Critical quenching heat treatment method for 20CrMo steel pressure-bearing stator part

Through normalization, critical quenching and tempering treatment of 20CrMo steel pressure-bearing stator parts, the impact toughness and hardness control problems in the prior art are solved, and the impact toughness and corrosion resistance are improved under the premise of satisfying mechanical properties. Effect.

CN118932156APending Publication Date: 2024-11-12SHENYANG TURBO MASCH CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411275352.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is difficult to improve the impact toughness while ensuring the mechanical properties of 20CrMo steel pressurized stator parts, and control the hardness to meet the corrosion resistance requirements under specific operating conditions.

Method used

A heat treatment method including normalization treatment, critical quenching treatment and tempering treatment is adopted: normalization treatment is insulated at 880-920°C and air-cooled, critical quenching treatment is insulated at 780-820°C and water-cooled, and tempering treatment is insulated at 620-660 Insulated at °C and air-cooled, these steps allow the material to refine the structure and optimize the distribution of harmful impurities in the two phase areas of austenite and ferrite.

Benefits of technology

It improves the impact toughness of the 20CrMo steel pressure-bearing stator parts, and effectively controls its hardness within the range of HBW≤237, meeting the corrosion resistance requirements under specific operating conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932156A_ABST
    Figure CN118932156A_ABST
Patent Text Reader

Abstract

The invention provides a critical quenching heat treatment method for a 20CrMo steel pressure-bearing stator part, which is characterized by comprising the following steps: normalizing treatment: preserving heat of the 20CrMo steel pressure-bearing stator part at 880-920 DEG C, and then discharging and air-cooling to room temperature; carrying out critical quenching treatment, namely carrying out heat preservation on the 20CrMo steel pressure-bearing stator part at 780-820 DEG C, and then discharging the 20CrMo steel pressure-bearing stator part from the furnace and carrying out water cooling; and tempering treatment is conducted, specifically, the 20CrMo steel pressure-bearing stator part is subjected to heat preservation at the temperature of 620-660 DEG C and then discharged out of the furnace to be air-cooled to the room temperature. According to the critical quenching heat treatment method for the 20CrMo steel pressure-bearing stator part, the impact toughness of the 20CrMo steel pressure-bearing stator part can be improved under the condition that the mechanical property of the 20CrMo steel pressure-bearing stator part meets the design requirement, and the hardness range of the 20CrMo steel pressure-bearing stator part can be effectively controlled so that the 20CrMo steel pressure-bearing stator part can meet the corrosion-resistant use requirement under the working condition of some special corrosive media.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of material heat treatment, and in particular to a critical quenching heat treatment method for 20CrMo steel pressure-bearing stator parts. Background Art

[0002] The stator parts of centrifugal compressors, such as cylindrical casings, are mainly made of 20CrMo hypoeutectoid steel. According to the classical heat treatment concept, hypoeutectoid steel must be heated to above AC3 for complete austenitization, that is, complete quenching to ensure the excellent performance of the steel. However, while ensuring the strength of the material, as a pressure-bearing part, it also has a high demand for impact toughness. At the same time, for some special process media such as corrosive gases such as H2S, its hardness must be controlled to meet relevant corrosion resistance standards such as NACE MR 0175 or NACE MR 0103 standards. The requirement of HBW≤237 (HRC22) results in that although complete quenching can ensure that the mechanical properties such as the yield strength of the stator parts can meet the design requirements, the probability of its impact toughness failing is often relatively high. Moreover, under some special working conditions, the hardness of the stator parts cannot be effectively controlled within the standard requirements.

[0003] Therefore, for 20CrMo steel pressure-bearing stator components such as cylindrical casings, a heat treatment process method is urgently needed to improve the impact toughness of the material while meeting the mechanical properties required by the design, and at the same time better control the hardness of the material to make it meet the corrosion resistance requirements under specific working conditions. Summary of the invention

[0004] The object of the present invention is to provide a critical quenching heat treatment method for a 20CrMo steel pressure-bearing stator component, so that after critical quenching, the impact toughness of the 20CrMo steel pressure-bearing stator component can be improved while the mechanical properties meet the design requirements, and the hardness range can be effectively controlled so that it can meet the corrosion resistance requirements under certain special corrosive medium working conditions.

