Preparation method of grain refiner

Through the coordination of modified graphene and yttrium regulator and chitosan liquid, grain refining agents are prepared, which solves the problems of low conductivity and mechanical properties of the alloy cable core, improves the stability of acid and corrosion resistance, and improves the product overall performance and efficiency.

CN118932208APending Publication Date: 2024-11-12GUANGXI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410991435.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing alloy cable cores have poor electrical conductivity, low mechanical properties, and insufficient acid and corrosion resistance, which limits the efficiency of the product.

Method used

Modified graphene and yttrium regulator are combined with chitosan liquid, and grain refining agents are prepared by modification treatment and ultrasonic blending, which optimizes the conductivity and mechanical properties of the alloy and improves the stability of acid and corrosion resistance.

Benefits of technology

It significantly improves the conductivity and mechanical properties of the cable, coordinates and improves the performance of the product, enhances the stability of acid and corrosion resistance, and improves the efficiency of use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004958980210000111
    Figure BDA0004958980210000111
Patent Text Reader

Abstract

The invention discloses a preparation method of a grain refiner. The preparation method comprises the following steps: 1, preparing a chitosan solution with the mass fraction of 5-7%; 2, adding 1-3 parts by weight of a silane coupling agent and 2-4 parts by weight of sodium dodecyl benzene sulfonate into 6-9 parts by weight of a chitosan solution, and fully stirring to obtain a chitosan solution; and step 3, adding 4-7 parts by weight of modified graphene and 1-3 parts by weight of a yttrium regulator into 5-8 parts by weight of a chitosan solution, stirring and modifying, and after stirring is finished, washing with water and drying to obtain the grain refiner. According to the grain refiner for the cable, the modified graphene and the yttrium regulator are adopted for mutual coordination, then the chitosan liquid is matched for regulation and improvement, through mutual coordination and cooperation of the raw materials, joint synergism and cooperation in alloy, the mechanical property and the electrical conductivity of a product are optimized, the performance effect of the product is coordinated and improved, meanwhile, the acid corrosion resistance stability of the product is optimized, and the service life of the cable is prolonged. And the performance of the product is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of grain refinement, and in particular to a method for preparing a grain refiner. Background Art

[0002] Cable is a general term for optical cables, electrical cables and other items. Cables have many uses, mainly used for control installation, connecting equipment, transmitting electricity and other multiple functions. They are common and indispensable in daily life. The existing alloy cable cores use aluminum alloy products. In the processing of aluminum alloy, grain refiners are rarely used. The prepared alloy products have poor conductivity and low mechanical properties. It is difficult to achieve coordinated improvement of the conductivity and mechanical properties of the products. The acid corrosion resistance of the products is low, which limits the use efficiency of the products. Summary of the invention

[0003] In view of the defects of the prior art, the object of the present invention is to provide a method for preparing a grain refiner to solve the problems raised in the above background technology.

[0004] The present invention solves the technical problem by adopting the following technical solution:

[0005] The present invention provides a method for preparing a grain refiner, comprising the following steps:

[0006] Step 1: First prepare a chitosan solution with a mass fraction of 5-7%;

[0007] Step 2: Add 1-3 parts by weight of silane coupling agent and 2-4 parts by weight of sodium dodecylbenzene sulfonate to 6-9 parts by weight of chitosan solution and stir well to obtain chitosan solution;

[0008] Step 3: Add 4-7 parts by weight of modified graphene and 1-3 parts by weight of yttrium regulator into 5-8 parts by weight of chitosan solution and stir for modification. After stirring, wash with water and dry to obtain a grain refiner.

[0009] Preferably, the silane coupling agent is silane coupling agent KH560.

[0010] Preferably, the stirring temperature of the stirring modification treatment in step 3 is 48-52° C., the stirring time is 20-30 min, and the stirring speed is 550-750 r / min.

