Method for improving superplasticity of Ti65 high-temperature titanium alloy plate
Through hot rolling and annealing processes, the superplastic properties of Ti65 high-temperature titanium alloy sheets are improved, the problem of poor forming characteristics is solved, and the hot processing and forming of complex geometric components is realized, which significantly improves the process efficiency and application value.
Patent Information
- Application Number
- CN202410983220.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-22
AI Technical Summary
Ti65 high-temperature titanium alloy has a narrow processing window and large deformation resistance, resulting in poor forming characteristics, which is difficult to meet the hot processing and forming needs of key components in complex geometric shapes in aircraft.
The Ti65 high-temperature titanium alloy sheet with excellent superplastic properties is prepared by using hot rolling and annealing processes, including cutting processing, muffle furnace heat treatment, solid solution treatment, aging treatment, surface polishing and antioxidant coating.
It significantly improves the superplasticity and thermal processing properties of Ti65 high-temperature titanium alloy, with tensile elongation reaching 600% to 700%, simplifies the process flow, is suitable for the thermal processing and forming of complex geometric components, and has good industrial application value.
Smart Images

Figure CN118932153A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of Ti65 high-temperature titanium alloy preparation technology, and specifically relates to a method for improving the superplasticity of a Ti65 high-temperature titanium alloy plate. Background Art
[0002] High-temperature titanium alloys have shown broad application prospects in the field of lightweight aerospace structures due to their excellent comprehensive mechanical properties, high specific strength, heat resistance and creep resistance. At present, high-temperature titanium alloys that are maturely applied in 600 ℃ environments have been systematically studied at home and abroad, but there are few reports on high-temperature titanium alloys with a long-term service temperature of 650 ℃. With the rapid development of new high-performance ultrasonic / hypersonic aircraft, the forming requirements for complex and high-performance key components in aircraft are getting higher and higher. However, due to the high degree of alloying, Ti65 high-temperature titanium alloy cannot get rid of the common shortcomings of titanium alloys, namely, narrow processing window and high deformation resistance, which indicates that the poor forming characteristics of Ti65 high-temperature titanium alloy will bring huge challenges to the manufacturing of complex geometric shapes of key components.
[0003] Chinese patent CN109750185B provides a method for preparing a 650°C high-temperature titanium alloy sheet for superplastic forming, which uses hot rolling to obtain a 650°C titanium alloy sheet with excellent superplastic properties. The preparation steps are as follows: (1) heating a 650°C titanium alloy ingot and then forging it to obtain a titanium alloy slab for rolling; (2) coating the obtained slab and heating it, and then rolling it on a rolling mill; (3) heating the plate blank and then rolling it for a second time; (4) subjecting the plate blank to a heat treatment above the β phase transformation point and then rapidly quenching it with water; (5) heating the plate blank and then hot rolling it for a third time; (6) heating the plate blank and then hot rolling it for a fourth time in reverse direction; (7) welding the obtained blank to obtain a coated roll-coated package; (8) heating the roll-coated package and then hot rolling it to obtain a semi-finished plate; (9) subjecting the semi-finished plate to creep correction, annealing, acid and alkali washing to obtain a 650°C titanium alloy sheet product with a thickness of 0.8 to 2.0 mm.
[0004] However, the above method can obtain a high-temperature titanium alloy sheet for superplastic forming by combining multiple hot rolling and annealing, which is complicated and not conducive to the hot working forming of key parts with complex geometric shapes in aircraft. Therefore, designing an excellent superplastic Ti65 high-temperature titanium alloy and improving the hot working performance of Ti65 high-temperature titanium alloy are the key issues that need to be solved at present to meet the requirements of manufacturing complex geometric shapes of key parts in aircraft. Summary of the invention
[0005] The object of the present invention is to provide a method for improving the superplasticity of Ti65 high temperature titanium alloy sheet, aiming to solve the above-mentioned problems.
