Method for shortening pure oxygen supply time of top-blown converter
By controlling the thermal balance and gun position flow in the top blowing converter, combining a large amount of cooling cold material and oxygen jet, the problem of excessively long pure oxygen supply time of the top blowing converter is solved, and efficient production and improvement of slag dephosphorization effect is achieved.
Patent Information
- Application Number
- CN202410964764.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-12
AI Technical Summary
The pure oxygen supply time of the top blowing converter is too long, which affects the efficient production of the converter. The kinetic conditions are poor under bottom blowing conditions, making it difficult to take into account the effects of slag dephosphorization and stirring.
通过控制转炉热平衡,加入大量降温冷料以提高炉渣氧化性,并采用低枪位操作模式和氧气射流以提高动力学条件,促进钢渣界面反应,控制炉气排除以减少喷溅。具体步骤包括开吹点火、加入降温冷料与造渣料、固定枪位与氧气流量吹炼、加入剩余冷料与造渣料和拉碳出钢。
The pure oxygen supply time of the top-blowing converter is effectively shortened by 2.14 minutes, and the blowing time is shortened by 15.62%, which improves the converter utilization rate, reduces energy consumption, and increases the slag dephosphorization rate.
Smart Images

Figure CN118932135A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of converter smelting, and in particular to a method for shortening the pure oxygen supply time of a top-blown converter. Background Art
[0002] Converter steelmaking uses molten iron, scrap steel and ferroalloy as the main raw materials. It does not rely on external energy sources, but relies on the physical heat of the molten iron itself and the heat generated by the chemical reaction between the components of the molten iron to complete the steelmaking process in the converter. According to the location where the gas is blown into the furnace, there are top blowing, bottom blowing and side blowing; according to the type of gas, there are air converters and oxygen converters. Basic oxygen top blowing and top and bottom combined blowing converters are the most commonly used steelmaking equipment due to their fast production speed, large output, high single furnace output, low cost and low investment. Converters are mainly used for the production of carbon steel, alloy steel and the smelting of copper and nickel.
[0003] The pure oxygen supply time of the converter is an important part of the converter smelting cycle. Its duration directly affects the efficient production of the converter, and has different degrees of impact on the converter utilization rate, power energy consumption, etc. Affected by slag dephosphorization, splashing control, etc., the top-blown converter has poor dynamic conditions under bottom-blowing conditions. If the oxygen lance position is lowered, the dynamic conditions can be improved but the slag-forming effect will be affected; if the oxygen lance position is increased, the slag oxidation will be increased to promote slag-forming, but the stirring effect is poor and it is easy to splash; for this reason, the lance position and oxygen flow rate are appropriately lowered to ensure slag-forming and dephosphorization. In this mode, the converter oxygen supply intensity is not high, and the oxygen supply flow rate is low, which affects the thermodynamic and kinetic conditions of the chemical reaction at the slag interface in the converter molten pool, resulting in a long pure oxygen supply time.
[0004] Therefore, a method for shortening the pure oxygen supply time of the converter was invented, which aims to lower the oxygen lance position as a whole and adopt a low lance position operation mode, while ensuring the kinetic and thermodynamic conditions, and solving the slag oxidation problem, shortening the oxygen supply time while meeting the requirements of dephosphorization and splashing control, so as to achieve the goal of efficient production. Summary of the invention
[0005] The object of the present invention is to provide a method for shortening the pure oxygen supply time of a top-blown converter. By controlling the thermal balance of the converter, a large amount of cooling cold material is added from the high-level silo of the converter to improve the oxidizability of the slag; a low-gun position operation mode is adopted, and an oxygen jet is used to increase the stirring of the molten pool to improve the dynamic conditions, promote the interface reaction of the steel slag, and at the same time facilitate the removal of furnace gas, and control the difficulty of discharging a large amount of furnace gas and accumulate to cause splashing.
[0006] The method for shortening the pure oxygen supply time of a top-blown converter of the present invention comprises the following steps:
[0007] S1 starts blowing and ignition;
[0008] S2 adds cooling material and slag-making material;
[0009] S3 fixed gun position and oxygen flow blowing;
[0010] S4 adds the remaining cooling material and slag-making material;
[0011] S5 carbon steel pulling.