[0011] Preferably, the modification method of the modified graphene is:

[0012] S01: The graphene is first heated to 150°C at a rate of 1-3°C / min, kept at this temperature for 5-10min, then heated to 310°C at a rate of 2-4°C / min, and finally air-cooled to room temperature;

[0013] S02: immersing the nano-silicon dioxide into a lanthanum chloride solution which is 3-5 times the total amount of the nano-silicon dioxide, then filtering and drying, and ultrasonically treating 3-5 parts by weight of the dried nano-silicon dioxide, 1-2 parts by weight of stearic acid, and 4-7 parts by weight of a sodium silicate solution, and then finishing the ultrasonic treatment to obtain a modified solution;

[0014] S03: The graphene product of S01 and the modified liquid are stirred at a weight ratio of 2:5. After stirring, the mixture is washed with water and dried to obtain modified graphene.

[0015] Preferably, the mass fraction of the lanthanum chloride solution is 3-6%; the mass fraction of the sodium silicate solution is 10-15%.

[0016] Preferably, the ultrasonic power of the S02 blending ultrasonic treatment is 350-400W, and the ultrasonic time is 20-30min; the stirring speed of the S03 stirring treatment is 450-500r / min, and the stirring time is 35-45min.

[0017] Preferably, the preparation method of the yttrium regulator is:

[0018] S101: yttrium oxide is first irradiated in a proton irradiation box for 5-10 minutes, with an irradiation power of 350-400W. After the irradiation is completed, irradiated yttrium oxide is obtained;

[0019] S102: The irradiated yttrium oxide is first subjected to a thermal reaction at a temperature of 210-230°C for 10-15 minutes, and then cooled to 55°C at a rate of 2-4°C / min and subjected to heat preservation treatment;

[0020] S103: 1-2 parts by weight of heat-insulated yttrium oxide, 1-3 parts by weight of sodium alginate solution, 1-2 parts by weight of nano-silica sol and 2-5 parts by weight of sodium lignin sulfonate solution are mixed and ball-milled. After the ball-milling is completed, the mixture is washed with water and dried to obtain a yttrium regulator.

[0021] Preferably, the mass fraction of the sodium alginate solution is 8-12%; the mass fraction of the sodium lignin sulfonate solution is 10-15%.

[0022] Preferably, the ball milling speed of the blended ball milling treatment is 1000-1500 r / min, and the ball milling is for 2 hours.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The grain refiner of the cable of the present invention adopts modified graphene and yttrium regulator to coordinate with each other, and then cooperates with chitosan liquid for adjustment and improvement. Through the mutual coordination and coordination between the raw materials, the synergy is enhanced together, and the alloy is combined to optimize the mechanical properties and conductivity of the product, coordinate and improve the performance effect of the product, and at the same time optimize the acid corrosion resistance stability of the product, so that the performance of the product is further improved. DETAILED DESCRIPTION

[0025] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] A method for preparing a grain refiner in this embodiment includes the following steps:

[0027] Step 1: First prepare a chitosan solution with a mass fraction of 5-7%;

[0028] Step 2: Add 1-3 parts by weight of silane coupling agent and 2-4 parts by weight of sodium dodecylbenzene sulfonate to 6-9 parts by weight of chitosan solution and stir well to obtain chitosan solution;

[0029] Step 3: Add 4-7 parts by weight of modified graphene and 1-3 parts by weight of yttrium regulator into 5-8 parts by weight of chitosan solution and stir for modification. After stirring, wash with water and dry to obtain a grain refiner.

[0030] The silane coupling agent of this embodiment is silane coupling agent KH560.

[0031] In step 3 of this embodiment, the stirring temperature of the stirring modification treatment is 48-52° C., the stirring time is 20-30 min, and the stirring speed is 550-750 r / min.