[0006] The present invention is mainly achieved through the following technical solutions: A method for improving the superplasticity of a Ti65 high temperature titanium alloy sheet comprises the following steps: Step S1: cutting and processing to obtain a Ti65 high temperature titanium alloy plate; Step S2: heat treating the Ti65 high temperature titanium alloy plate in a muffle furnace, and then hot rolling it on a rolling mill; Step S3: subjecting the Ti65 high temperature titanium alloy plate to a solution treatment in a muffle furnace at a temperature of 1050°C for 120 min, and then water cooling; Step S4: subjecting the Ti65 high temperature titanium alloy plate to aging treatment in a muffle furnace at 520° C. to 720° C. for 60 min to 80 min, and then air cooling; Step S5: grinding the Ti65 high temperature titanium alloy plate on sandpaper to eliminate surface oxides, and evenly coating the Ti-1 antioxidant on the surface of the Ti65 high temperature titanium alloy plate to protect it from high temperature oxidation.
[0007] In order to better implement the present invention, further, in the step S1, a cast Ti65 high-temperature titanium alloy with a purity of 99.9% is prepared by vacuum induction levitation melting.
[0008] In order to better implement the present invention, further, in the step S1, the Ti65 high-temperature titanium alloy is subjected to slow-wire electrospark machining to obtain a Ti65 high-temperature titanium alloy plate with a thickness of 4.2 mm.
[0009] In order to better implement the present invention, further, in step S2, the Ti65 high-temperature titanium alloy plate is kept in a muffle furnace at a temperature of 1150° C. for 60 min.
[0010] In order to better implement the present invention, further, in step S2, the thickness is reduced by 0.05 mm in each rolling pass until the final thickness is 1.2 mm.
[0011] In order to better implement the present invention, further, in the step S4, the Ti65 high temperature titanium alloy plate is subjected to aging treatment in a muffle furnace at 600° C. for 70 min to 80 min.
[0012] In order to better implement the present invention, further, in step S5, the superplastic elongation of the treated Ti65 high-temperature titanium alloy plate at 950° C. is 600% to 700%.
[0013] The beneficial effects of the present invention are as follows: The present invention prepares the microstructure of Ti65 high-temperature titanium alloy by combining hot rolling and annealing. The present invention prepares Ti65 high-temperature titanium alloy sheet by simple rolling and heat treatment process, and the sheet exhibits excellent superplasticity, with a tensile elongation of up to 600% to 700%, which can meet the requirements of hot processing and forming of parts with complex geometric shapes, while having simple procedures and high efficiency. Compared with the existing process, the present invention significantly improves the superplasticity and hot processing properties of Ti65 high-temperature titanium alloy, making it exhibit excellent industrial application value, and can fully realize the hot processing and forming of parts with complex geometric shapes in aircraft, and has good practicality. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 It is the structural schematic diagram of the tensile specimen; Figure 2 This is the morphology of the tensile fracture of the sample after aging treatment at 550°C for 60 min in Example 1; Figure 3 This is the morphology of the tensile fracture of the sample after aging treatment at 600 °C for 60 min in Example 2; Figure 4 This is the morphology of the tensile fracture of the sample after aging treatment at 600 °C for 70 min in Example 3; Figure 5 This is the morphology of the tensile fracture of the sample after aging treatment at 600 °C for 80 min in Example 4; Figure 6 This is the morphology of the tensile fracture of the sample after aging treatment at 650°C for 60 min in Example 5; Figure 7 This is the morphology of the tensile fracture of the sample after aging treatment at 700 °C for 60 min in Example 6; Figure 8 This is the morphology of the tensile fracture of the untreated sample in Comparative Example 1; Fig. 9 This is the stress-strain curve of the sample after aging treatment at 600°C for 70 min in Example 3. DETAILED DESCRIPTION
[0015] Embodiment 1: A method for improving the superplasticity of a Ti65 high temperature titanium alloy sheet comprises the following steps: The cast Ti65 high-temperature titanium alloy was electrospark machined by slow wire cutting to obtain a plate-shaped sample with a thickness of 4.2 mm. The plate was placed in a muffle furnace at 1150 °C for 60 min and then hot rolled on a rolling mill. The thickness reduction of each rolling pass was 0.05 mm, and the final thickness of the rolled plate was 1.2 mm. Then, if Figure 1As shown in the figure, a tensile specimen is cut from the rolled plate, and the gauge section size of the tensile specimen is 42.5 mm × 12.5 mm. The tensile specimen is placed in a muffle furnace at a temperature of 1050 °C for solution treatment for 120 min and then water-cooled. Secondly, the tensile specimen after solution treatment is placed in a muffle furnace at 550 °C for aging treatment for 60 min and then air-cooled. The tensile specimens after aging treatment were polished on sandpaper to eliminate surface oxides, and Ti-1 antioxidant was evenly coated on the surface of the specimens to protect the tensile specimens from high-temperature oxidation. Finally, the tensile specimens were subjected to a high-temperature tensile test at 950 °C on a universal high-temperature tensile machine with a tensile strain rate of 1×10 -2 s -1 .
