Derivative fuel based on waste EVA and preparation method thereof
By mixing EVA waste with other waste in a specific proportion and hot-pressing form, high-calorie derivative fuel is prepared, which solves the problem of secondary pollution and resource utilization in the EVA recycling process, and realizes the resource utilization of EVA and improve fuel stability, providing new solutions to energy conservation and carbon reduction.
Patent Information
- Application Number
- CN202411168347.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-12
AI Technical Summary
There are problems of secondary pollution and resource utilization during the existing EVA recycling process, resulting in limited EVA application scenarios and the inability to completely realize EVA reduction.
Using a method of producing derivative fuel based on waste EVA, the EVA waste is mixed with combustible materials, agricultural and forestry waste, combustion aids, compatibilizers and oxidants in a specific proportion, and the high-calorie derivative fuel is prepared through the hot pressing molding process, using To replace fuel from coal-fired power plants, the addition of strong acids or strong alkalis is avoided to change the properties of EVA, and the derived fuel formed does not produce harmful gases after combustion.
The resource utilization of EVA has been achieved, the stability and utilization rate of derivative fuels have been improved, the impact of fuel carbon emissions on the environment has been reduced, and a new solution for energy saving and carbon reduction has been provided. It has also been added to reduce the The viscosity of the fuel is improved and the drop strength of the fuel is improved.
Smart Images

Figure CN118931610A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of environmentally friendly new energy, and in particular to a derivative fuel based on waste EVA and a preparation method thereof. Background Art
[0002] EVA (ethylene-vinyl acetate copolymer) is a general-purpose plastic widely used in photovoltaics, footwear, adhesives and other fields. According to statistics, photovoltaic modules contain about 5% EVA by mass. In recent years, a large number of photovoltaic modules have reached the retirement period of 25 years, which will generate a large number of discarded photovoltaic modules.
[0003] In addition to the use of EVA film in photovoltaic module production (accounting for 33% of the market), EVA is also used in industrial production processes such as foamed shoe materials, functional greenhouse films, packaging films, hot melt adhesives, wires and cables, and toys. These products still have waste such as recycled materials or scraps in their entire life cycle. If not properly disposed of, it will cause serious environmental pollution. At present, there have been many reports on the recycling of EVA waste. For example: CN114181448A discloses a method for preparing low-temperature EVA and a method for recycling resources using low-temperature EVA, wherein metallocene polyethylene, calcium stabilizer, peroxide, antioxidant, toughening agent and lubricant are added to the EVA in the solar cell module, and the mixture is melt-extruded and molded, and the compounded EVA can be reused; CN113980348A discloses a method for preparing meltable EVA recycled material, meltable EVA recycled material and its application, wherein cross-linked EVA plastic is pre-treated by swelling with a weak acid or weak base solvent, then fused with an antioxidant, and finally melt-extruded and granulated to form EVA recycled particles; CN115975114A discloses a method for preparing core-shell structured EVA particles by recycling EVA waste and its application, wherein thermoplastic and cross-linked EVA are ground into powder, aromatic hydrocarbons are added for swelling, and then reactive monomers are added to finally prepare core-shell EVA powder having a cross-linked EVA core and a reactive monomer shell, which can be used for plastic toughening or foaming material filling.
[0004] The above recycling methods all classify EVA waste before recycling. The source of waste is relatively single, and antioxidants and other swellable EVA are added during the recycling process. Waste gas may be generated during the recycling process, causing secondary pollution. The recycled products also have problems such as unstable quality, which limits the application scenarios of the recycled EVA and makes it impossible to completely achieve EVA reduction. Summary of the invention
[0005] The present invention aims to provide a derivative fuel based on waste EVA and a preparation method thereof, so as to solve the problems of secondary pollution and limited resource utilization in the EVA recovery process in the prior art.
[0006] To achieve the above-mentioned purpose, the present invention adopts the following technical scheme: a derivative fuel based on waste EVA, which includes, by mass, 40 to 60 parts of EVA waste, 10 to 30 parts of combustibles, 10 to 30 parts of agricultural and forestry wastes, 1 to 10 parts of combustion aids, 1 to 10 parts of volume extenders, 1 to 5 parts of oxidants, and 0.1 to 1 parts of inhibitors.
[0007] Preferably, as an improvement, the EVA waste is at least one of hot knife method EVA waste, irradiation pulse method EVA waste, physical disassembly method EVA waste, chemical dissolution method EVA waste, and EVA scraps in industrial production.
