Nickel-based superalloy carbide morphology control method
By adding rare earth elements La and Ce to the intermediate alloy during the smelting of nickel-based superalloys, the nucleation points of carbides are controlled, solving the problem of uneven carbide distribution in deformed superalloys. This achieves a small-sized granular dispersion distribution, improving the material's microstructure uniformity and crack resistance.
Patent Information
- Application Number
- CN202411008780.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-12
AI Technical Summary
The aggregation and large-size distribution of carbides in deformed superalloys lead to poor microstructure uniformity, which easily forms crack initiation sites and affects the quality of billets and parts.
By adding rare earth elements La and Ce as intermediate alloys during the smelting process of nickel-based superalloys, the nucleation points of carbides are controlled to form small-sized granular dispersed distribution. Vacuum induction melting and self-consumable remelting processes are used to control the morphology and distribution of carbides.
This method transformed the large-sized, Chinese character-shaped aggregated distribution of carbides in the GH4169 alloy into a small-sized, dispersed granular distribution, improving the material's microstructure uniformity and reducing crack initiation.
Smart Images

Figure CN118932210A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high-temperature alloy smelting, and in particular to a method for controlling the morphology of nickel-based high-temperature alloy carbides. Background Art
[0002] In deformed high-temperature alloys, Nb, Ti and other elements are usually added for strengthening, and they all contain a certain amount of C elements, so MC carbides are inevitably formed. For alloys with higher Ti content, such as GH710 and GH738, a large amount of TiC is usually formed, and for alloys with higher Nb content, such as GH4169, GH2150 and GH1015, a large amount of NbC is usually formed. The ingot specifications of deformed high-temperature alloys are large, easy to segregate, and will form aggregated and larger carbides, which will reduce the uniformity of the material's organization on the one hand, and easily form crack sources during subsequent deformation and use, leading to cracking of billets or parts. Summary of the invention
[0003] The object of the present invention is to provide a method for controlling the morphology of nickel-based high-temperature alloy carbides to solve the problems raised in the above-mentioned background technology.
[0004] To achieve the above object, the present invention provides the following technical solution: a method for controlling the morphology of nickel-based high-temperature alloy carbides, comprising the following steps;
[0005] Step 1: Raw material preparation:
[0006] S1.1. Prepare ingredients according to the composition requirements of GH4169 alloy;
[0007] S1.2, weigh the alloy materials Fe, graphite, Ni plate, Mo bar, Cr, Nb bar, Ti block, Al bean and NiCe, NiLa master alloy respectively according to the above mass percentages for later use;
[0008] S2. Vacuum induction melting:
[0009] S2.1. After evacuating the furnace until the vacuum degree is less than 5 Pa and the leakage rate is less than 25 mbar / L·s-1, first add all the Ni plates, metal Fe, Nb bars, Mo bars, and metal Cr into the crucible of the vacuum induction furnace in sequence, slowly increase the power until the steel is completely melted, and control the temperature of the molten steel to ≥1500℃;
[0010] S2.2, adding NiCe and NiLa master alloys, controlling the temperature of the molten steel at 1460℃-1500℃ after melting, and refining, the refining time is ≥30min, and electromagnetic stirring is applied during the refining process;
[0011] S2.3, then reduce the power until the melt surface forms a film, add graphite first, dissolve it, reduce the power until the melt surface forms a film, add Al beans, dissolve it, reduce the power until the melt surface forms a film, and finally add Ti blocks, dissolve it, and control the temperature at 1460℃-1500℃ during the process;
[0012] S2.4, adjust the temperature of molten steel to the pouring temperature of 1440-1450℃, and prepare for pouring;
[0013] S2.5, hoisting the mold assembly with the preheated temperature to the ingot mold chamber and then casting to obtain a vacuum induction ingot;
[0014] S3. Consumable electrode treatment:
[0015] S3.1, vacuum induction casting ingot is prepared into consumable electrode after stress relief annealing, surface treatment and head and tail cutting;
[0016] S4: Vacuum consumable remelting:
[0017] S4.1. Weld, center, load and vacuum the prepared consumable electrode. When the vacuum degree is ≤0.1Pa and the leakage rate is ≤0.1Pa / min, input the process parameters for smelting.