[0032] The modification method of the modified graphene of this embodiment is:

[0033] S01: The graphene is first heated to 150°C at a rate of 1-3°C / min, kept at this temperature for 5-10min, then heated to 310°C at a rate of 2-4°C / min, and finally air-cooled to room temperature;

[0034] S02: immersing the nano-silicon dioxide into a lanthanum chloride solution which is 3-5 times the total amount of the nano-silicon dioxide, then filtering and drying, and ultrasonically treating 3-5 parts by weight of the dried nano-silicon dioxide, 1-2 parts by weight of stearic acid, and 4-7 parts by weight of a sodium silicate solution, and then finishing the ultrasonic treatment to obtain a modified solution;

[0035] S03: The graphene product of S01 and the modified liquid are stirred at a weight ratio of 2:5. After stirring, the mixture is washed with water and dried to obtain modified graphene.

[0036] The mass fraction of the lanthanum chloride solution in this embodiment is 3-6%; the mass fraction of the sodium silicate solution is 10-15%.

[0037] In the present embodiment, the ultrasonic power of the S02 blending ultrasonic treatment is 350-400 W, and the ultrasonic time is 20-30 min; the stirring speed of the S03 stirring treatment is 450-500 r / min, and the stirring time is 35-45 min.

[0038] The preparation method of the yttrium regulator of this embodiment is:

[0039] S101: yttrium oxide is first irradiated in a proton irradiation box for 5-10 minutes, with an irradiation power of 350-400W. After the irradiation is completed, irradiated yttrium oxide is obtained;

[0040] S102: The irradiated yttrium oxide is first subjected to a thermal reaction at a temperature of 210-230°C for 10-15 minutes, and then cooled to 55°C at a rate of 2-4°C / min and subjected to heat preservation treatment;

[0041] S103: 1-2 parts by weight of heat-insulated yttrium oxide, 1-3 parts by weight of sodium alginate solution, 1-2 parts by weight of nano-silica sol and 2-5 parts by weight of sodium lignin sulfonate solution are mixed and ball-milled. After the ball-milling is completed, the mixture is washed with water and dried to obtain a yttrium regulator.

[0042] The mass fraction of the sodium alginate solution in this embodiment is 8-12%; the mass fraction of the sodium lignin sulfonate solution is 10-15%.

[0043] The ball milling speed of the blended ball milling treatment in this embodiment is 1000-1500 r / min, and the ball milling is 2 h.

[0044] Example 1.

[0045] A method for preparing a grain refiner in this embodiment includes the following steps:

[0046] Step 1: First prepare a chitosan solution with a mass fraction of 5%;

[0047] Step 2: Add 1 part by weight of silane coupling agent and 2 parts by weight of sodium dodecylbenzene sulfonate to 6 parts by weight of chitosan solution and stir well to obtain chitosan solution;

[0048] Step 3: Add 4 parts by weight of modified graphene and 1 part by weight of yttrium regulator into 5 parts by weight of chitosan solution and stir for modification. After stirring, wash with water and dry to obtain a grain refiner.

[0049] The silane coupling agent of this embodiment is silane coupling agent KH560.

[0050] In step 3 of this embodiment, the stirring temperature of the stirring modification treatment is 48° C., the stirring time is 20 min, and the stirring speed is 550 r / min.

[0051] The modification method of the modified graphene of this embodiment is:

[0052] S01: The graphene was first heated to 150°C at a rate of 1°C / min, kept at this temperature for 5 min, then heated to 310°C at a rate of 2°C / min, and finally air-cooled to room temperature;

[0053] S02: immersing the nano-silicon dioxide into a lanthanum chloride solution which is 3 times the total amount of the nano-silicon dioxide, then filtering and drying, blending 3 parts by weight of the dried nano-silicon dioxide, 1 part by weight of stearic acid, and 4 parts by weight of sodium silicate solution and ultrasonically treating them, and then ending the ultrasonic treatment to obtain a modified solution;

[0054] S03: The graphene product of S01 and the modified liquid are stirred at a weight ratio of 2:5. After stirring, the mixture is washed with water and dried to obtain modified graphene.