[0008] Preferably, as an improvement, the combustion aid includes the following raw materials in parts by weight: 40-50 parts of calcium oxide, 10-20 parts of water-soluble silicate, 5-10 parts of activated carbon, 1-5 parts of magnesium hydroxide, 1-5 parts of manganese dioxide, 1-5 parts of saltpeter, 1-5 parts of sodium bicarbonate, 1-5 parts of potassium bicarbonate, 1-5 parts of bentonite, 1-5 parts of boron powder, and 1-5 parts of aluminum oxide.
[0009] Preferably, as an improvement, the compatibilizer is at least one of maleic anhydride graft copolymer, dioctyl phthalate, stearic acid, zinc stearate, polycarbonate, polyethylene acrylate, and aluminum stearate.
[0010] Preferably, as an improvement, the oxidant is at least one of potassium permanganate, calcium peroxide, sodium percarbonate and potassium perborate.
[0011] Preferably, as an improvement, the inhibitor is at least one of a surfactant, a Tween polymer, a high molecular weight polymer, and an organic compound.
[0012] Preferably, as an improvement, the inhibitor is at least one of rhamnolipid, trehalose lipid, betaine, span, Tween polymer, polyacrylamide, polyvinyl alcohol, ethylene oxide, lanolin and lecithin.
[0013] Preferably, as an improvement, a method for preparing a derived fuel based on waste EVA comprises the following steps:
[0014] S1 Raw material acquisition: prepare waste EVA, combustibles, agricultural and forestry wastes, combustion aids, polymerization inhibitors, volume extenders and oxidants according to the weight ratio requirements and set them aside;
[0015] S2 Coarse crushing: crush EVA waste into particles with a particle size of ≤5mm to make EVA recycling waste; crush combustibles and agricultural and forestry waste into particles with a particle size of ≤5mm for standby use;
[0016] S3 de-crosslinking: mixing EVA waste, compatibilizer and inhibitor to prepare de-crosslinked EVA waste;
[0017] S4 fine crushing: Use a low-temperature crusher to crush the de-crosslinked EVA waste, control the crushing temperature to less than 40°C, and crush the EVA waste to a particle size of ≤1mm
[0018] S5 stirring and mixing: mixing the above powder, screened combustibles, agricultural and forestry wastes, combustion aids, and oxidants according to proportions;
[0019] S6 hot pressing: The raw materials are extruded and formed using a twin-screw granulator to obtain the finished RDF / SRF derived fuel.
[0020] Preferably, as an improvement, in step S2, the mass ratio of EVA fertilizer, solubilizer and inhibitor is: 100:1-10:0.1-1.
[0021] Preferably, as an improvement, in step S6, the extrusion molding process adopts a hot pressing molding process with a temperature of 80 to 100° C. and a pressure of 15 to 30 MPa.
[0022] The principle and advantage of this solution are: in actual application, waste EVA is usually used to prepare foaming agents, etc., and this technical solution breaks away from the barriers of the existing technology, creatively uses waste EVA as a raw material to obtain high calorific value derivative fuels, and turns EVA into a resource, providing a new alternative fuel solution for coal-fired power plants. In the prior art, inhibitors and compatibilizers are usually added to hinder the reaction of molecules with free radicals to form non-free radical substances or low-activity free radicals that cannot be triggered. The purpose of the compatibilizer is to reduce interfacial tension and promote dispersion; improve the interfacial adhesion between components and improve the mechanical properties of the blend. In this technical solution, by adding inhibitors and compatibilizers, the viscosity of the fuel can be effectively reduced, while the drop strength of the fuel can be improved. In addition, this solution scientifically proportions EVA and other solid wastes, and improves the subsequent utilization efficiency through the interaction between the raw materials. The derivative fuel preparation method of the present invention is simple, easy to operate, suitable for large-scale mass production, does not add strong acid, strong alkali and other substances to change the properties of EVA, and the derivative fuel formed does not produce harmful gases after combustion, is safe and environmentally friendly, and can achieve the reduction of EVA film and improve the stability and utilization rate of the derivative fuel. At the same time, it can provide a new solution for energy conservation and carbon reduction, and reduce the impact of fuel carbon emissions on the environment.