[0005] In order to solve the above technical problems, the present invention provides a critical quenching heat treatment method for 20CrMo steel pressure-bearing stator parts, comprising the following steps:

[0006] Normalizing treatment: keep the 20CrMo steel pressure-bearing stator parts at 880-920℃, then take them out of the furnace and air-cool them to room temperature;

[0007] Critical quenching treatment: keep the 20CrMo steel pressure-bearing stator parts at 780-820℃, then water-cool them after they are taken out of the furnace;

[0008] Tempering treatment: The 20CrMo steel pressure-bearing stator parts are kept at 620-660°C, then taken out of the furnace and air-cooled to room temperature.

[0009] Furthermore, during the normalizing treatment of the 20CrMo steel pressure-bearing stator component, the furnace is charged at ≤500°C, and heated to 630-680°C at a speed of ≤100°C / h and kept warm for 1-4h, and then heated to 880-920°C at a speed of ≤100°C / h, and the holding time t is 0.9×effective thickness mm / 30mm hour, and the holding time shall not be less than 2 hours, and then taken out of the furnace and air-cooled to room temperature.

[0010] Furthermore, during the critical quenching treatment of the 20CrMo steel pressure-bearing stator components, the furnace is charged at ≤500°C, and heated to 630-680°C at a speed of ≤100°C / h and kept warm for 1-4h, and then heated to 780-820°C at a speed of ≤100°C / h, and the holding time t is 0.9×effective thickness mm / 30mm hour, and the holding time is not less than 2 hours, and then taken out of the furnace and water-cooled.

[0011] Furthermore, during the tempering treatment of the 20CrMo steel pressure-bearing stator components, the furnace is charged at ≤350°C and heated to 620-660°C at a speed of ≤70°C / h. The holding time t is 0.9×effective thickness mm / 30mm hour, and the holding time is not less than 3 hours. The components are then taken out of the furnace and air-cooled to room temperature.

[0012] Furthermore, the 20CrMo steel pressure-bearing stator component is a centrifugally compressed barrel-type casing.

[0013] Furthermore, the effective thickness is the maximum inscribed circle diameter of the wall thickness of the cylindrical casing.

[0014] The invention provides a critical quenching heat treatment method for a 20CrMo steel pressure-bearing stator component. According to the heat treatment process of normalizing, critical quenching and tempering, the 20CrMo steel pressure-bearing stator component is normalized at a temperature of 880 to 920° C., critical quenched at a temperature of 780 to 820° C. and tempered at a temperature of 620 to 660° C., so that the impact toughness of the 20CrMo steel pressure-bearing stator component can be improved while meeting the mechanical properties required by the design, and the hardness range can be better controlled within HBW≤237, so that the component meets the requirements for corrosion resistance under specific working conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 A flow chart of a critical quenching heat treatment method for 20CrMo steel pressure-bearing stator components provided in an embodiment of the present invention;

[0016] Figure 2 A schematic diagram of a normalizing heat treatment process in a critical quenching heat treatment method for a 20CrMo steel pressure-bearing stator component provided in an embodiment of the present invention;

[0017] Figure 3 A schematic diagram of a critical quenching heat treatment process in a critical quenching heat treatment method for a 20CrMo steel pressure-bearing stator component provided in an embodiment of the present invention;

[0018] Figure 4 A schematic diagram of a tempering heat treatment process in a critical quenching heat treatment method for a 20CrMo steel pressure-bearing stator component provided in an embodiment of the present invention;

[0019] Figure 5 A schematic diagram of the effective thickness of a cylindrical casing in a critical quenching heat treatment method for a 20CrMo steel pressure-bearing stator component provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0020] See also Figure 1 The embodiment of the present invention provides a critical quenching heat treatment method for a 20CrMo steel pressure-bearing stator component, comprising the following steps:

[0021] Step 1) Normalizing treatment: The 20CrMo steel pressure-bearing stator parts are kept at 880-920°C and then taken out of the furnace and air-cooled to room temperature.

[0022] 20CrMo steel is a hypoeutectoid steel. During normalizing treatment, the heat treatment method provided by the present invention heats the 20CrMo steel pressure-bearing stator parts to 30-50°C above the austenite transformation end temperature Ac3, so that the part material structure completes the austenite transformation, eliminates the hot coarse-grained structure and Widmanstatten structure in the forging process, refines the grains, and prepares a matrix structure for the subsequent quenching process.

[0023] Specifically, see Figure 2 When normalizing the 20CrMo steel pressure-bearing stator parts, load the furnace at ≤500℃, heat to 630-680℃ at a speed of ≤100℃ / h, and keep warm for 1-4h, then heat to 880-920℃ at a speed of ≤100℃ / h, and the holding time t is 0.9×effective thickness mm / 30mm hour, and the holding time shall not be less than 2 hours, and then take out of the furnace and air cool to room temperature.