[0055] The mass fraction of the lanthanum chloride solution in this embodiment is 3%; the mass fraction of the sodium silicate solution is 10%.

[0056] The ultrasonic power of the S02 blending ultrasonic treatment in this embodiment is 350W, and the ultrasonic time is 20min; the stirring speed of the S03 stirring treatment is 450r / min, and the stirring time is 35min.

[0057] The preparation method of the yttrium regulator of this embodiment is:

[0058] S101: yttrium oxide is first irradiated in a proton irradiation box for 5 minutes, with an irradiation power of 350W. After the irradiation is completed, irradiated yttrium oxide is obtained;

[0059] S102: The irradiated yttrium oxide is first subjected to a thermal reaction at a temperature of 210°C for 10 minutes, and then cooled to 55°C at a rate of 2°C / min for heat preservation;

[0060] S103: 1 part by weight of heat-insulated yttrium oxide, 1 part by weight of sodium alginate solution, 1 part by weight of nano-silica sol and 2 parts by weight of sodium lignin sulfonate solution are mixed and ball-milled. After the ball-milling is completed, the mixture is washed with water and dried to obtain a yttrium regulator.

[0061] The mass fraction of the sodium alginate solution in this embodiment is 8%; the mass fraction of the sodium lignin sulfonate solution is 10%.

[0062] The ball milling speed of the blended ball milling treatment in this embodiment is 1000 r / min, and the ball milling is 2 h.

[0063] Example 2.

[0064] A method for preparing a grain refiner in this embodiment includes the following steps:

[0065] Step 1: First prepare a chitosan solution with a mass fraction of 7%;

[0066] Step 2: Add 3 parts by weight of silane coupling agent and 4 parts by weight of sodium dodecylbenzene sulfonate to 9 parts by weight of chitosan solution and stir well to obtain chitosan solution;

[0067] Step 3: Add 7 parts by weight of modified graphene and 3 parts by weight of yttrium regulator into 8 parts by weight of chitosan solution and stir for modification. After stirring, wash with water and dry to obtain a grain refiner.

[0068] The silane coupling agent of this embodiment is silane coupling agent KH560.

[0069] In step 3 of this embodiment, the stirring temperature for the stirring modification treatment is 52° C., the stirring time is 30 min, and the stirring speed is 750 r / min.

[0070] The modification method of the modified graphene of this embodiment is:

[0071] S01: The graphene was first heated to 150°C at a rate of 3°C / min, kept at this temperature for 10 min, then heated to 310°C at a rate of 4°C / min, and finally air-cooled to room temperature;

[0072] S02: immersing the nano-silicon dioxide into a lanthanum chloride solution of 5 times the total amount of the nano-silicon dioxide, then filtering and drying, blending 5 parts by weight of the dried nano-silicon dioxide, 2 parts by weight of stearic acid, and 7 parts by weight of sodium silicate solution and ultrasonically treating them, and then ending the ultrasonic treatment to obtain a modified solution;

[0073] S03: The graphene product of S01 and the modified liquid are stirred at a weight ratio of 2:5. After stirring, the mixture is washed with water and dried to obtain modified graphene.

[0074] The mass fraction of the lanthanum chloride solution in this embodiment is 6%; the mass fraction of the sodium silicate solution is 15%.

[0075] In this embodiment, the ultrasonic power of the S02 blending ultrasonic treatment is 400 W, and the ultrasonic time is 30 min; the stirring speed of the S03 stirring treatment is 500 r / min, and the stirring time is 45 min.

[0076] The preparation method of the yttrium regulator of this embodiment is:

[0077] S101: the yttrium oxide is first irradiated in a proton irradiation box for 10 minutes, the irradiation power is 400W, and the irradiation is completed to obtain irradiated yttrium oxide;

[0078] S102: The irradiated yttrium oxide is first subjected to a thermal reaction at a temperature of 230°C for 15 minutes, and then cooled to 55°C at a rate of 4°C / min for heat preservation;

[0079] S103: 2 parts by weight of heat-insulated yttrium oxide, 3 parts by weight of sodium alginate solution, 2 parts by weight of nano-silica sol and 5 parts by weight of sodium lignin sulfonate solution are mixed and ball-milled. After the ball-milling is completed, the mixture is washed with water and dried to obtain a yttrium regulator.