[0012] The step S1 of the present invention is to start blowing and ignite, specifically: the converter iron consumption is controlled to be above 900kg / t to ensure the thermal balance of the converter, the oxygen lance position is set to a fixed value of 1.7-1.9m, and the oxygen flow rate is set to a fixed value of 21000-23000Nm 3 / h to start blowing and ignition.
[0013] Preferably, the oxygen gun position is fixed at 1.8m and the oxygen flow rate is fixed at 22000Nm 3 / h to start blowing and ignition.
[0014] The step S2 of the present invention is to add cooling cold material and slag-making material, specifically: after the converter is successfully started and ignited, 1 / 3 of the total amount of cooling cold material is added into the furnace from the converter high-level material bin according to the heat balance calculation result, and 1 / 2 of the total amount of slag-making material is added after oxygen is supplied for 28 to 30 seconds, and the slag-making material includes light-burned dolomite and active lime.
[0015] The step S3 of the present invention is to fix the gun position and oxygen flow rate for blowing, specifically: the oxygen gun position is lowered from the ignition gun position to 1.2-1.3m and maintained, and the oxygen flow rate is fixed to 21000-23000Nm 3 / h for blowing.
[0016] Preferably, the oxygen gun position is lowered from the ignition gun position to 1.2m and maintained, and the oxygen flow rate is fixed at 22000Nm 3 / h for blowing.
[0017] The step S4 of the present invention is to add the remaining cooling material and slag-making material, specifically: after slagging, add the remaining 2 / 3 cooling material and 1 / 2 slag-making material in small batches, and add all of them within 6 minutes.
[0018] Step S5 of the present invention is to carbon-pull steel, specifically: in the later stage of smelting, according to the carbon content and temperature of the molten steel, the gun position is lowered to the 1.1m carbon-pulling gun position, and TCO is used for endpoint detection. After reaching the endpoint control target of C ≥ 0.05% and temperature 1630 ~ 1670 ° C, the gun is raised to directly tap the steel.
[0019] The specific composition of the cooling material in step S2 and step S4 of the present invention is: cold solid ball TFe 55% to 65%, CaO 10% to 18%, P 0.1% to 0.3%, S 0.04% to 0.08%
[0020] The beneficial effects of the present invention are:
[0021] 1. Adopt the low-gun position operation mode throughout the whole process after the ignition is started. In the absence of bottom blowing of the converter, the stirring effect of the molten pool is improved, the contact area of the slag is increased, and the interface reaction of the slag is promoted;
[0022] 2. Use a large number of cold solid balls as cooling materials to directly improve the oxidizability of the slag, without the need to use high-position oxygen supply;
[0023] 3. Without large economic investment, by optimizing the slag oxidation control means and lowering the gun position to promote stirring, the slag dephosphorization effect is guaranteed, the molten pool reaction speed is promoted and splashing is controlled, effectively shortening the pure oxygen supply time by 2.14 minutes and the blowing time by 15.62%. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a schematic diagram of specific gun position and flow control in Example 1 of the present invention. DETAILED DESCRIPTION
[0025] The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention. These modifications or improvements made without departing from the spirit of the present invention all belong to the scope of protection claimed in the present invention.
[0026] Example 1
[0027] S1 blow and ignite: add 88.1 tons of molten iron and 13.9 tons of scrap steel into the converter, with a total loading of 102 tons. The iron consumption is calculated to be 945kg / t. The static heat balance calculation result of the converter is 2000kg, that is, 2000kg of cooling material is required for this furnace steel. Lower the oxygen lance to 1.8m and the oxygen flow rate to 22000Nm 3 / h to start blowing and ignition.
[0028] S2 adds cooling cold material and slag-making material: after successful ignition, add 1000kg of cold solid balls, supply oxygen for 28 seconds, and then add 800kg of light-burned dolomite and 1200kg of active lime.