[0018] S4.2. During the smelting process, the melting rate and droplet are controlled. After the smelting is completed, the smelter is cooled for a certain period of time and then taken out of the furnace to obtain a consumable ingot.
[0019] Preferably, the GH4169 alloy composition requires the following component mass percentage requirements: Fe (balance), C: 0.015-0.06%, Cr: 17-21%, Ni: 50-55%, Mo: 2.80-3.30%, Nb: 4.75-5.50%, Ti: 0.75-1.15%, Al: 0.3-0.7%, B≤0.006%, P≤0.015%, Co≤1%, Ta≤0.10%, Mn≤0.35%, Si≤0.35%, S≤0.015%, Cu≤0.30%, La+Ce: 0.03-0.06%.
[0020] Preferably, the rare earth elements La and Ce are used as additives in S1, and the total amount of La and Ce added is 0.03-0.06% by weight.
[0021] Preferably, the order of adding materials in S2 is: (Ni, Fe, Nb, Mo, Cr)→La+Ce→C→Al→Ti.
[0022] Preferably, the O content in the molten steel before adding the intermediate alloy of La and Ce in S2 is 30-50 ppm, and the refining temperature after adding the intermediate alloy of NiLa and NiCe is 1460-1480° C., and the refining time is 30-50 min.
[0023] Preferably, after the intermediate alloy of La and Ce is added to S2, the temperature of the molten steel until the steel is poured is ≤1500°C, the vacuum degree is ≤5 Pa, and the steel pouring temperature is ≤1450°C.
[0024] Preferably, the melting rate range in the consumable melting process in S4 is 2.8-3.5 kg / min, the droplet range is 2-101 / s, and the cooling gas pressure is ≥1000 Pa.
[0025] Compared with the prior art, the beneficial effects of the present invention are: by increasing the carbide nucleation points of the high-temperature alloy during the solidification process, and the nucleation points can also hinder the solute flow between dendrites during the solidification process, the morphology and distribution of the carbides can be controlled; the advantage of the present invention is that by controlling the number and size of rare earth oxide particles as carbide nucleation cores, the morphology and distribution of carbides in the GH4169 alloy can be changed, so that the carbides in the GH4169 alloy are changed from large-sized Chinese character-shaped aggregated distribution to small-sized granular dispersed distribution, thereby improving the uniformity of the carbides of the GH4169 alloy. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The carbide in the core of the GH4169Ф508mm consumable ingot corresponding to Example 1;
[0027] Figure 2 The carbide in the core of the GH4169Ф508mm consumable ingot corresponding to Example 2;
[0028] Figure 3 The carbide in the core of the GH4169Ф508mm consumable ingot corresponding to Comparative Example 1;
[0029] Figure 4 This is the carbide in the core of the GH4169Ф508mm consumable ingot corresponding to Comparative Example 2. DETAILED DESCRIPTION
[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] See also Figure 1-4The present invention provides a technical solution: The present invention provides a method for controlling the morphology of nickel-based high-temperature alloy carbides, and the specific solution is as follows:
[0032] S1. Raw material preparation:
[0033] S1.1. Prepare the ingredients according to the composition requirements of GH4169 alloy. The mass percentage requirements of the components are as follows: Fe (balance), C: 0.015-0.06%, Cr: 17-21%, Ni: 50-55%, Mo: 2.80-3.30%, Nb: 4.75-5.50%, Ti: 0.75-S1.15%, Al: 0.3-0.7%, B≤0.006%, P≤0.015%, Co≤1%, Ta≤0.10%, Mn≤0.35%, Si≤0.35%, S≤0.015%, Cu≤0.30%, La+Ce: 0.03-0.06%.
[0034] S1.2. Weigh the alloy materials of metal Fe, graphite, Ni plate, Mo bar, metal Cr, Nb bar, Ti block, Al bean and NiCe, NiLa intermediate alloy according to the above mass percentages and set aside.