[0080] The mass fraction of the sodium alginate solution in this embodiment is 12%; the mass fraction of the sodium lignin sulfonate solution is 15%.

[0081] The ball milling speed of the blended ball milling treatment in this embodiment is 1500 r / min, and the ball milling is 2 h.

[0082] Example 3.

[0083] A method for preparing a grain refiner in this embodiment includes the following steps:

[0084] Step 1: First prepare a chitosan solution with a mass fraction of 6%;

[0085] Step 2: Add 2 parts by weight of silane coupling agent and 3 parts by weight of sodium dodecylbenzene sulfonate to 7.5 parts by weight of chitosan solution and stir well to obtain chitosan solution;

[0086] Step 3: Add 5.5 parts by weight of modified graphene and 2 parts by weight of yttrium regulator into 6.5 parts by weight of chitosan solution and stir for modification. After stirring, wash with water and dry to obtain a grain refiner.

[0087] The silane coupling agent of this embodiment is silane coupling agent KH560.

[0088] In step 3 of this embodiment, the stirring temperature of the stirring modification treatment is 50° C., the stirring time is 25 min, and the stirring speed is 600 r / min.

[0089] The modification method of the modified graphene of this embodiment is:

[0090] S01: The graphene was first heated to 150°C at a rate of 2°C / min, kept at this temperature for 7.5min, then heated to 310°C at a rate of 3°C / min, and finally air-cooled to room temperature;

[0091] S02: immersing the nano-silicon dioxide into a lanthanum chloride solution of 4 times the total amount of the nano-silicon dioxide, then filtering and drying, blending 4 parts by weight of the dried nano-silicon dioxide, 1.5 parts by weight of stearic acid, and 5.5 parts by weight of sodium silicate solution and ultrasonically treating the mixture, and then ending the ultrasonic treatment to obtain a modified solution;

[0092] S03: The graphene product of S01 and the modified liquid are stirred at a weight ratio of 2:5. After stirring, the mixture is washed with water and dried to obtain modified graphene.

[0093] The mass fraction of the lanthanum chloride solution in this embodiment is 4.5%; the mass fraction of the sodium silicate solution is 12.5%.

[0094] The ultrasonic power of the S02 blending ultrasonic treatment in this embodiment is 370W, and the ultrasonic time is 25min; the stirring speed of the S03 stirring treatment is 470r / min, and the stirring time is 40min.

[0095] The preparation method of the yttrium regulator of this embodiment is:

[0096] S101: yttrium oxide is first irradiated in a proton irradiation box for 7.5 minutes, with an irradiation power of 370W. After the irradiation is completed, irradiated yttrium oxide is obtained;

[0097] S102: The irradiated yttrium oxide is first subjected to a thermal reaction at a temperature of 220°C for 12 minutes, and then cooled to 55°C at a rate of 3°C / min for heat preservation;

[0098] S103: 1.5 minutes of heat-insulated yttrium oxide, 2 parts by weight of sodium alginate solution, 1.5 parts by weight of nano-silica sol and 3.5 parts by weight of sodium lignin sulfonate solution are mixed and ball-milled. After the ball-milling is completed, the mixture is washed with water and dried to obtain a yttrium regulator.

[0099] The mass fraction of the sodium alginate solution in this embodiment is 10%; the mass fraction of the sodium lignin sulfonate solution is 12.5%.

[0100] The ball milling speed of the blended ball milling treatment in this embodiment is 1250 r / min, and the ball milling is performed for 2 hours.

[0101] Example 4.