[0023] In the technical research and development stage, the determination of the EVA ratio is one of the difficulties of this technical solution: if the EVA content exceeds 60%, the fuel rod cannot be formed, and it will melt and wrap the remaining mixture during the pressing process; the polymerization inhibitor, the compatibilizer and the combustion aid are formulated. The reasonable addition of the three makes EVA more combustible and improves the burnout performance of EVA. Technical obstacles: reduce the possibility of EVA melting. In order to make EVA fully mixed with polymerization inhibitors and other additives to play a role, the additives are mixed first, then mixed with the remaining components, and finally pressed at a controlled temperature. Temperature control is very important. When the EVA content is high, the pressing temperature should be appropriately lowered to avoid EVA melting and sticking. In addition, the study also found that the combination of EVA and agricultural and forestry waste can promote the degradation of macromolecular polymers, inhibit the condensation process of small molecules in synergistic pyrolysis and the removal of oxygen-containing functional groups and hydrogen atoms, and has unexpected technical effects. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The figure is a flow chart of the preparation process of the derivative fuel based on waste EVA according to the present invention. DETAILED DESCRIPTION
[0025] The following is further described in detail through specific implementations, but the implementation of the present invention is not limited thereto. Unless otherwise specified, the technical means used in the following implementations are conventional means well known to those skilled in the art; the experimental methods used are all conventional methods; the materials, reagents, etc. used can all be obtained from commercial channels.
[0026] A derivative fuel based on waste EVA comprises, by weight, 40 to 60 parts of EVA waste, 10 to 30 parts of screened combustibles, 10 to 30 parts of agricultural and forestry wastes, 1 to 10 parts of combustion aids, 1 to 10 parts of volume extenders, 1 to 5 parts of oxidants, and 0.1 to 1 part of polymerization inhibitors.
[0027] EVA waste mainly comes from two categories. Waste EVA obtained from dismantling photovoltaic modules can come from methods such as hot knife method, irradiation method, physical disassembly method, chemical dissolution method, etc., but not limited to the waste EVA obtained by the above methods; EVA scraps in industrial production can come from EVA produced in the production process of shoe factories, functional greenhouse films, packaging films, hot melt adhesives, wires and cables, and toys, but not limited to the above methods. EVA also includes thermoplastic EVA waste and cross-linked EVA waste.
[0028] The combustible materials after screening mainly refer to dry garbage except food waste sorted from domestic garbage by manual or mechanical means, removing non-combustible impurities such as metal, glass, ceramic and stone. After sorting, they mainly contain waste paper, plastic (including PP, PVC, PE, PS, PET and HDPE, but not limited to the listed plastics), rubber, leather, textiles, and wood and bamboo waste combustibles, which mainly provide fibers, plastics and proteins for derived fuels.
[0029] Agricultural and forestry waste comes from furniture factories, edible fungus factories, garden waste, or agricultural production (straw, peanut shells, rice husks, wheat bran, etc.), and contains a large amount of cellulose and hemicellulose.
[0030] The combustion aid includes the following raw materials in parts by weight: 40-50 parts of calcium oxide, 10-20 parts of water-soluble silicate, 5-10 parts of activated carbon, 1-5 parts of magnesium hydroxide, 1-5 parts of manganese dioxide, 1-5 parts of saltpeter, 1-5 parts of sodium bicarbonate, 1-5 parts of potassium bicarbonate, 1-5 parts of bentonite, 1-5 parts of boron powder, and 1-5 parts of aluminum oxide.
[0031] The compatibilizer is at least one of maleic anhydride graft copolymer, dioctyl phthalate, stearic acid, zinc stearate, polycarbonate, polyethylene acrylate, and aluminum stearate.
[0032] The oxidant is at least one of potassium permanganate, calcium peroxide, sodium percarbonate and potassium perborate.
[0033] The inhibitor is a biosurfactant, a surfactant, a Tween polymer, a high molecular weight polymer or an organic compound, specifically at least one of rhamnolipid, trehalose lipid, betaine, span, Tween polymer, polyacrylamide, polyvinyl alcohol, ethylene oxide, lanolin and lecithin.