[0029] S3 fixed gun position and oxygen flow blowing: then lower the gun position to 1.2m and set the oxygen flow to 22000Nm 3 / h continues until the smelting end point and the gun is lifted.
[0030] S4 adds the remaining cooling cold materials and slag-making materials: after slagging, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 4 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 5 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 6 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls.
[0031] S5 Carbon pulling and steel tapping: In the later stage of smelting, according to the carbon content and temperature of the molten steel, the gun position is lowered to 1.1m carbon pulling gun position, and TCO is used for endpoint detection. After reaching the endpoint control target of C ≥ 0.05% and temperature 1630 ~ 1670℃, the gun is raised and steel is tapped directly.
[0032] Example 2
[0033] S1 blow and ignite: add 88.1 tons of molten iron and 13.9 tons of scrap steel into the converter, with a total loading of 102 tons. The iron consumption is calculated to be 945kg / t. The static heat balance calculation result of the converter is 2000kg, that is, 2000kg of cooling material is required for this furnace steel. Lower the oxygen lance to 1.9m and the oxygen flow rate to 21000Nm 3 / h to start blowing and ignition.
[0034] S2 adds cooling cold materials and slag-making materials: after successful ignition, add 1000kg of cold solid balls, and after supplying oxygen for 30 seconds, add 800kg of light-burned dolomite and 1200kg of active lime.
[0035] S3 fixed gun position and oxygen flow blowing: then lower the gun position to 1.2m and set the oxygen flow to 21000Nm 3 / h continues until the smelting end point and the gun is lifted.
[0036] S4 adds the remaining cooling cold materials and slag-making materials: after slagging, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 4 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 5 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 6 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls.
[0037] S5 Carbon pulling and steel tapping: In the later stage of smelting, according to the carbon content and temperature of the molten steel, the gun position is lowered to 1.1m carbon pulling gun position, and TCO is used for endpoint detection. After reaching the endpoint control target of C ≥ 0.05% and temperature 1630 ~ 1670℃, the gun is raised and steel is tapped directly.
[0038] Example 3
[0039] S1 blow and ignite: add 88.1 tons of molten iron and 13.9 tons of scrap steel into the converter, with a total loading of 102 tons. The iron consumption is calculated to be 945kg / t. The static heat balance calculation result of the converter is 2000kg, that is, 2000kg of cooling material is required for this furnace steel. Lower the oxygen lance to 1.7m and the oxygen flow rate to 23000Nm 3 / h to start blowing and ignition.
[0040] S2 adds cooling cold material and slag-making material: after successful ignition, add 1000kg of cold solid balls, supply oxygen for 29 seconds, and then add 800kg of light-burned dolomite and 1200kg of active lime.
[0041] S3 fixed gun position and oxygen flow blowing: then lower the gun position to 1.2m and set the oxygen flow to 23000Nm 3 / h continues until the smelting end point and the gun is lifted.
[0042] S4 adds the remaining cooling cold materials and slag-making materials: after slagging, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 4 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 5 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 6 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls.
[0043] S5 Carbon pulling and steel tapping: In the later stage of smelting, according to the carbon content and temperature of the molten steel, the gun position is lowered to 1.1m carbon pulling gun position, and TCO is used for endpoint detection. After reaching the endpoint control target of C ≥ 0.05% and temperature 1630 ~ 1670℃, the gun is raised and steel is tapped directly.
[0044] Example 4
[0045] S1 blow and ignite: add 88.1 tons of molten iron and 13.9 tons of scrap steel into the converter, with a total loading of 102 tons. The iron consumption is calculated to be 945kg / t. The static heat balance calculation result of the converter is 2000kg, that is, 2000kg of cooling material is required for this furnace steel. Lower the oxygen lance to 1.8m and the oxygen flow rate to 21000Nm 3 / h to start blowing and ignition.
[0046] S2 adds cooling cold materials and slag-making materials: after successful ignition, add 1000kg of cold solid balls, and after supplying oxygen for 30 seconds, add 800kg of light-burned dolomite and 1200kg of active lime.