[0102] A method for preparing a grain refiner in this embodiment includes the following steps:

[0103] Step 1: First prepare a chitosan solution with a mass fraction of 6%;

[0104] Step 2: Add 2 parts by weight of silane coupling agent and 3 parts by weight of sodium dodecylbenzene sulfonate to 7 parts by weight of chitosan solution and stir well to obtain chitosan solution;

[0105] Step 3: Add 5 parts by weight of modified graphene and 2 parts by weight of yttrium regulator into 6 parts by weight of chitosan solution and stir for modification. After stirring, wash with water and dry to obtain a grain refiner.

[0106] The silane coupling agent of this embodiment is silane coupling agent KH560.

[0107] In step 3 of this embodiment, the stirring temperature of the stirring modification treatment is 49° C., the stirring time is 22 min, and the stirring speed is 580 r / min.

[0108] The modification method of the modified graphene of this embodiment is:

[0109] S01: The graphene was first heated to 150°C at a rate of 2°C / min, kept at this temperature for 6 min, then heated to 310°C at a rate of 3°C / min, and finally air-cooled to room temperature;

[0110] S02: immersing the nano-silicon dioxide into a lanthanum chloride solution which is 3-5 times the total amount of the nano-silicon dioxide, then filtering and drying, and ultrasonically treating 4 parts by weight of the dried nano-silicon dioxide, 1.2 parts by weight of stearic acid, and 5 parts by weight of a sodium silicate solution, and then finishing the ultrasonic treatment to obtain a modified solution;

[0111] S03: The graphene product of S01 and the modified liquid are stirred at a weight ratio of 2:5. After stirring, the mixture is washed with water and dried to obtain modified graphene.

[0112] The mass fraction of the lanthanum chloride solution in this embodiment is 4%; the mass fraction of the sodium silicate solution is 12%.

[0113] The ultrasonic power of the S02 blending ultrasonic treatment in this embodiment is 370W, and the ultrasonic time is 22min; the stirring speed of the S03 stirring treatment is 460r / min, and the stirring time is 38min.

[0114] The preparation method of the yttrium regulator of this embodiment is:

[0115] S101: yttrium oxide is first irradiated in a proton irradiation box for 6 minutes at an irradiation power of 360W. After the irradiation is completed, irradiated yttrium oxide is obtained;

[0116] S102: The irradiated yttrium oxide is first subjected to a thermal reaction at a temperature of 220°C for 12 minutes, and then cooled to 55°C at a rate of 3°C / min for heat preservation;

[0117] S103: 1 part by weight of heat-insulated yttrium oxide, 2 parts by weight of sodium alginate solution, 1.5 parts by weight of nano-silica sol and 3.5 parts by weight of sodium lignin sulfonate solution are mixed and ball-milled. After the ball-milling is completed, the mixture is washed with water and dried to obtain a yttrium regulator.

[0118] The mass fraction of the sodium alginate solution in this embodiment is 10%; the mass fraction of the sodium lignin sulfonate solution is 12.5%.

[0119] The ball milling speed of the blended ball milling treatment in this embodiment is 1250 r / min, and the ball milling is performed for 2 hours.

[0120] Example 5.

[0121] A method for preparing a grain refiner in this embodiment includes the following steps:

[0122] Step 1: First prepare a chitosan solution with a mass fraction of 6%;

[0123] Step 2: Add 2 parts by weight of silane coupling agent and 3 parts by weight of sodium dodecylbenzene sulfonate to 8 parts by weight of chitosan solution and stir well to obtain chitosan solution;

[0124] Step 3: Add 6 parts by weight of modified graphene and 2 parts by weight of yttrium regulator into 7 parts by weight of chitosan solution and stir for modification. After stirring, wash with water and dry to obtain a grain refiner.

[0125] The silane coupling agent of this embodiment is silane coupling agent KH560.

[0126] In step 3 of this embodiment, the stirring temperature for the stirring modification treatment is 51° C., the stirring time is 28 min, and the stirring speed is 730 r / min.