[0016] like Figure 2 As shown, the superplastic elongation of the Ti65 high-temperature titanium alloy plate prepared in this embodiment when stretched at 950°C is 341%.
[0017] Embodiment 2: A method for improving the superplasticity of a Ti65 high temperature titanium alloy sheet comprises the following steps: The cast Ti65 high-temperature titanium alloy was electrospark machined by slow wire cutting to obtain a plate-shaped sample with a thickness of 4.2 mm. The plate was placed in a muffle furnace at 1150 °C for 60 min and then hot rolled on a rolling mill. The thickness reduction of each rolling pass was 0.05 mm, and the final thickness of the rolled plate was 1.2 mm. Then, if Figure 1 As shown in the figure, a tensile specimen is cut from the rolled plate, and the gauge section size of the tensile specimen is 42.5 mm × 12.5 mm. The tensile specimen is placed in a muffle furnace at a temperature of 1050 °C for solution treatment for 120 min and then water-cooled. Secondly, the tensile specimen after solution treatment is placed in a muffle furnace at 600 °C for aging treatment for 60 min and then air-cooled. The tensile specimens after aging treatment were polished on sandpaper to eliminate surface oxides, and Ti-1 antioxidant was evenly coated on the surface of the specimens to protect the tensile specimens from high-temperature oxidation. Finally, the tensile specimens were subjected to a high-temperature tensile test at 950 °C on a universal high-temperature tensile machine with a tensile strain rate of 1×10 -2 s -1 .
[0018] like Figure 3 As shown, the superplastic elongation of the Ti65 high-temperature titanium alloy plate prepared in this embodiment when stretched at 950°C is 488%.
[0019] Embodiment 3: A method for improving the superplasticity of a Ti65 high temperature titanium alloy sheet comprises the following steps: The cast Ti65 high-temperature titanium alloy was electrospark machined by slow wire cutting to obtain a plate-shaped sample with a thickness of 4.2 mm. The plate was placed in a muffle furnace at 1150 °C for 60 min and then hot rolled on a rolling mill. The thickness reduction of each rolling pass was 0.05 mm, and the final thickness of the rolled plate was 1.2 mm. Then, if Figure 1 As shown in the figure, a tensile specimen is cut from the rolled plate, and the gauge section size of the tensile specimen is 42.5 mm × 12.5 mm. The tensile specimen is placed in a muffle furnace at 1050 °C for solution treatment for 120 min and then water-cooled. Secondly, the tensile specimen after solution treatment is placed in a muffle furnace at 600 °C for aging treatment for 70 min and then air-cooled. The tensile specimens after aging treatment were polished on sandpaper to eliminate surface oxides, and Ti-1 antioxidant was evenly coated on the surface of the specimens to protect the tensile specimens from high-temperature oxidation. Finally, the tensile specimens were subjected to a high-temperature tensile test at 950 °C on a universal high-temperature tensile machine with a tensile strain rate of 1×10 -2 s -1 .
[0020] like Figure 4 As shown, the superplastic elongation of the Ti65 high-temperature titanium alloy plate prepared in this embodiment when stretched at 950°C is 680%.