[0035] S2. Vacuum induction melting
[0036] S2.1. After evacuating the furnace until the vacuum degree is less than 5 Pa and the leakage rate is less than 25 mbar / L·s-1, first add all the Ni plates, metal Fe, Nb bars, Mo bars, and metal Cr into the crucible of the vacuum induction furnace in sequence, slowly increase the power until the steel is completely melted, and control the temperature of the molten steel to ≥1500℃;
[0037] S2.2, adding NiCe and NiLa master alloys, controlling the temperature of the molten steel at 1460℃-1500℃ after melting, and refining, the refining time is ≥30min, and electromagnetic stirring is applied during the refining process;
[0038] S2.3, then reduce the power until the melt surface forms a film, add graphite first, dissolve it, reduce the power until the melt surface forms a film, add Al beans, dissolve it, reduce the power until the melt surface forms a film, and finally add Ti blocks, dissolve it, and control the temperature at 1460℃-1500℃ during the process;
[0039] S2.4, adjust the temperature of molten steel to the pouring temperature of 1440-1450℃, and prepare for pouring;
[0040] S2.5. The mold set with a certain preheating temperature is hoisted into the ingot mold room and then poured to obtain a vacuum induction ingot.
[0041] S3. Consumable electrode treatment
[0042] The S3.1 vacuum induction ingot is prepared as a consumable electrode after stress relief annealing, surface treatment and head and tail cutting.
[0043] S4: Vacuum consumable remelting
[0044] S4.1 Weld, center, load and vacuum the prepared consumable electrode. When the vacuum degree is ≤0.1Pa and the leakage rate is ≤0.1Pa / min, input the process parameters for smelting;
[0045] S4.2 During the smelting process, the melting rate and droplet are controlled. After the smelting is completed, the smelter is cooled for a certain period of time and then taken out of the furnace to obtain a consumable ingot.
[0046] The mass percentages of some elements in S1 are as follows: C: 0.020-0.030%, Nb: 5.40-5.45%, Ti: 0.95-1.05%, La+Ce: 0.045%.
[0047] The content of O in the molten steel before adding the intermediate alloy of La and Ce in S2 is 40-50 ppm, the refining temperature after adding the intermediate alloy of NiLa and NiCe is 1470-1480° C., and the refining time is 40 min.
[0048] Wherein, after the intermediate alloy of La and Ce is added to S2, the temperature range of the molten steel is 1460-1480°C, the vacuum degree is ≤5pa, and the pouring temperature is 1440-1450°C. ;
[0049] The electrode annealing temperature in S3 is 900-1050°C, the holding time is 4-7h, and when the furnace is cooled to a temperature ≤500°C, it is air-cooled out of the furnace; the surface is polished to be free of oxide scale, the head is sawed to remove the riser, and the tail is sawed to remove the affected area;
[0050] Among them, the melting rate range of S4 is 2.8-3.5kg / min, the droplet range is 3-71 / s, and the cooling gas pressure is 1200-1300pa.
[0051] The present invention is further described in detail below with reference to specific embodiments.
[0052] Embodiment 1, comprises the following S:
[0053] S1. Raw material preparation:
[0054] S1.1. Prepare the ingredients according to the composition requirements of GH4169 alloy. The mass percentage requirements of the components are as follows: Fe (balance), C: 0.015-0.06%, Cr: 17-21%, Ni: 50-55%, Mo: 2.80-3.30%, Nb: 4.75-5.50%, Ti: 0.75-S1.15%, Al: 0.3-0.7%, B≤0.006%, P≤0.015%, Co≤1%, Ta≤0.10%, Mn≤0.35%, Si≤0.35%, S≤0.015%, Cu≤0.30%, La+Ce: 0.03-0.06%.
[0055] S1.2. Weigh the alloy materials of metal Fe, graphite, Ni plate, Mo bar, metal Cr, Nb bar, Ti block, Al bean and NiCe, NiLa intermediate alloy according to the above mass percentages and set aside.
[0056] S2. Vacuum induction melting
[0057] S2.1. After evacuating the furnace until the vacuum degree is less than 5 Pa and the leakage rate is less than 25 mbar / L·s-1, first add all the Ni plates, metal Fe, Nb bars, Mo bars, and metal Cr into the crucible of the vacuum induction furnace in sequence, slowly increase the power until the steel is completely melted, and control the temperature of the molten steel to ≥1500℃;
[0058] S2.2, adding NiCe and NiLa master alloys, controlling the temperature of the molten steel at 1460℃-1500℃ after melting, and refining, the refining time is ≥30min, and electromagnetic stirring is applied during the refining process;
[0059] S2.3, then reduce the power until the melt surface forms a film, add graphite first, dissolve it, reduce the power until the melt surface forms a film, add Al beans, dissolve it, reduce the power until the melt surface forms a film, and finally add Ti blocks, dissolve it, and control the temperature at 1460℃-1500℃ during the process;
[0060] S2.4, adjust the temperature of molten steel to the pouring temperature of 1440-1450℃, and prepare for pouring;
[0061] S2.5. The mold set with a certain preheating temperature is hoisted into the ingot mold room and then poured to obtain a vacuum induction ingot.