[0127] The modification method of the modified graphene of this embodiment is:

[0128] S01: The graphene was first heated to 150°C at a rate of 2°C / min, kept at this temperature for 9 minutes, then heated to 310°C at a rate of 3°C / min, and finally air-cooled to room temperature;

[0129] S02: immersing the nano-silicon dioxide into a lanthanum chloride solution of 4 times the total amount of the nano-silicon dioxide, then filtering and drying, blending 4 parts by weight of the dried nano-silicon dioxide, 2 parts by weight of stearic acid, and 6 parts by weight of sodium silicate solution and ultrasonically treating them, and then ending the ultrasonic treatment to obtain a modified solution;

[0130] S03: The graphene product of S01 and the modified liquid are stirred at a weight ratio of 2:5. After stirring, the mixture is washed with water and dried to obtain modified graphene.

[0131] The mass fraction of the lanthanum chloride solution in this embodiment is 5%; the mass fraction of the sodium silicate solution is 14%.

[0132] The ultrasonic power of the S02 blending ultrasonic treatment in this embodiment is 385W, and the ultrasonic time is 25min; the stirring speed of the S03 stirring treatment is 490r / min, and the stirring time is 42min.

[0133] The preparation method of the yttrium regulator of this embodiment is:

[0134] S101: yttrium oxide is first irradiated in a proton irradiation box for 8 minutes, with an irradiation power of 370W. After the irradiation is completed, irradiated yttrium oxide is obtained;

[0135] S102: The irradiated yttrium oxide is first subjected to a thermal reaction at a temperature of 210-230°C for 10-15 minutes, and then cooled to 55°C at a rate of 3°C / min and subjected to a heat preservation treatment;

[0136] S103: 2 parts by weight of heat-insulated yttrium oxide, 2 parts by weight of sodium alginate solution, 2 parts by weight of nano-silica sol and 4 parts by weight of sodium lignin sulfonate solution are mixed and ball-milled. After the ball-milling is completed, the mixture is washed with water and dried to obtain a yttrium regulator.

[0137] The mass fraction of the sodium alginate solution in this embodiment is 10%; the mass fraction of the sodium lignin sulfonate solution is 14%.

[0138] The ball milling speed of the blended ball milling treatment in this embodiment is 1400 r / min, and the ball milling is 2 h.

[0139] Comparative Example 1.

[0140] The difference from Example 3 is that modified graphene treatment is not used.

[0141] Comparative Example 2.

[0142] The difference from Example 3 is that no modifying liquid treatment is used in the modified graphene.

[0143] Comparative Example 3.

[0144] The difference from Example 3 is that no dry nano-silicon dioxide is added in the preparation of the modified solution.

[0145] Comparative Example 4.

[0146] The difference from Example 3 is that no yttrium regulator is added.

[0147] Comparative Example 5.

[0148] The difference from Example 3 is that the sodium alginate solution, nano-silica sol and sodium lignin sulfonate solution are not mixed and ball-milled in the preparation of the yttrium regulator.

[0149] 2-5% of the total amount of pure aluminum was added to pure aluminum by the products of Examples 1-5 and Comparative Examples 1-5, and the aluminum core of the cable was prepared by conventional technology. The products were placed in 2% hydrochloric acid mist for 12 hours, and the acid corrosion resistance of the products was tested for performance.

[0150]

[0151] It can be seen from comparative examples 1-5 and examples 1-5 that the product of example 3 has excellent tensile strength and electrical conductivity, which can play a significant coordinated improvement effect, and the acid corrosion resistance stability of the product is significant; the product is not treated with modified graphene and yttrium regulator is not added, and the performance of the product is significantly deteriorated. The two are coordinated and synergistic, and the performance effect of the product is most significant;

[0152] The modified graphene of the present invention is not treated with a modifying liquid, dry nano-silicon dioxide is not added in the preparation of the modifying liquid, and the yttrium regulator is not treated by mixing and ball milling with a sodium alginate solution, a nano-silica sol and a sodium lignin sulfonate solution in the preparation of the yttrium regulator. The performance of the products tends to deteriorate. The modified graphene and yttrium regulator obtained by the method of the present invention have the most significant performance effect of the product. Other methods are not as obvious as the effect of the present invention.