[0034] like Figure 1 As shown, a method for preparing a derivative fuel based on waste EVA comprises the following steps:
[0035] S1 Raw material acquisition: prepare waste EVA, screened combustibles, agricultural and forestry wastes, combustion aids, polymerization inhibitors, volume extenders and oxidants according to the weight ratio requirements and set them aside;
[0036] S2 Coarse crushing: crush the EVA waste into particles with a particle size of ≤5mm to make EVA recycling waste; crush the screened combustibles and agricultural and forestry wastes into particles with a particle size of ≤5mm for standby use;
[0037] S3 de-crosslinking: 100 parts by weight of the above-mentioned EVA waste are mixed with 1 to 10 parts by weight of a compatibilizer and 0.1 to 1 part by weight of a polymerization inhibitor to prepare de-crosslinked EVA waste;
[0038] S4 fine crushing: Use a low-temperature crusher to crush the de-crosslinked EVA waste, control the crushing temperature to less than 40°C, and crush the EVA waste to a particle size of ≤1mm;
[0039] S5 stirring and mixing: putting the above powder, screened combustibles, agricultural and forestry wastes, combustion aids, and oxidants in different proportions into a closed container and stirring and mixing at room temperature to make the de-crosslinked EVA powder fully contact with the remaining raw materials;
[0040] S6 hot pressing: The raw materials are extruded and formed by a twin-screw granulator, and the hot pressing process is used. The temperature is controlled at 80-100°C and the pressure is 15-30MPa, and the finished RDF / SRF derivative fuel is finally obtained. In order to prevent EVA from melting and sticking, the inside of the granulator is made of 304 stainless steel and coated with polytetrafluoroethylene.
[0041] The EVA-derived fuel particles prepared by the above method are used in coal-fired power plants, cement kiln boilers and other coal-using boilers to replace coal or are used for pyrolysis to produce gas as combustible gas.
[0042] Example 1
[0043] A derivative fuel based on waste EVA comprises, by weight, 50 parts of EVA waste, 20 parts of screened combustibles, 20 parts of agricultural and forestry wastes, 2 parts of combustion aids, 5 parts of volume extenders, 2.7 parts of oxidants, and 0.3 parts of inhibitors.
[0044] Furthermore, EVA waste comes from EVA obtained by any one or more methods including physical method, chemical method, irradiation method and thermal conductivity method in the recycling process of photovoltaic modules; the screened combustibles are domestic waste that has been screened to remove non-combustible impurities such as metal, glass, ceramic and stone, and after sorting, it mainly contains combustibles such as waste paper, plastic (including PP, PVC, PE, PS, PET and HDPE, but not limited to the listed plastics), rubber, leather, textiles, wood and bamboo waste, etc., which mainly provide fiber, plastic, protein and other substances for derived fuels; agricultural and forestry waste is garden waste.
[0045] The combustion aid is composed of 45 parts of calcium oxide, 10 parts of water-soluble silicate, 10 parts of activated carbon, 5 parts of magnesium hydroxide, 5 parts of manganese dioxide, 5 parts of saltpeter, 5 parts of sodium bicarbonate, 5 parts of potassium bicarbonate, 5 parts of bentonite, 2 parts of boron powder and 3 parts of aluminum oxide.
[0046] The compatibilizer is dioctyl phthalate.
[0047] The oxidizing agent is potassium permanganate.
[0048] The inhibitor is a mixture of rhamnolipid, polyvinyl alcohol and lanolin in a mass ratio of 1:1:1.
[0049] A method for preparing a derivative fuel from EVA comprises the following steps:
[0050] S1 Raw material acquisition: prepare waste EVA, screened combustibles, agricultural and forestry wastes, combustion aids, polymerization inhibitors, volume extenders and oxidants according to the weight ratio requirements and set them aside;
[0051] S2 Coarse crushing: crush the EVA waste into particles with a particle size of ≤5mm to make EVA recycling waste; crush the screened combustibles and agricultural and forestry wastes into particles with a particle size of ≤5mm for standby use;
[0052] S3 de-crosslinking: 50 parts by weight of the above-mentioned EVA waste are mixed with 5 parts by weight of a compatibilizer and 0.3 parts by weight of a polymerization inhibitor to prepare de-crosslinked EVA waste;
[0053] S4 fine crushing: Use a low-temperature crusher to crush the de-crosslinked EVA waste, control the crushing temperature to less than 40°C, and crush the EVA waste to a particle size of ≤1mm;
[0054] S5 stirring and mixing: putting the above powder, screened combustibles, agricultural and forestry wastes, combustion aids, and oxidants in different proportions into a closed container and stirring and mixing at room temperature to make the de-crosslinked EVA powder fully contact with the remaining raw materials;
[0055] S6 hot pressing: The raw materials are extruded and formed by a twin-screw granulator, and the hot pressing process is used. The temperature is controlled at 80°C and the pressure is 20MPa. Finally, the finished product EVA content is greater than 40% of the derived fuel. In order to prevent EVA from melting and sticking, the inside of the granulator is made of 304 stainless steel and coated with polytetrafluoroethylene.