[0024] Step 2) critical quenching treatment: the 20CrMo steel pressure-bearing stator parts are kept at 780-820°C and then water-cooled after being taken out of the furnace.

[0025] Complete quenching is to heat the steel material to a temperature above Ac3 to avoid the presence of undissolved ferrite in the steel material. After keeping it warm for a period of time to completely austenitize it, it is quickly cooled to below the martensitic transformation end temperature Ms to obtain a martensitic structure and then tempered to obtain troostite to obtain good mechanical properties.

[0026] The critical quenching heat treatment method for 20CrMo steel pressure-bearing stator parts provided by the present invention adopts critical quenching to heat the 20CrMo steel pressure-bearing stator parts to above the austenite start transformation temperature Ac1 and below Ac3, that is, between Ac1 and Ac3. The austenite + ferrite dual-phase structure in the material can be retained, and after a period of heat preservation, it is quickly cooled to below the martensite transformation end temperature Ms to obtain a martensite + ferrite dual-phase structure, and a subsequent tempering treatment can obtain a troostite + ferrite structure. Compared with complete quenching, due to the incomplete transformation of the austenite of the material, relatively less martensite structure is obtained, so that the tensile strength and yield strength of the material will be slightly lower, but the presence of undissolved ferrite in the material can prevent the stress concentration of the material and hinder the crack propagation, which can greatly improve the impact toughness of the material.

[0027] Specifically, see Figure 3 When the critical quenching treatment of 20CrMo steel pressure-bearing stator parts is carried out, the furnace is loaded at ≤500℃, and heated to 630-680℃ at a speed of ≤100℃ / h and kept warm for 1-4h, and then heated to 780-820℃ at a speed of ≤100℃ / h. The holding time t is 0.9×effective thickness mm / 30mm hour, and the holding time is not less than 2 hours, and then it is taken out of the furnace and water-cooled.

[0028] The present invention adopts critical quenching to significantly refine the grain size of 20CrMo steel pressure-bearing stator parts, and the heating temperature is in the austenite and ferrite two-phase region. Since the heating temperature is lower than that of complete quenching, the initial austenite grains formed are relatively small. At the same time, the undissolved ferrite in the material is dispersed in the form of fine needles or particles, which also cuts the generated austenite grains, hinders the growth of austenite grains, and effectively refines the austenite grains of the material.

[0029] In addition, the critical quenching temperature of the present invention is below Ac3, so a part of fine undissolved ferrite is retained in the material. The presence of ferrite with low hardness and good plasticity can prevent stress concentration and hinder crack propagation, so the toughness of the material can be improved. Before the material breaks, the crack propagates in the plastic zone at its tip. In the duplex alloy, when the radius of the plastic zone is larger than the radius of the grain, the crack propagates along the softer phase. When the crack propagates to the undissolved ferrite in the tough phase, the propagation is blocked or forced to change to a direction with less resistance and less harm, such as delamination, thereby relaxing energy and improving toughness.

[0030] At the same time, the present invention adopts critical quenching heat treatment to improve the distribution of harmful impurity elements in the material. On the one hand, when the austenite and ferrite two-phase region is heated, the grains in the material are refined, the grain volume is reduced, the ratio of surface area to volume increases, the total grain boundary area is significantly increased, and the area of ​​the ferrite and austenite grain boundary is 10 to 50 times larger than the austenite grain boundary area in the conventional quenching organization. Since the total grain boundary area increases and the grain boundaries increase, the content of harmful impurity elements (P, Sn, Sb, S, etc.) per unit area is reduced, and the segregation of harmful impurity elements is effectively reduced. On the other hand, after the critical quenching heat treatment, the organization is austenite and ferrite, wherein the generated ferrite mainly plays a purification role, and since the solubility of the impurity elements in ferrite is much greater than the solubility in austenite, it plays an enrichment role on the impurity elements, effectively suppresses the segregation of harmful impurity elements on the austenite grain boundary, and improves toughness.

[0031] Therefore, the critical quenching heat treatment method for 20CrMo steel pressure-bearing stator components provided by the present invention adopts a critical quenching heat treatment method, which can effectively improve the impact toughness of 20CrMo steel pressure-bearing stator components and effectively control the hardness value HBW≤237 of 20CrMo steel pressure-bearing stator components, so that it meets the requirements for corrosion resistance under specific working conditions.

[0032] Step 3) Tempering treatment: The 20CrMo steel pressure-bearing stator parts are kept at 620-660° C. and then taken out of the furnace and air-cooled to room temperature.