[0153] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0154] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A method for preparing a grain refiner, characterized in that: The following steps are involved: Step 1: First prepare a chitosan solution with a mass fraction of 5-7%; Step 2: Add 1-3 parts by weight of silane coupling agent and 2-4 parts by weight of sodium dodecylbenzene sulfonate to 6-9 parts by weight of chitosan solution and stir well to obtain chitosan solution; Step 3: Add 4-7 parts by weight of modified graphene and 1-3 parts by weight of yttrium regulator into 5-8 parts by weight of chitosan solution and stir for modification. After stirring, wash with water and dry to obtain a grain refiner.

2. A method for preparing a grain refiner according to claim 1, characterized in that: The silane coupling agent is silane coupling agent KH560.

3. The method for preparing a grain refiner according to claim 1, characterized in that: The stirring temperature of the stirring modification treatment in step 3 is 48-52° C., the stirring time is 20-30 min, and the stirring speed is 550-750 r / min.

4. The method for preparing a grain refiner according to claim 1, characterized in that: The modification method of the modified graphene is: S01: The graphene is first heated to 150°C at a rate of 1-3°C / min, kept at this temperature for 5-10min, then heated to 310°C at a rate of 2-4°C / min, and finally air-cooled to room temperature; S02: immersing the nano-silicon dioxide into a lanthanum chloride solution which is 3-5 times the total amount of the nano-silicon dioxide, then filtering and drying, and ultrasonically treating 3-5 parts by weight of the dried nano-silicon dioxide, 1-2 parts by weight of stearic acid, and 4-7 parts by weight of a sodium silicate solution, and then finishing the ultrasonic treatment to obtain a modified solution; S03: The graphene product of S01 and the modified liquid of S02 are stirred at a weight ratio of 2:

5. After the stirring is completed, the mixture is washed with water and dried to obtain modified graphene.

5. A method for preparing a grain refiner according to claim 4, characterized in that: The mass fraction of the lanthanum chloride solution is 3-6%; the mass fraction of the sodium silicate solution is 10-15%.

6. A method for preparing a grain refiner according to claim 4, characterized in that: The ultrasonic power of the S02 blending ultrasonic treatment is 350-400W, and the ultrasonic time is 20-30min; the stirring speed of the S03 stirring treatment is 450-500r / min, and the stirring time is 35-45min.

7. The method for preparing a grain refiner according to claim 1, characterized in that: The preparation method of the yttrium regulator is: S101: yttrium oxide is first irradiated in a proton irradiation box for 5-10 minutes, with an irradiation power of 350-400W. After the irradiation is completed, irradiated yttrium oxide is obtained; S102: The irradiated yttrium oxide is first subjected to a thermal reaction at a temperature of 210-230°C for 10-15 minutes, and then cooled to 55°C at a rate of 2-4°C / min and subjected to heat preservation treatment; S103: 1-2 parts by weight of heat-insulated yttrium oxide, 1-3 parts by weight of sodium alginate solution, 1-2 parts by weight of nano-silica sol and 2-5 parts by weight of sodium lignin sulfonate solution are mixed and ball-milled. After the ball-milling is completed, the mixture is washed with water and dried to obtain a yttrium regulator.

8. A method for preparing a grain refiner according to claim 7, characterized in that: The mass fraction of the sodium alginate solution is 8-12%; the mass fraction of the sodium lignin sulfonate solution is 10-15%.

9. A method for preparing a grain refiner according to claim 7, characterized in that: The ball milling speed of the blended ball milling treatment is 1000-1500 r / min, and the ball milling is performed for 2 hours.