[0056] The EVA derivative fuel prepared above can be used in cement kiln incinerators and thermal power plants as a coal substitute. The lower calorific value of the derivative fuel is 33.4MJ / kg and the chlorine content is 0.5%, which complies with the group standard "Solid Alternative Fuels for Thermal Power Generation" (T / CIC048-2021).
[0057] Example 2
[0058] A derivative fuel based on waste EVA comprises, by weight, 40 parts of EVA waste, 20 parts of screened combustibles, 35 parts of agricultural and forestry wastes, 2 parts of combustion aids, 2 parts of volume extenders, 0.8 parts of oxidants, and 0.2 parts of inhibitors.
[0059] Furthermore, EVA waste comes from EVA waste generated in the production processes of shoe factories, functional greenhouse films, packaging films, hot melt adhesives, wires and cables, and toys in industrial production; the screened combustibles are domestic waste that has been screened to remove non-combustible impurities such as metals, glass, ceramics, and stones. After sorting, it mainly contains combustibles such as waste paper, plastics (including PP, PVC, PE, PS, PET, and HDPE, but not limited to the listed plastics), rubber, leather, textiles, and wood and bamboo waste, which mainly provide fiber, plastic, protein and other substances for derived fuels; agricultural and forestry waste is garden waste.
[0060] The combustion aid is composed of 50 parts of calcium oxide, 18 parts of water-soluble silicate, 12 parts of activated carbon, 2 parts of magnesium hydroxide, 2 parts of manganese dioxide, 2 parts of saltpeter, 2 parts of sodium bicarbonate, 5 parts of potassium bicarbonate, 2 parts of bentonite, 2 parts of boron powder and 3 parts of aluminum oxide.
[0061] The compatibilizer is a mixture of maleic anhydride graft copolymer and stearic acid in a mass ratio of 1:3.
[0062] The oxidant is a mixture of calcium peroxide and sodium percarbonate in a mass ratio of 1:1.
[0063] The inhibitor is rhamnolipid.
[0064] A method for preparing a derivative fuel from EVA comprises the following steps:
[0065] S1 Raw material acquisition: prepare waste EVA, screened combustibles, agricultural and forestry wastes, combustion aids, polymerization inhibitors, volume extenders and oxidants according to the weight ratio requirements and set them aside;
[0066] S2 Coarse crushing: crush the EVA waste into particles with a particle size of ≤5mm to make EVA recycling waste; crush the screened combustibles and agricultural and forestry wastes into particles with a particle size of ≤5mm for standby use;
[0067] S3 de-crosslinking: 40 parts by weight of the above-mentioned EVA waste are mixed with 2 parts by weight of a compatibilizer and 0.2 parts by weight of a polymerization inhibitor to prepare de-crosslinked EVA waste;
[0068] S4 fine crushing: Use a low-temperature crusher to crush the de-crosslinked EVA waste, control the crushing temperature to less than 40°C, and crush the EVA waste to a particle size of ≤1mm;
[0069] S5 stirring and mixing: putting the above powder, screened combustibles, agricultural and forestry wastes, combustion aids, and oxidants in different proportions into a closed container and stirring and mixing at room temperature to make the de-crosslinked EVA powder fully contact with the remaining raw materials;
[0070] S6 hot pressing: The raw materials are extruded and formed by a twin-screw granulator, and the hot pressing process is used. The temperature is controlled at 100°C and the pressure is 22MPa. Finally, the finished product EVA content is greater than 40% of the derived fuel. In order to prevent EVA from melting and sticking, the inside of the granulator is made of 304 stainless steel and coated with polytetrafluoroethylene.
[0071] The EVA derivative fuel prepared above can be used in cement kiln incinerators and thermal power plants as a coal substitute. The lower calorific value of the derivative fuel is 31.2MJ / kg and the chlorine content is 0.65%, which complies with the group standard "Solid Alternative Fuels for Thermal Power Generation" (T / CIC048-2021).
[0072] Example 3
[0073] A derivative fuel based on waste EVA, which comprises, by weight, 60 parts of EVA waste, 10 parts of screened combustibles, 10 parts of agricultural and forestry wastes, 10 parts of combustion aids, 6 parts of volume extenders, 3.4 parts of oxidants, and 0.6 parts of inhibitors.