[0062] S3. Consumable electrode treatment
[0063] The S3.1 vacuum induction ingot is prepared as a consumable electrode after stress relief annealing, surface treatment and head and tail cutting.
[0064] S4: Vacuum consumable remelting
[0065] S4.1 Weld, center, load and vacuum the prepared consumable electrode. When the vacuum degree is ≤0.1Pa and the leakage rate is ≤0.1Pa / min, input the process parameters for smelting;
[0066] S4.2 During the smelting process, the melting rate and droplet are controlled. After the smelting is completed, the smelter is cooled for a certain period of time and then taken out of the furnace to obtain a consumable ingot.
[0067] The mass percentages of some elements in S1 are as follows: C: 0.025%, Nb: 5.43%, Ti: 1.0%, La+Ce: 0.045%.
[0068] The O content in the molten steel before adding NiLa and NiCe master alloys in S2 is 42ppm, the refining temperature is 1471°C, the refining time is 40min, and the test temperatures of the molten steel after adding graphite, Al beans and Ti blocks are 1473°C, 1465°C and 1477°C respectively; the pouring temperature is 1448°C; and the preheating temperature of the ingot mold is 400°C;
[0069] In the S3, the electrode annealing temperature is 1000, the holding time is 5h, and when the furnace is cooled to a temperature ≤ 500°C, it is taken out of the furnace and air-cooled; the surface is polished until there is no oxide scale, the head is sawed to remove the riser, and the tail is sawed to remove the affected area;
[0070] In the S4, the melting rate is 3.2 kg / min, the droplet range is 61 / s, and the cooling gas pressure is controlled at 1250 Pa.
[0071] The sample was cut from the GH4169 consumable ingot head at 500 mm, and the longitudinal cast carbides were observed at the center. Figure 1 shown.
[0072] Embodiment 2, comprises the following S:
[0073] S1. Raw material preparation:
[0074] S1.1. Prepare the ingredients according to the composition requirements of GH4169 alloy. The mass percentage requirements of the components are as follows: Fe (balance), C: 0.015-0.06%, Cr: 17-21%, Ni: 50-55%, Mo: 2.80-3.30%, Nb: 4.75-5.50%, Ti: 0.75-S1.15%, Al: 0.3-0.7%, B≤0.006%, P≤0.015%, Co≤1%, Ta≤0.10%, Mn≤0.35%, Si≤0.35%, S≤0.015%, Cu≤0.30%, La+Ce: 0.03-0.06%.
[0075] S1.2. Weigh the alloy materials of metal Fe, graphite, Ni plate, Mo bar, metal Cr, Nb bar, Ti block, Al bean and NiCe, NiLa intermediate alloy according to the above mass percentages and set aside.
[0076] S2. Vacuum induction melting
[0077] S2.1. After evacuating the furnace until the vacuum degree is less than 5 Pa and the leakage rate is less than 25 mbar / L·s-1, first add all the Ni plates, metal Fe, Nb bars, Mo bars, and metal Cr into the crucible of the vacuum induction furnace in sequence, slowly increase the power until the steel is completely melted, and control the temperature of the molten steel to ≥1500℃;
[0078] S2.2, adding NiCe and NiLa master alloys, controlling the temperature of the molten steel at 1460℃-1500℃ after melting, and refining, the refining time is ≥30min, and electromagnetic stirring is applied during the refining process;
[0079] S2.3, then reduce the power until the melt surface forms a film, add graphite first, dissolve it, reduce the power until the melt surface forms a film, add Al beans, dissolve it, reduce the power until the melt surface forms a film, and finally add Ti blocks, dissolve it, and control the temperature at 1460℃-1500℃ during the process;
[0080] S2.4, adjust the temperature of molten steel to the pouring temperature of 1440-1450℃, and prepare for pouring;
[0081] S2.5. The mold set with a certain preheating temperature is hoisted into the ingot mold room and then poured to obtain a vacuum induction ingot.