[0021] Embodiment 4: A method for improving the superplasticity of a Ti65 high temperature titanium alloy sheet comprises the following steps: The cast Ti65 high-temperature titanium alloy was electrospark machined by slow wire cutting to obtain a plate sample with a thickness of 4.2 mm. The plate was placed in a muffle furnace at a temperature of 1150 ℃ for 60 min and then hot rolled on a rolling mill. The thickness reduction of each rolling pass was 0.05 mm, and the final thickness of the rolled plate was 1.2 mm. Then, if Figure 1 As shown in the figure, a tensile specimen is cut from the rolled plate, and the gauge section size of the tensile specimen is 42.5 mm × 12.5 mm. The tensile specimen is placed in a muffle furnace at 1050 °C for solution treatment for 120 min and then water-cooled. Secondly, the tensile specimen after solution treatment is placed in a muffle furnace at 600 °C for aging treatment for 80 min and then air-cooled. The tensile specimens after aging treatment were polished on sandpaper to eliminate surface oxides, and Ti-1 antioxidant was evenly coated on the surface of the specimens to protect the tensile specimens from high-temperature oxidation. Finally, the tensile specimens were subjected to a high-temperature tensile test at 950 °C on a universal high-temperature tensile machine with a tensile strain rate of 1×10 -2 s -1 .
[0022] like Figure 5 As shown, the superplastic elongation of the Ti65 high-temperature titanium alloy plate prepared in this embodiment when stretched at 950°C is 600%.
[0023] Embodiment 5: A method for improving the superplasticity of a Ti65 high temperature titanium alloy sheet comprises the following steps: The cast Ti65 high-temperature titanium alloy was electrospark machined by slow wire cutting to obtain a plate-shaped sample with a thickness of 4.2 mm. The plate was placed in a muffle furnace at 1150°C for 60 min and then hot rolled on a rolling mill. The thickness reduction of each rolling pass was 0.05 mm, and the final thickness of the rolled plate was 1.2 mm. Then, if Figure 1 As shown in the figure, a tensile specimen is cut from the rolled plate, and the gauge section size of the tensile specimen is 42.5 mm × 12.5 mm. The tensile specimen is placed in a muffle furnace at a temperature of 1050 °C for solution treatment for 120 min and then water-cooled. Secondly, the tensile specimen after solution treatment is placed in a muffle furnace at 650 °C for aging treatment for 60 min and then air-cooled. The tensile specimens after aging treatment were polished on sandpaper to eliminate surface oxides, and Ti-1 antioxidant was evenly coated on the surface of the specimens to protect the tensile specimens from high-temperature oxidation. Finally, the tensile specimens were subjected to a high-temperature tensile test at 950 °C on a universal high-temperature tensile machine with a tensile strain rate of 1×10 -2 s -1 .
[0024] like Figure 6 As shown, the superplastic elongation of the Ti65 high-temperature titanium alloy plate prepared in this embodiment when stretched at 950°C is 585%.
[0025] Embodiment 6: A method for improving the superplasticity of a Ti65 high temperature titanium alloy sheet comprises the following steps: The cast Ti65 high-temperature titanium alloy was electrospark machined by slow wire cutting to obtain a plate-shaped sample with a thickness of 4.2 mm. The plate was placed in a muffle furnace at 1150 °C for 60 min and then hot rolled on a rolling mill. The thickness reduction of each rolling pass was 0.05 mm, and the final thickness of the rolled plate was 1.2 mm. Then, if Figure 1 As shown in the figure, a tensile specimen is cut from the rolled plate, and the gauge section size of the tensile specimen is 42.5 mm × 12.5 mm. The tensile specimen is placed in a muffle furnace at 1050 °C for solution treatment for 120 min and then water-cooled. Secondly, the tensile specimen after solution treatment is placed in a muffle furnace at 700 °C for aging treatment for 60 min and then air-cooled. The tensile specimens after aging treatment were polished on sandpaper to eliminate surface oxides, and Ti-1 antioxidant was evenly coated on the surface of the specimens to protect the tensile specimens from high-temperature oxidation. Finally, the tensile specimens were subjected to a high-temperature tensile test at 950 °C on a universal high-temperature tensile machine with a tensile strain rate of 1×10 -2 s -1 .
[0026] like Figure 7 As shown, the superplastic elongation of the Ti65 high-temperature titanium alloy plate prepared in this embodiment when stretched at 950°C is 594%.