[0074] EVA waste comes from EVA waste generated in the production processes of shoe factories, functional shed films, packaging films, hot melt adhesives, wires and cables, and toys in industrial production; the combustibles after screening are made from domestic waste that has been screened to remove non-combustible impurities such as metal, glass, ceramics, and stones. After sorting, it mainly contains combustibles such as waste paper, plastics (including PP, PVC, PE, PS, PET, and HDPE, but not limited to the listed plastics), rubber, leather, textiles, and wood and bamboo waste, which mainly provide fiber, plastic, protein and other substances for derived fuels; agricultural and forestry waste refers to agricultural production waste (straw, peanut shells, rice husks, and wheat bran).
[0075] The combustion aid is composed of 40 parts of calcium oxide, 15 parts of water-soluble silicate, 15 parts of activated carbon, 5 parts of magnesium hydroxide, 5 parts of manganese dioxide, 5 parts of saltpeter, 5 parts of sodium bicarbonate, 5 parts of potassium bicarbonate, 5 parts of bentonite, 2 parts of boron powder and 3 parts of aluminum oxide.
[0076] The compatibilizer is a mixture of dioctyl phthalate, stearic acid, zinc stearate, polycarbonate, polyethylene acrylate and aluminum stearate in equal mass ratios.
[0077] The oxidant is a mixture of potassium permanganate and calcium peroxide in equal mass ratio.
[0078] The inhibitor is trehalose lipid.
[0079] A method for preparing a derivative fuel from EVA comprises the following steps:
[0080] S1 Raw material acquisition: prepare waste EVA, screened combustibles, agricultural and forestry wastes, combustion aids, polymerization inhibitors, volume extenders and oxidants according to the weight ratio requirements and set them aside;
[0081] S2 Coarse crushing: crush the EVA waste into particles with a particle size of ≤5mm to make EVA recycling waste; crush the screened combustibles and agricultural and forestry wastes into particles with a particle size of ≤5mm for standby use;
[0082] S3 de-crosslinking: 60 parts by weight of the above-mentioned EVA waste are mixed with 6 parts by weight of a compatibilizer and 0.6 parts by weight of a polymerization inhibitor to prepare de-crosslinked EVA waste;
[0083] S4 fine crushing: Use a low-temperature crusher to crush the de-crosslinked EVA waste, control the crushing temperature to less than 40°C, and crush the EVA waste to a particle size of ≤1mm;
[0084] S5 stirring and mixing: putting the above powder, screened combustibles, agricultural and forestry wastes, combustion aids, and oxidants in different proportions into a closed container and stirring and mixing at room temperature to make the de-crosslinked EVA powder fully contact with the remaining raw materials;
[0085] S6 hot pressing: The raw materials are extruded and formed by a twin-screw granulator, and the hot pressing process is used. The temperature is controlled at 100°C and the pressure is 15MPa, and the finished derivative fuel is finally obtained. To prevent EVA from melting and sticking, the inside of the granulator is lined with 304 stainless steel and coated with polytetrafluoroethylene.
[0086] The EVA derived fuel prepared above can be used for pyrolysis to produce gas. The gas-liquid-solid ratio of the pyrolysis product is 30:64:5, and the gas is mainly H 2 , CO 2 (dominant), CH 4 and C2-C3 olefins and alkanes. The liquid products are mainly alcohols, aldehydes, ketones and acid esters. The solid is mainly coke. The specific surface area of the carbon structure is 3.561m 2 / g, pore volume 0.0245cm 3 / g, the char after pyrolysis still has good potential as solid fuel.
[0087] Example 4
[0088] A derivative fuel based on waste EVA, which comprises, by weight, 40 parts of EVA waste, 20 parts of screened combustibles, 20 parts of agricultural and forestry wastes, 10 parts of combustion aids, 4 parts of volume extenders, 5.6 parts of oxidants, and 0.4 parts of inhibitors.
[0089] EVA waste comes from EVA waste generated in the production processes of shoe factories, functional shed films, packaging films, hot melt adhesives, wires and cables, and toys in industrial production; the combustibles after screening are made from domestic waste that has been screened to remove non-combustible impurities such as metal, glass, ceramics, and stones. After sorting, it mainly contains combustibles such as waste paper, plastics (including PP, PVC, PE, PS, PET, and HDPE, but not limited to the listed plastics), rubber, leather, textiles, and wood and bamboo waste, which mainly provide fiber, plastic, protein and other substances for derived fuels; agricultural and forestry waste refers to agricultural production waste (straw, peanut shells, rice husks, and wheat bran).
[0090] The combustion aid is composed of 40 parts of calcium oxide, 20 parts of water-soluble silicate, 10 parts of activated carbon, 5 parts of magnesium hydroxide, 5 parts of manganese dioxide, 5 parts of saltpeter, 5 parts of sodium bicarbonate, 5 parts of potassium bicarbonate, 5 parts of bentonite, 2 parts of boron powder and 3 parts of aluminum oxide.