[0082] S3. Consumable electrode treatment
[0083] S3.1. The vacuum induction cast ingot is prepared into a consumable electrode after stress relief annealing, surface treatment and head and tail cutting.
[0084] S4: Vacuum consumable remelting
[0085] S4.1. Weld, center, load and vacuum the prepared consumable electrode. When the vacuum degree is ≤0.1Pa and the leakage rate is ≤0.1Pa / min, input the process parameters for smelting.
[0086] S4.2. During the smelting process, the melting rate and droplet are controlled. After the smelting is completed, the smelter is cooled for a certain period of time and then taken out of the furnace to obtain a consumable ingot.
[0087] The mass percentages of some elements in S1 are as follows: C: 0.025%, Nb: 5.43%, Ti: 1.0%, La+Ce: 0.045%.
[0088] The O content in the molten steel before adding NiLa and NiCe master alloys in S2 is 48ppm, the refining temperature is 1478°C, the refining time is 40min, and the test temperatures of the molten steel after adding graphite, Al beans and Ti blocks are 1461°C, 1467°C and 1471°C respectively; the pouring temperature is 1445°C; and the preheating temperature of the ingot mold is 400°C;
[0089] In the S3, the electrode annealing temperature is 1000, the holding time is 5h, and when the furnace is cooled to a temperature ≤ 500°C, it is taken out of the furnace and air-cooled; the surface is polished until there is no oxide scale, the head is sawed to remove the riser, and the tail is sawed to remove the affected area;
[0090] In the S4, the melting rate is 3.2 kg / min, the droplet range is 61 / s, and the cooling gas pressure is controlled at 1250 Pa.
[0091] The sample was cut from the GH4169 consumable ingot head at 500 mm, and the longitudinal cast carbides were observed at the center. Figure 2 shown.
[0092] Comparative Example 1 includes the following S:
[0093] S1. Raw material preparation:
[0094] S1.1. Prepare the ingredients according to the composition requirements of GH4169 alloy. The mass percentage requirements of the components are as follows: Fe (balance), C: 0.015-0.06%, Cr: 17-21%, Ni: 50-55%, Mo: 2.80-3.30%, Nb: 4.75-5.50%, Ti: 0.75-S1.15%, Al: 0.3-0.7%, B≤0.006%, P≤0.015%, Co≤1%, Ta≤0.10%, Mn≤0.35%, Si≤0.35%, S≤0.015%, Cu≤0.30%, La+Ce: 0.03-0.06%.
[0095] S1.2. Weigh the alloy materials of metal Fe, graphite, Ni plate, Mo bar, metal Cr, Nb bar, Ti block and Al bean according to the above mass percentages and set aside.
[0096] S2. Vacuum induction melting
[0097] S2.1. After evacuating the furnace until the vacuum degree is less than 5 Pa and the leakage rate is less than 25 mbar / L·s-1, first add all the Ni plates, metal Fe, Nb bars, Mo bars, and metal Cr into the crucible of the vacuum induction furnace in sequence, slowly increase the power until the steel is completely melted, and control the temperature of the molten steel to ≥1500℃;
[0098] S2.2, after melting, the temperature of the molten steel is controlled at 1460℃-1500℃, and refining is carried out. The refining time is ≥30min, and electromagnetic stirring is applied during the refining process;
[0099] S2.3, then reduce the power until the melt surface forms a film, add graphite first, dissolve it, reduce the power until the melt surface forms a film, add Al beans, dissolve it, reduce the power until the melt surface forms a film, and finally add Ti blocks, dissolve it, and control the temperature at 1460℃-1500℃ during the process;
[0100] S2.4, adjust the temperature of molten steel to the pouring temperature of 1440-1450℃, and prepare for pouring;
[0101] S2.5. The mold set with a certain preheating temperature is hoisted into the ingot mold room and then poured to obtain a vacuum induction ingot.
[0102] S3. Consumable electrode treatment
[0103] S3.1. The vacuum induction cast ingot is prepared into a consumable electrode after stress relief annealing, surface treatment and head and tail cutting.
[0104] S4: Vacuum consumable remelting
[0105] S4.1. Weld, center, load and vacuum the prepared consumable electrode. When the vacuum degree is ≤0.1Pa and the leakage rate is ≤0.1Pa / min, input the process parameters for smelting.