[0047] S3 fixed gun position and oxygen flow blowing: then lower the gun position to 1.2m and set the oxygen flow to 22000Nm 3 / h continues until the smelting end point and the gun is lifted.
[0048] S4 adds the remaining cooling cold materials and slag-making materials: after slagging, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 4 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 5 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 6 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls.
[0049] S5 Carbon pulling and steel tapping: In the later stage of smelting, according to the carbon content and temperature of the molten steel, the gun position is lowered to 1.1m carbon pulling gun position, and TCO is used for endpoint detection. After reaching the endpoint control target of C ≥ 0.05% and temperature 1630 ~ 1670℃, the gun is raised and steel is tapped directly.
[0050] Example 5
[0051] S1 blow and ignite: add 88.1 tons of molten iron and 13.9 tons of scrap steel into the converter, with a total loading of 102 tons. The iron consumption is calculated to be 945kg / t. The static heat balance calculation result of the converter is 2000kg, that is, 2000kg of cooling material is required for this furnace steel. Lower the oxygen lance to 1.8m and the oxygen flow rate to 23000Nm 3 / h to start blowing and ignition.
[0052] S2 adds cooling cold material and slag-making material: after successful ignition, add 1000kg of cold solid balls, supply oxygen for 29 seconds, and then add 800kg of light-burned dolomite and 1200kg of active lime.
[0053] S3 fixed gun position and oxygen flow blowing: then lower the gun position to 1.2m and set the oxygen flow to 22000Nm 3 / h continues until the smelting end point and the gun is lifted.
[0054] S4 adds the remaining cooling cold materials and slag-making materials: after slagging, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 4 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 5 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 6 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls.
[0055] S5 Carbon pulling and steel tapping: In the later stage of smelting, according to the carbon content and temperature of the molten steel, the gun position is lowered to 1.1m carbon pulling gun position, and TCO is used for endpoint detection. After reaching the endpoint control target of C ≥ 0.05% and temperature 1630 ~ 1670℃, the gun is raised and steel is tapped directly.
[0056] Example 6
[0057] S1 blow and ignite: add 88.1 tons of molten iron and 13.9 tons of scrap steel into the converter, with a total loading of 102 tons. The iron consumption is calculated to be 945kg / t. The static heat balance calculation result of the converter is 2000kg, that is, 2000kg of cooling material is required for this furnace steel. Lower the oxygen lance to 1.8m and the oxygen flow rate to 22000Nm 3 / h to start blowing and ignition.
[0058] S2 adds cooling cold material and slag-making material: after successful ignition, add 1000kg of cold solid balls, supply oxygen for 28 seconds, and then add 800kg of light-burned dolomite and 1200kg of active lime.
[0059] S3 fixed gun position and oxygen flow blowing: then lower the gun position to 1.3m and set the oxygen flow to 22000Nm 3 / h continues until the smelting end point and the gun is lifted.
[0060] S4 adds the remaining cooling cold materials and slag-making materials: after slagging, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 4 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 5 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 6 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls.
[0061] S5 Carbon pulling and steel tapping: In the later stage of smelting, according to the carbon content and temperature of the molten steel, the gun position is lowered to 1.1m carbon pulling gun position, and TCO is used for endpoint detection. After reaching the endpoint control target of C ≥ 0.05% and temperature 1630 ~ 1670℃, the gun is raised and steel is tapped directly.
[0062] Example 7
[0063] S1 blow and ignite: add 88.1 tons of molten iron and 13.9 tons of scrap steel into the converter, with a total loading of 102 tons. The iron consumption is calculated to be 945kg / t. The static heat balance calculation result of the converter is 2000kg, that is, 2000kg of cooling material is required for this furnace steel. Lower the oxygen lance to 1.8m and the oxygen flow rate to 22000Nm 3 / h to start blowing and ignition.
[0064] S2 adds cooling cold materials and slag-making materials: after successful ignition, add 1000kg of cold solid balls, and after supplying oxygen for 30 seconds, add 800kg of light-burned dolomite and 1200kg of active lime.
[0065] S3 fixed gun position and oxygen flow blowing: then lower the gun position to 1.2m and set the oxygen flow to 21000Nm 3 / h continues until the smelting end point and the gun is lifted.