[0091] The compatibilizer is a mixture of stearic acid and zinc stearate in a mass ratio of 1:1.
[0092] The oxidizing agent is potassium perborate.
[0093] The inhibitor is trehalose lipid.
[0094] A method for preparing a derived fuel based on waste EVA comprises the following steps:
[0095] S1 Raw material acquisition: prepare waste EVA, screened combustibles, agricultural and forestry wastes, combustion aids, polymerization inhibitors, volume extenders and oxidants according to the weight ratio requirements and set them aside;
[0096] S2 Coarse crushing: crush the EVA waste into particles with a particle size of ≤5mm to make EVA recycling waste; crush the screened combustibles and agricultural and forestry wastes into particles with a particle size of ≤5mm for standby use;
[0097] S3 de-crosslinking: 40 parts by weight of the above-mentioned EVA waste are mixed with 4 parts by weight of a compatibilizer and 0.4 parts by weight of a polymerization inhibitor to prepare de-crosslinked EVA waste;
[0098] S4 fine crushing: crushing the above-mentioned de-crosslinked EVA waste into a particle size of ≤200 μm, and grinding it into powder;
[0099] S5 stirring and mixing: putting the above powder, screened combustibles, agricultural and forestry wastes, combustion aids, and oxidants in different proportions into a closed container and stirring and mixing at room temperature to make the de-crosslinked EVA powder fully contact with the remaining raw materials;
[0100] S6 hot pressing: The raw materials are extruded and formed by a twin-screw granulator, and the hot pressing process is used. The temperature is controlled at 120℃ and the pressure is 25MPa, and the finished derivative fuel is finally obtained. In order to prevent EVA from melting and sticking, the inside of the granulator is made of 304 stainless steel and coated with polytetrafluoroethylene.
[0101] The EVA derived fuel prepared above can be used for pyrolysis to produce gas. The gas-liquid-solid ratio of the pyrolysis product is 38:54:7, and the gas is mainly H 2 , CO 2 , CH 4 and C2-C3 olefins and alkanes. The liquid products are mainly alcohols, aldehydes, ketones and acid esters. The solid is mainly coke. The specific surface area is 5.903m 2 / g, pore volume 0.0181cm 3 / g, the char after pyrolysis still has good potential as solid fuel.
[0102] Experimental Example 1: Analysis of main raw materials
[0103] Elemental analysis was performed on waste EVA, combustibles, and agricultural and forestry waste. The elemental analysis was performed according to the national standard GB476-91, and an automatic elemental analyzer was used to analyze the C, H, N, and S elements in the samples. The O element content was analyzed using the subtraction method, using 100 to subtract C, H, N, S, moisture, and ash content to obtain the O element content on an air-dried basis. The analysis results are shown in Table 1:
[0104] Table 1
[0105]
[0106] Experimental Example 2
[0107] The mechanical properties and combustion performance tests were carried out on the fuels prepared in the above embodiments, and the drop strength, ignition performance and low calorific value were tested. The drop strength reference method was MT / T2004, which was measured by the falling ball test method; the ignition temperature was measured by the Shimadzu differential thermal-thermogravimetric analysis device (model) of Japan. The RDF was ground and powdered, and 3-5 mg of the sample was taken and placed in an Al2O3 crucible. The heating rate was 10K / min, the final temperature was 1073K, and the air flow rate was 30ml / min. The low calorific value was measured by the GB / T212-2008 "Industrial Analysis Method of Coal" test method. The specific experimental results are shown in Table 2.
[0108] Table 2
[0109] Table 2
[0110]
[0111] It can be seen from the data in Table 2 that the derivative fuel product obtained in the embodiment has high drop resistance and high calorific value. Therefore, the EVA derivative fuel product of the present invention has excellent performance characteristics such as high drop resistance and high calorific value.