[0033] During the tempering treatment, the 20CrMo steel pressure-bearing stator parts are heated to below Ac1, kept warm for a period of time and then cooled to room temperature. The martensite + ferrite structure is transformed into the troostite + ferrite structure through tempering treatment, so that the material has excellent tensile strength, yield strength and impact toughness.

[0034] Specifically, see Figure 4 When tempering 20CrMo steel pressure-bearing stator parts, the furnace is loaded at ≤350℃ and heated to 620-660℃ at a speed of ≤70℃ / h. The holding time t is 0.9×effective thickness mm / 30mm hour, and the holding time is not less than 3 hours. Then it is taken out of the furnace and air-cooled to room temperature.

[0035] As a specific implementation of the present invention, the 20CrMo steel pressure-bearing stator component is a centrifugally compressed barrel-type casing.

[0036] Of course, the critical quenching heat treatment method for 20CrMo steel pressure-bearing stator components provided by the present invention can be applied not only to pressure-bearing components such as 20CrMo steel cylindrical casings, but also to other components made of 20CrMo steel.

[0037] Among them, see Figure 5The effective thickness is the maximum inscribed circle diameter of the cylindrical casing wall thickness.

[0038] The critical quenching heat treatment method for the 20CrMo steel pressure-bearing stator component provided by the present invention is specifically described below by taking the 20CrMo steel pressure-bearing stator component being a cylindrical housing as an example.

[0039] Example 1

[0040] The performance heat treatment of the cylindrical casing is sequentially performed with normalizing treatment, critical quenching treatment and tempering treatment.

[0041] Among them, normalizing treatment: 20CrMo steel cylindrical casing is charged into the furnace at 300℃, heated to 630℃ at a heating rate of 90℃ / h and kept at this temperature for 1h, then heated to 920℃ at a heating rate of 90℃ / h and kept at this temperature for 2h, and then taken out of the furnace and air-cooled to room temperature.

[0042] Quenching treatment: 20CrMo steel cylindrical casing is loaded into the furnace at 300℃, heated to 630℃ at a heating rate of 90℃ / h and kept at that temperature for 1h, then heated to 820℃ at a heating rate of 90℃ / h and kept at that temperature for 2h, and then taken out of the furnace and water-cooled.

[0043] Tempering treatment: 20CrMo steel cylindrical casing is charged into the furnace at 200℃, heated to 630℃ at a heating rate of 60℃ / h, kept at this temperature for 3h, and then taken out of the furnace and air-cooled to room temperature.

[0044] After the above-mentioned heat treatment is performed on the cylindrical casing in this embodiment, the mechanical properties of the 20CrMo steel cylindrical casing are tested. The mechanical properties are shown in Table 1.

[0045] Table 1

[0046]

[0047] Example 2

[0048] The performance heat treatment of the cylindrical casing is sequentially performed with normalizing treatment, critical quenching treatment and tempering treatment.

[0049] Among them, normalizing treatment: 20CrMo steel cylindrical casing is charged into the furnace at 280℃, heated to 640℃ at a heating rate of 80℃ / h and kept warm for 1h, then heated to 900℃ at 80℃ / h and kept warm for 2h, and then taken out of the furnace and air-cooled to room temperature.

[0050] Quenching treatment: 20CrMo steel cylindrical casing is charged into the furnace at 280℃, heated to 640℃ at a heating rate of 80℃ / h and kept at that temperature for 1h, then heated to 800℃ at a heating rate of 80℃ / h and kept at that temperature for 2h, and then taken out of the furnace and water-cooled.

[0051] Tempering treatment: 20CrMo steel cylindrical casing is placed in a furnace at 180℃, heated to 640℃ at a heating rate of 50℃ / h, kept at this temperature for 3h, and then taken out of the furnace and air-cooled to room temperature.

[0052] After the above-mentioned heat treatment is performed on the cylindrical casing in this embodiment, the mechanical properties of the 20CrMo steel cylindrical casing are tested. The mechanical properties are shown in Table 2.

[0053] Table 2

[0054]

[0055] Example 3

[0056] The performance heat treatment of the cylindrical casing is sequentially performed with normalizing treatment, critical quenching treatment and tempering treatment.

[0057] Among them, normalizing treatment: 20CrMo steel cylindrical casing is charged into the furnace at 280℃, heated to 640℃ at a heating rate of 100℃ / h and kept warm for 1h, then heated to 880℃ at 100℃ / h and kept warm for 2h, and then taken out of the furnace and air-cooled to room temperature.