[0066] S4 adds the remaining cooling cold materials and slag-making materials: after slagging, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 4 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 5 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 6 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls.
[0067] S5 Carbon pulling and steel tapping: In the later stage of smelting, according to the carbon content and temperature of the molten steel, the gun position is lowered to 1.1m carbon pulling gun position, and TCO is used for endpoint detection. After reaching the endpoint control target of C ≥ 0.05% and temperature 1630 ~ 1670℃, the gun is raised and steel is tapped directly.
[0068] Example 8
[0069] S1 blow and ignite: add 88.1 tons of molten iron and 13.9 tons of scrap steel into the converter, with a total loading of 102 tons. The iron consumption is calculated to be 945kg / t. The static heat balance calculation result of the converter is 2000kg, that is, 2000kg of cooling material is required for this furnace steel. Lower the oxygen lance to 1.8m and the oxygen flow rate to 22000Nm 3 / h to start blowing and ignition.
[0070] S2 adds cooling cold material and slag-making material: after successful ignition, add 1000kg of cold solid balls, supply oxygen for 29 seconds, and then add 800kg of light-burned dolomite and 1200kg of active lime.
[0071] S3 fixed gun position and oxygen flow blowing: then lower the gun position to 1.2m and set the oxygen flow to 23000Nm 3 / h continues until the smelting end point and the gun is lifted.
[0072] S4 adds the remaining cooling cold materials and slag-making materials: after slagging, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 4 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 5 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 6 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls.
[0073] S5 Carbon pulling and steel tapping: In the later stage of smelting, according to the carbon content and temperature of the molten steel, the gun position is lowered to 1.1m carbon pulling gun position, and TCO is used for endpoint detection. After reaching the endpoint control target of C ≥ 0.05% and temperature 1630 ~ 1670℃, the gun is raised and steel is tapped directly.
[0074] Example 9
[0075] S1 blow and ignite: add 88.1 tons of molten iron and 13.9 tons of scrap steel into the converter, with a total loading of 102 tons. The iron consumption is calculated to be 945kg / t. The static heat balance calculation result of the converter is 2000kg, that is, 2000kg of cooling material is required for this furnace steel. Lower the oxygen lance to 1.9m and the oxygen flow rate to 21000Nm 3 / h to start blowing and ignition.
[0076] S2 adds cooling cold material and slag-making material: after successful ignition, add 1000kg of cold solid balls, supply oxygen for 28 seconds, and then add 800kg of light-burned dolomite and 1200kg of active lime.
[0077] S3 fixed gun position and oxygen flow blowing: then lower the gun position to 1.2m and set the oxygen flow to 22000Nm 3 / h continues until the smelting end point and the gun is lifted.
[0078] S4 adds the remaining cooling cold materials and slag-making materials: after slagging, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 4 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 5 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 6 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls.
[0079] S5 Carbon pulling and steel tapping: In the later stage of smelting, according to the carbon content and temperature of the molten steel, the gun position is lowered to 1.1m carbon pulling gun position, and TCO is used for endpoint detection. After reaching the endpoint control target of C ≥ 0.05% and temperature 1630 ~ 1670℃, the gun is raised and steel is tapped directly.
[0080] Example 10
[0081] S1 blow and ignite: add 88.1 tons of molten iron and 13.9 tons of scrap steel into the converter, with a total loading of 102 tons. The iron consumption is calculated to be 945kg / t. The static heat balance calculation result of the converter is 2000kg, that is, 2000kg of cooling material is required for this furnace. Lower the oxygen lance to 1.9m and the oxygen flow rate to 23000Nm 3 / h to start blowing and ignition.
[0082] S2 adds cooling cold materials and slag-making materials: after successful ignition, add 1000kg of cold solid balls, and after supplying oxygen for 30 seconds, add 800kg of light-burned dolomite and 1200kg of active lime.
[0083] S3 fixed gun position and oxygen flow blowing: then lower the gun position to 1.2m and set the oxygen flow to 22000Nm 3 / h continues until the smelting end point and the gun is lifted.