[0106] S4.2. During the smelting process, the melting rate and droplet are controlled. After the smelting is completed, the smelter is cooled for a certain period of time and then taken out of the furnace to obtain a consumable ingot.
[0107] The mass percentages of some elements in S1 are as follows: C: 0.025%, Nb: 5.43%, Ti: 1.0%.
[0108] The O content of S2 before refining is 37ppm, the refining temperature is 1471℃, the refining time is 40min, and the test temperatures of the molten steel after adding graphite, Al beans and Ti blocks are 1477℃, 1462℃ and 1473℃ respectively; the pouring temperature is 1449℃; and the preheating temperature of the ingot mold is 400℃;
[0109] In the S3, the electrode annealing temperature is 1000, the holding time is 5h, and when the furnace is cooled to a temperature ≤ 500°C, it is taken out of the furnace and air-cooled; the surface is polished until there is no oxide scale, the head is sawed to remove the riser, and the tail is sawed to remove the affected area;
[0110] In the S4, the melting rate is 3.2 kg / min, the droplet range is 61 / s, and the cooling gas pressure is controlled at 1250 Pa.
[0111] The sample was cut from the GH4169 consumable ingot head at 500 mm, and the longitudinal cast carbides were observed at the center. Figure 3 shown.
[0112] Comparative Example 2 includes the following S:
[0113] S1. Raw material preparation:
[0114] S1.1. Prepare the ingredients according to the composition requirements of GH4169 alloy. The mass percentage requirements of the components are as follows: Fe (balance), C: 0.015-0.06%, Cr: 17-21%, Ni: 50-55%, Mo: 2.80-3.30%, Nb: 4.75-5.50%, Ti: 0.75-S1.15%, Al: 0.3-0.7%, B≤0.006%, P≤0.015%, Co≤1%, Ta≤0.10%, Mn≤0.35%, Si≤0.35%, S≤0.015%, Cu≤0.30%, La+Ce: 0.03-0.06%.
[0115] S1.2. Weigh the alloy materials of metal Fe, graphite, Ni plate, Mo bar, metal Cr, Nb bar, Ti block and Al bean according to the above mass percentages and set aside.
[0116] S2. Vacuum induction melting
[0117] S2.1. After evacuating the furnace until the vacuum degree is less than 5 Pa and the leakage rate is less than 25 mbar / L·s-1, first add all the Ni plates, metal Fe, Nb bars, Mo bars, metal Cr, and graphite into the crucible of the vacuum induction furnace in sequence, slowly increase the power until it is completely melted, and control the temperature of the molten steel to ≥1500℃;
[0118] S2.2, then reduce the power until the melt surface forms a film, then add Al beans, melt and clear, reduce the power until the melt surface forms a film, then add Ti blocks, melt and clear, and control the temperature at 1460℃-1500℃ during the process;
[0119] S2.3, after melting, the temperature of the molten steel is controlled at 1460℃-1500℃, and refining is carried out. The refining time is ≥30min, and electromagnetic stirring is applied during the refining process;
[0120] S2.4, adjust the temperature of molten steel to the pouring temperature of 1440-1450℃, and prepare for pouring;
[0121] S2.5. The mold set with a certain preheating temperature is hoisted into the ingot mold room and then poured to obtain a vacuum induction ingot.
[0122] S3. Consumable electrode treatment
[0123] S3.1. The vacuum induction cast ingot is prepared into a consumable electrode after stress relief annealing, surface treatment and head and tail cutting.
[0124] S4: Vacuum consumable remelting
[0125] S4.1. Weld, center, load and vacuum the prepared consumable electrode. When the vacuum degree is ≤0.1Pa and the leakage rate is ≤0.1Pa / min, input the process parameters for smelting.
[0126] S4.2. During the smelting process, the melting rate and droplet are controlled. After the smelting is completed, the smelter is cooled for a certain period of time and then taken out of the furnace to obtain a consumable ingot.
[0127] The mass percentages of some elements in S1 are as follows: C: 0.025%, Nb: 5.43%, Ti: 1.0%.