[0112] Experimental Example 3
[0113] Comparing Example 3 and Example 4, different addition ratios of EVA and agricultural and forestry waste will lead to different solid-liquid-gas ratios produced by pyrolysis. When the ratio of EVA to agricultural and forestry waste is 6:1, the gas produced is C 3 H 6 When the ratio of EVA to agricultural and forestry waste is 2:1, the C 3 H 6 The proportion of EVA is significantly reduced. This is because the C=C bond of EVA breaks during the pyrolysis process to generate C3 monomers, while the cellulose in the agricultural and forestry biomass undergoes dehydrogenation or glycosidic bond cleavage to generate pyrolysis intermediates with carboxyl and carbonyl groups during the secondary condensation process of reforming reaction. Therefore, as the proportion of agricultural and forestry biomass increases, the gaseous products tend to be short-chain hydrocarbons (C1~C2). In addition, the synergistic effect between EVA and cellulose can promote the degradation of macromolecular polymers, inhibit the condensation process of small molecules in the synergistic pyrolysis and the removal of oxygen-containing functional groups and hydrogen atoms, resulting in more O and H remaining in the system pyrolysis charcoal, increasing the solid ratio. Therefore, the solid-liquid ratio can be adjusted by controlling the ratio of EVA and agricultural and forestry biomass, thereby achieving purposeful industrial applications.
[0114] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions and / or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several modifications and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.
Claims
1. A derivative fuel based on waste EVA, characterized in that: Calculated by mass, it includes 40-60 parts of EVA waste, 10-30 parts of combustibles, 10-30 parts of agricultural and forestry wastes, 1-10 parts of combustion aids, 1-10 parts of volume extenders, 1-5 parts of oxidants, and 0.1-1 parts of inhibitors.
2. A derived fuel based on waste EVA according to claim 1, characterized in that: The EVA waste is at least one of hot knife method EVA waste, irradiation pulse method EVA waste, physical disassembly method EVA waste, chemical dissolution method EVA waste, and EVA scraps in industrial production.
3. A derived fuel based on waste EVA according to claim 2, characterized in that: The combustion aid includes the following raw materials in parts by weight: 40-50 parts of calcium oxide, 10-20 parts of water-soluble silicate, 5-10 parts of activated carbon, 1-5 parts of magnesium hydroxide, 1-5 parts of manganese dioxide, 1-5 parts of saltpeter, 1-5 parts of sodium bicarbonate, 1-5 parts of potassium bicarbonate, 1-5 parts of bentonite, 1-5 parts of boron powder, and 1-5 parts of aluminum oxide.
4. A derived fuel based on waste EVA according to claim 3, characterized in that: The compatibilizer is at least one of maleic anhydride graft copolymer, dioctyl phthalate, stearic acid, zinc stearate, polycarbonate, polyethylene acrylate, and aluminum stearate.
5. A derived fuel based on waste EVA according to claim 4, characterized in that: The oxidant is at least one of potassium permanganate, calcium peroxide, sodium percarbonate and potassium perborate.
6. A derived fuel based on waste EVA according to claim 5, characterized in that: The polymerization inhibitor is at least one of a surfactant, a Tween polymer, a high molecular weight polymer, and an organic compound.
7. A derived fuel based on waste EVA according to claim 6, characterized in that: The inhibitor is at least one of rhamnolipid, trehalose lipid, betaine, span, Tween polymer, polyacrylamide, polyvinyl alcohol, ethylene oxide, lanolin and lecithin.
8. A method for preparing a derived fuel based on waste EVA according to any one of claims 1 to 7, characterized in that: The steps include: S1 Raw material acquisition: prepare waste EVA, combustibles, agricultural and forestry wastes, combustion aids, polymerization inhibitors, volume extenders and oxidants according to the weight ratio requirements and set them aside; S2 Coarse crushing: crush EVA waste into particles with a particle size of ≤5mm to make EVA recycling waste; crush combustibles and agricultural and forestry waste into particles with a particle size of ≤5mm for standby use; S3 de-crosslinking: mixing EVA waste, compatibilizer and inhibitor to prepare de-crosslinked EVA waste; S4 fine crushing: Use a low-temperature crusher to crush the de-crosslinked EVA waste to a particle size of ≤1mm, controlling the crushing temperature to less than 40°C. S5 stirring and mixing: mixing the above powder, screened combustibles, agricultural and forestry wastes, combustion aids, and oxidants according to proportions; S6 hot pressing: The raw materials are extruded and formed using a twin-screw granulator to obtain the finished RDF / SRF derived fuel.
9. The method for preparing a derived fuel based on waste EVA according to claim 8, characterized in that: In step S2, the mass ratio of EVA fertilizer, solubilizer and inhibitor is 100:1-10:0.1-1.
10. The method for preparing a derived fuel based on waste EVA according to claim 9, characterized in that: In step S6, the extrusion molding process adopts a hot pressing molding process, with a temperature of 80-100° C. and a pressure of 15-30 MPa.