[0084] S4 adds the remaining cooling cold materials and slag-making materials: after slagging, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 4 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 5 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 6 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls.
[0085] S5 Carbon pulling and steel tapping: In the later stage of smelting, according to the carbon content and temperature of the molten steel, the gun position is lowered to 1.1m carbon pulling gun position, and TCO is used for endpoint detection. After reaching the endpoint control target of C ≥ 0.05% and temperature 1630 ~ 1670℃, the gun is raised and steel is tapped directly.
[0086] Embodiment 11
[0087] S1 blow and ignite: add 88.1 tons of molten iron and 13.9 tons of scrap steel into the converter, with a total loading of 102 tons. The iron consumption is calculated to be 945kg / t. The static heat balance calculation result of the converter is 2000kg, that is, 2000kg of cooling material is required for this furnace steel. Lower the oxygen lance to 1.7m and the oxygen flow rate to 21000Nm 3 / h to start blowing and ignition.
[0088] S2 adds cooling cold material and slag-making material: after successful ignition, add 1000kg of cold solid balls, supply oxygen for 29 seconds, and then add 800kg of light-burned dolomite and 1200kg of active lime.
[0089] S3 fixed gun position and oxygen flow blowing: then lower the gun position to 1.2m and set the oxygen flow to 22000Nm 3 / h continues until the smelting end point and the gun is lifted.
[0090] S4 adds the remaining cooling cold materials and slag-making materials: after slagging, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 4 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 5 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 6 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls.
[0091] S5 Carbon pulling and steel tapping: In the later stage of smelting, according to the carbon content and temperature of the molten steel, the gun position is lowered to 1.1m carbon pulling gun position, and TCO is used for endpoint detection. After reaching the endpoint control target of C ≥ 0.05% and temperature 1630 ~ 1670℃, the gun is raised and steel is tapped directly.
[0092] Example 12
[0093] S1 blow and ignite: add 88.1 tons of molten iron and 13.9 tons of scrap steel into the converter, with a total loading of 102 tons. The iron consumption is calculated to be 945kg / t. The static heat balance calculation result of the converter is 2000kg, that is, 2000kg of cooling material is required for this furnace steel. Lower the oxygen lance to 1.7m and the oxygen flow rate to 23000Nm 3 / h to start blowing and ignition.
[0094] S2 adds cooling cold material and slag-making material: after successful ignition, add 1000kg of cold solid balls, supply oxygen for 28 seconds, and then add 800kg of light-burned dolomite and 1200kg of active lime.
[0095] S3 fixed gun position and oxygen flow blowing: then lower the gun position to 1.2m and set the oxygen flow to 22000Nm 3 / h continues until the smelting end point and the gun is lifted.
[0096] S4 adds the remaining cooling cold materials and slag-making materials: after slagging, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 4 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 5 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls; when the oxygen is supplied for 6 minutes, add slag-making materials such as 200kg light-burned dolomite, 300kg active lime, and 250kg cold-solidified balls.
[0097] S5 Carbon pulling and steel tapping: In the later stage of smelting, according to the carbon content and temperature of the molten steel, the gun position is lowered to 1.1m carbon pulling gun position, and TCO is used for endpoint detection. After reaching the endpoint control target of C ≥ 0.05% and temperature 1630 ~ 1670℃, the gun is raised and steel is tapped directly.