[0027] Comparative Example 1: A method for improving the superplasticity of a Ti65 high temperature titanium alloy sheet comprises the following steps: The cast Ti65 high-temperature titanium alloy was electrospark machined by slow wire cutting to obtain a plate-shaped sample with a thickness of 1.2 mm. Then, if Figure 1 As shown, a tensile specimen is cut from a plate specimen, the gauge section size of the tensile specimen is 42.5 mm × 12.5 mm, and a Ti-1 antioxidant is evenly coated on the surface of the specimen to protect the tensile specimen from high temperature oxidation; Finally, the tensile specimens were subjected to a high-temperature tensile test at 950 °C on a universal high-temperature tensile machine with a tensile strain rate of 1×10 -2 s -1 .like Figure 8 As shown, this comparative example is an untreated Ti65 high temperature titanium alloy plate, and its superplastic elongation under tension at 950°C is 245%.
[0028] Table 1 As shown in Table 1, compared with the untreated comparative example 1, the high temperature tensile elongation of the Ti65 high temperature titanium alloy after hot rolling and annealing treatment is greatly improved, showing extremely excellent superplasticity. Fig. 9As shown in the figure, after aging treatment at 600 °C for 70 min, the superplastic elongation of the sample is as high as 680%, which is 435% higher than that of comparative example 1. The process is simple and efficient, which makes Ti65 high-temperature titanium alloy suitable for hot working of complex geometric parts in aircraft. It has important guiding significance for the processing of complex parts in my country's aerospace industry. At the same time, it broadens people's horizons on the research of superplastic materials and has good practicality.
[0029] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification or equivalent change made to the above embodiment based on the technical essence of the present invention shall fall within the protection scope of the present invention.
Claims
1. A method for improving the superplasticity of Ti65 high temperature titanium alloy sheet, characterized in that: The following steps are involved: Step S1: cutting and processing to obtain a Ti65 high temperature titanium alloy plate; Step S2: heat treating the Ti65 high temperature titanium alloy plate in a muffle furnace, and then hot rolling it on a rolling mill; Step S3: subjecting the Ti65 high temperature titanium alloy plate to a solution treatment in a muffle furnace at a temperature of 1050°C for 120 min, and then water cooling; Step S4: subjecting the Ti65 high temperature titanium alloy plate to aging treatment in a muffle furnace at 520° C. to 720° C. for 60 min to 80 min, and then air cooling; Step S5: grinding the Ti65 high temperature titanium alloy plate on sandpaper to eliminate surface oxides, and evenly coating the Ti-1 antioxidant on the surface of the Ti65 high temperature titanium alloy plate to protect it from high temperature oxidation.
2. A method for improving superplasticity of Ti65 high temperature titanium alloy sheet according to claim 1, characterized in that: In the step S1, a cast Ti65 high-temperature titanium alloy with a purity of 99.9% is prepared by vacuum induction levitation melting.
3. A method for improving superplasticity of Ti65 high temperature titanium alloy sheet according to claim 2, characterized in that: In the step S1, the Ti65 high-temperature titanium alloy is subjected to slow-wire electrospark machining to obtain a Ti65 high-temperature titanium alloy plate with a thickness of 4.2 mm.
4. The method for improving superplasticity of Ti65 high temperature titanium alloy sheet according to claim 1, characterized in that: In the step S2, the Ti65 high temperature titanium alloy plate is kept in a muffle furnace at a temperature of 1150° C. for 60 min.
5. A method for improving superplasticity of Ti65 high temperature titanium alloy sheet according to claim 4, characterized in that: In step S2, the thickness is reduced by 0.05 mm in each rolling pass until the final thickness is 1.2 mm.
6. A method for improving superplasticity of Ti65 high temperature titanium alloy sheet according to any one of claims 1 to 5, characterized in that: In the step S4, the Ti65 high temperature titanium alloy plate is subjected to aging treatment in a muffle furnace at 600° C. for 70 min to 80 min.
7. A method for improving superplasticity of Ti65 high temperature titanium alloy sheet according to claim 6, characterized in that: In the step S5, the superplastic elongation of the treated Ti65 high temperature titanium alloy plate at 950° C. is 600% to 700%.
Citation Information
Patent Citations
Preparation method of high-temperature titanium alloy bar
CN109234554A
Heat-resisting titanium alloy and preparation method thereof
CN109536776A
Preparation method of 650 DEG C high-temperature titanium alloy sheet for superplastic forming
CN109750185A
In-situ strengthening and rapid forming method for thin-walled titanium alloy tubular component
US20240002988A1