[0058] Quenching treatment: 20CrMo steel cylindrical casing is charged into the furnace at 280℃, heated to 640℃ at a heating rate of 100℃ / h and kept at that temperature for 1h, then heated to 780℃ at a heating rate of 100℃ / h and kept at that temperature for 2h, and then taken out of the furnace and water-cooled.

[0059] Tempering treatment: 20CrMo steel cylindrical casing is placed in a furnace at 180℃, heated to 640℃ at a heating rate of 50℃ / h, kept at this temperature for 3h, and then taken out of the furnace and air-cooled to room temperature.

[0060] After the above-mentioned heat treatment is performed on the cylindrical casing in this embodiment, the mechanical properties of the 20CrMo steel cylindrical casing are tested. The mechanical properties are shown in Table 3.

[0061] Table 3

[0062]

[0063] It is calculated that the austenite transformation end temperature Ac3 of 20CrMo steel is about 830°C, and the critical quenching temperatures of Examples 1-3 of the present invention are 820°C, 800°C, and 780°C, respectively. From the mechanical properties in Table 1-3 of Examples 1-3 of the present invention, it can be seen that the closer to the critical quenching temperature Ac3, the better the tensile and yield strengths are, and the better the impact toughness is. The impact toughness is inversely proportional to the tensile yield strength, that is, the higher the tensile yield strength, the worse the impact toughness. The critical quenching heat treatment method for 20CrMo steel pressure-bearing stator parts provided by the present invention, the 20CrMo steel cylindrical casing obtained after heat treatment not only has good tensile yield strength, but also can successfully improve the impact toughness of the material through the undissolved ferrite retained by the critical quenching, and can also achieve the purpose of controlling its hardness value ≤ HBW237 through the low hardness and good plasticity of the undissolved ferrite, thereby ensuring the corrosion resistance of the 20CrMo steel cylindrical casing under specific working conditions.

[0064] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A critical quenching heat treatment method for 20CrMo steel pressure-bearing stator parts, characterized in that: The steps include: Normalizing treatment: keep the 20CrMo steel pressure-bearing stator parts at 880-920℃, then take them out of the furnace and air-cool them to room temperature; Critical quenching treatment: keep the 20CrMo steel pressure-bearing stator parts at 780-820℃, then water-cool them after they are taken out of the furnace; Tempering treatment: The 20CrMo steel pressure-bearing stator parts are kept at 620-660°C, then taken out of the furnace and air-cooled to room temperature.

2. The critical quenching heat treatment method for 20CrMo steel of pressure-bearing stator parts according to claim 1 is characterized in that: During the normalizing treatment of the 20CrMo steel pressure-bearing stator parts, the furnace is charged at ≤500°C, and heated to 630-680°C at a speed of ≤100°C / h and kept warm for 1-4h, and then heated to 880-920°C at a speed of ≤100°C / h, and the holding time t is 0.9×effective thickness mm / 30mm hour, and the holding time shall not be less than 2 hours, and then the parts are taken out of the furnace and air-cooled to room temperature.

3. The critical quenching heat treatment method for 20CrMo steel of pressure-bearing stator parts according to claim 2 is characterized in that: During the critical quenching treatment of the 20CrMo steel pressure-bearing stator parts, the furnace is charged at ≤500°C, and heated to 630-680°C at a speed of ≤100°C / h and kept warm for 1-4h, and then heated to 780-820°C at a speed of ≤100°C / h, and the holding time t is 0.9×effective thickness mm / 30mm hour, and the holding time is not less than 2 hours, and then taken out of the furnace and water-cooled.

4. The critical quenching heat treatment method for 20CrMo steel of pressure-bearing stator parts according to claim 3 is characterized in that: During the tempering treatment of the 20CrMo steel pressure-bearing stator parts, the furnace is charged at ≤350°C and heated to 620-660°C at a speed of ≤70°C / h. The holding time t is 0.9×effective thickness mm / 30mm hour, and the holding time is not less than 3 hours. The parts are then taken out of the furnace and air-cooled to room temperature.

5. The critical quenching heat treatment method for 20CrMo steel of pressure-bearing stator parts according to claim 4 is characterized in that: The 20CrMo steel pressure-bearing stator component is a centrifugally compressed barrel-type casing.

6. The critical quenching heat treatment method for 20CrMo steel of pressure-bearing stator parts according to claim 5, characterized in that: The effective thickness is the maximum inscribed circle diameter of the wall thickness of the cylindrical casing.