[0098] In order to verify the effectiveness of the present invention, the inventor conducted a verification test, and the excerpts are as follows:
[0099] Solution 1 New process - Cold solid ball as cooling material
[0100] 88.1 tons of molten iron and 13.9 tons of scrap steel were added to the converter, with a total loading of 102 tons. The iron consumption was calculated to be 945 kg / t. The static heat balance calculation result of the converter was 2000 kg, which means that 2000 kg of cold material was needed to cool the steel in this furnace. The oxygen lance was lowered to 1.8 m and the oxygen flow rate was 22000 Nm 3 / h for ignition. After successful ignition, add 1000kg of cold solid balls, supply oxygen for 28 seconds, add 800kg of lightly burned dolomite and 1200kg of active lime. Then lower the gun position to 1.2m and set the oxygen flow rate to 22000Nm 3 / h until the end of smelting. Slag is started when oxygen is supplied for 3.5 minutes. At this time, 200kg of light-burned dolomite, 300kg of active lime and 250kg of cold-solidified balls are added as slag-making materials. 200kg of light-burned dolomite, 300kg of active lime and 250kg of cold-solidified balls are added when oxygen is supplied for 4 minutes. 200kg of light-burned dolomite, 300kg of active lime and 250kg of cold-solidified balls are added when oxygen is supplied for 5 minutes. 200kg of light-burned dolomite, 300kg of active lime and 250kg of cold-solidified balls are added when oxygen is supplied for 6 minutes. When the oxygen supply reaches 11 minutes, the carbon content of the molten steel is observed to reach the time for carbon pulling. At this time, the oxygen lance position is lowered to 1.1m for carbon pulling. When the oxygen supply reaches 11.56 minutes, the carbon in the molten steel is observed to be around 0.09% and the molten steel temperature is around 1640℃. At this time, the lance is raised and TCO is used for endpoint detection. The result is that the molten steel temperature is 1642℃ and the carbon content of the molten steel is 0.11%. The control target is achieved, and the furnace is shaken directly to the back of the furnace to discharge steel.
[0101] Option 2: Traditional process - limestone as cooling material
[0102] 87.8 tons of molten iron and 14.0 tons of scrap steel were added to the converter, with a total loading of 101.8 tons. The iron consumption was calculated to be 942 kg / t, and the static heat balance calculation result of the converter was 1900 kg. The oxygen lance was lowered to 1.8 m and the oxygen flow rate was 22000 Nm 3 / h for ignition. After ignition, add 700kg limestone, 750kg light-burned dolomite and 1250kg active lime. Then lower the gun position to 1.7m and set the oxygen flow rate to 20000Nm 3 / h. When the oxygen supply reaches 4.1 minutes, slagging occurs. At this time, 250kg of lightly burned dolomite, 300kg of active lime, and 500kg of limestone are added as slagging materials. When the oxygen supply reaches 5 minutes, 200kg of lightly burned dolomite, 300kg of active lime, and 300kg of limestone are added as slagging materials. The gun position is lowered to 1.4m and the oxygen flow rate is set to 19000Nm 3 / h. Sputtering occurred after 6 minutes of oxygen supply. At this time, 150kg of light-burned dolomite, 250kg of active lime and 200kg of limestone were added as slag-making materials, the gun position was kept at 1.4m, and the oxygen flow rate was set to 18000Nm3 / h. The splashing was not well controlled until 7 minutes of oxygen supply. At this time, 100kg of light-burned dolomite, 200kg of active lime and 100kg of limestone were added as slag-making materials, and the splashing was controlled by slag pressing. The splashing was controlled after 8 minutes of oxygen supply, but the slag was dried out. The gun position was raised to 1.6m and the oxygen flow rate was adjusted to 20000Nm 3 / h, and continue to supply oxygen for 9 minutes. Then, from 12.3 minutes onwards, the gun position is gradually lowered to 1.3m, at which point the gun position is raised to 1.7m and the oxygen flow rate is adjusted to 22000Nm 3 / h, and then lower the gun position to 1.1m for carbon pulling after 20 seconds. When carbon pulling lasted for 13.7 minutes, the temperature of the molten steel was observed to be around 1640℃. The gun was raised and TCO was used for endpoint detection. The result was that the temperature of the molten steel was 1637℃ and the carbon content was 0.05%. The temperature reached the target, but the molten steel was seriously over-oxidized, so it was directly tapped to the back of the furnace.
[0103] Table 1 Comparison of blowing effects between the process of the present invention and the conventional process
[0104]
[0105] The comparison of the blowing effects of the two schemes is shown in Table 1. The oxygen supply time for scheme 1 is 11.56 minutes, the slag process is normal, and there is no splashing. The final molten steel was analyzed and the phosphorus content was 0.018%. The corresponding dephosphorization rate was calculated to be 86.2%, which meets the steel grade composition control requirements. The oxygen supply time for scheme 2 was 13.7 minutes, and slag drying and splashing occurred in the middle of smelting. The final molten steel was analyzed and the phosphorus content was 0.024%. The corresponding dephosphorization rate was calculated to be 81.5%, which meets the steel grade composition control requirements.
