfide core-shell quantum dots according to claim 1, characterized in that: The insulation time in step S2 is 20 to 30 minutes.

6. The method for preparing copper indium selenide / zinc sulfide core-shell quantum dots according to claim 1, characterized in that: The selenium precursor solution in step S2 is prepared by the following steps: dissolving selenium powder in a mixture of oleylamine and n-dodecyl mercaptan, stirring to fully dissolve, and obtaining a selenium precursor solution. The amount ratio of the selenium powder, oleylamine, n-dodecyl mercaptan and the mixture obtained in step S1 is 0.3-0.5 mmol: 0.6-0.8 ml: 0.2-0.4 ml: 10-13 ml.

7. The method for preparing copper indium selenide / zinc sulfide core-shell quantum dots according to claim 1, characterized in that: The zinc sulfide shell solution in step S3 is prepared by the following steps: zinc stearate, n-dodecyl mercaptan and octadecene are mixed, and heated to 180-200° C. under an inert gas atmosphere to dissolve and form, and the amount ratio of zinc stearate, n-dodecyl mercaptan, octadecene and copper indium selenide quantum dot solution is 1.5-1.7 mmol: 0.3-0.5 ml: 1.5-1.7 ml: 10-13 ml.

8. The method for preparing copper indium selenide / zinc sulfide core-shell quantum dots according to claim 1, characterized in that: In step S3, the dropwise addition rate is about 0.9 to 1.1 ml / min, and the insulation time is 60 to 70 min.

9. Copper indium selenide / zinc sulfide core-shell quantum dots prepared according to the preparation method according to any one of claims 1 to 8.

10. Application of the copper indium selenide / zinc sulfide core-shell quantum dots according to claim 9 in near-infrared light wireless communication.