[0106] In summary, the present invention can avoid slag back-drying and splashing during smelting; effectively shorten the pure oxygen supply time by 2.14 minutes, with a time reduction of 15.62%; improve the utilization rate of the converter, reduce energy consumption, and achieve efficient production; the dephosphorization rate is increased by 4.7% compared with the conventional process, indicating that it also has a certain effect on improving the dephosphorization rate.
[0107] Although the present invention has been described in detail above by means of general description, specific implementation methods and experiments, it is obvious to those skilled in the art that some modifications or improvements can be made to the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.
Claims
1. A method for shortening the pure oxygen supply time of a top-blown converter, characterized in that: The steps include: S1 starts blowing and ignition; S2 adds cooling material and slag-making material; S3 fixed gun position and oxygen flow blowing; S4 adds the remaining cooling material and slag-making material; S5 carbon steel pulling.
2. The method for shortening the pure oxygen supply time of a top-blown converter according to claim 1, characterized in that: The step S1 starts blowing and igniting, specifically: the converter iron consumption is controlled to be above 900kg / t to ensure the thermal balance of the converter, the oxygen lance position is set to a fixed value of 1.7-1.9m, and the oxygen flow rate is set to a fixed value of 21000-23000Nm 3 / h to start blowing and ignition.
3. The method for shortening the pure oxygen supply time of a top-blown converter according to claim 1, characterized in that: The step S1 starts the ignition, specifically: the oxygen gun position is set to 1.8m, the oxygen flow rate is set to 22000Nm 3 / h to start blowing and ignition.
4. The method for shortening the pure oxygen supply time of a top-blown converter according to claim 1, characterized in that: The step S2 of adding cooling cold material and slag-making material is specifically as follows: after the converter is successfully opened and ignited, 1 / 3 of the total amount of cooling cold material is added into the furnace from the converter high-level material bin according to the heat balance calculation result, and 1 / 2 of the total amount of slag-making material is added after oxygen is supplied for 28 to 30 seconds.
5. The method for shortening the pure oxygen supply time of a top-blown converter according to claim 1, characterized in that: The step S3 fixes the gun position and oxygen flow rate for blowing, specifically: the oxygen gun position is lowered from the ignition gun position to 1.2-1.3m and maintained, and the oxygen flow rate is fixed to 21000-23000Nm 3 / h for blowing.
6. The method for shortening the pure oxygen supply time of a top-blown converter according to claim 1, characterized in that: The step S3 fixes the gun position and oxygen flow rate for blowing, specifically: the oxygen gun position is lowered from the ignition gun position to 1.2m and maintained, and the oxygen flow rate is fixed to 22000Nm 3 / h for blowing.
7. The method for shortening the pure oxygen supply time of a top-blown converter according to claim 1, characterized in that: The step S4 of adding the remaining cooling material and slag-making material is specifically as follows: after slagging, the remaining 2 / 3 cooling material and 1 / 2 slag-making material are added in small batches, and all are added within 6 minutes.
8. The method for shortening the pure oxygen supply time of a top-blown converter according to claim 1, characterized in that: The step S5 of carbon drawing and steel tapping is specifically as follows: in the later stage of smelting, according to the carbon content and temperature of the molten steel, the gun position is lowered to the 1.1m carbon drawing gun position, and TCO is used for endpoint detection. After reaching the endpoint control target of C ≥ 0.05% and temperature 1630 ~ 1670 ° C, the gun is raised to directly tap the steel.
9. The method for shortening the pure oxygen supply time of a top-blown converter according to claim 1, characterized in that: The cooling cold material is a cold solid ball, and its components are: TFe 55%-65%, CaO 10%-18%, P 0.1%-0.3%, S 0.04%-0.08%.