[0128] The O content in the S2 before adding Al beans is 32ppm, and the test temperatures of the molten steel after adding Al beans and adding Ti blocks are 1468°C and 1461°C respectively; the refining temperature is 1475°C, the refining time is 40min, the pouring temperature is 1442°C; the preheating temperature of the ingot mold is 400°C;
[0129] In the S3, the electrode annealing temperature is 1000, the holding time is 5h, and when the furnace is cooled to a temperature ≤ 500°C, it is taken out of the furnace and air-cooled; the surface is polished until there is no oxide scale, the head is sawed to remove the riser, and the tail is sawed to remove the affected area;
[0130] In the S4, the melting rate is 3.2 kg / min, the droplet range is 61 / s, and the cooling gas pressure is controlled at 1250 Pa.
[0131] The sample was cut from the GH4169 consumable ingot head at 500 mm, and the longitudinal cast carbides were observed at the center. Figure 4 shown.
[0132] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for controlling the morphology of nickel-based high-temperature alloy carbides, characterized in that: The steps include: S1. Raw material preparation: S1.
1. Prepare ingredients according to the composition requirements of GH4169 alloy; S1.2, weigh the alloy materials Fe, graphite, Ni plate, Mo bar, Cr, Nb bar, Ti block, Al bean and NiCe, NiLa master alloy respectively according to the above mass percentages for later use; S2. Vacuum induction melting: S2.
1. After evacuating the furnace until the vacuum degree is less than 5 Pa and the leakage rate is less than 25 mbar / L·s-1, first add all the Ni plates, metal Fe, Nb bars, Mo bars, and metal Cr into the crucible of the vacuum induction furnace in sequence, slowly increase the power until the steel is completely melted, and control the temperature of the molten steel to ≥1500℃; S2.2, adding NiCe and NiLa master alloys, controlling the temperature of the molten steel at 1460℃-1500℃ after melting, and refining, the refining time is ≥30min, and electromagnetic stirring is applied during the refining process; S2.3, then reduce the power until the melt surface forms a film, add graphite first, dissolve it, reduce the power until the melt surface forms a film, add Al beans, dissolve it, reduce the power until the melt surface forms a film, and finally add Ti blocks, dissolve it, and control the temperature at 1460℃-1500℃ during the process; S2.4, adjust the temperature of molten steel to the pouring temperature of 1440-1450℃, and prepare for pouring; S2.5, hoisting the mold assembly with the preheated temperature to the ingot mold chamber and then casting to obtain a vacuum induction ingot; S3. Consumable electrode treatment: S3.1, vacuum induction casting ingot is prepared into consumable electrode after stress relief annealing, surface treatment and head and tail cutting; S4: Vacuum consumable remelting: S4.
1. Weld, center, load and vacuum the prepared consumable electrode. When the vacuum degree is ≤0.1Pa and the leakage rate is ≤0.1Pa / min, input the process parameters for smelting. S4.
2. During the smelting process, the melting rate and droplet are controlled. After the smelting is completed, the smelter is cooled for a certain period of time and then taken out of the furnace to obtain a consumable ingot.
2. The method for controlling the morphology of nickel-based high-temperature alloy carbides according to claim 1, characterized in that: The GH4169 alloy composition requirements are as follows: Fe (balance), C: 0.015-0.06%, Cr: 17-21%, Ni: 50-55%, Mo: 2.80-3.30%, Nb: 4.75-5.50%, Ti: 0.75-1.15%, Al: 0.3-0.7%, B≤0.006%, P≤0.015%, Co≤1%, Ta≤0.10%, Mn≤0.35%, Si≤0.35%, S≤0.015%, Cu≤0.30%, La+Ce: 0.03-0.06%.
3. The method for controlling the morphology of nickel-based high-temperature alloy carbides according to claim 1, characterized in that: The rare earth elements La and Ce are used as additives in S1, and the total amount of La and Ce added is 0.03-0.06% by weight.
4. The method for controlling the morphology of nickel-based high-temperature alloy carbides according to claim 1, characterized in that: The order of adding materials in S2 is: (Ni, Fe, Nb, Mo, Cr)→La+Ce→C→Al→Ti.
5. The method for controlling the morphology of nickel-based high-temperature alloy carbides according to claim 1, characterized in that: The O content in the molten steel before adding the intermediate alloy of La and Ce in the S2 is 30-50ppm, and the refining temperature after adding the intermediate alloy of NiLa and NiCe is 1460-1480°C, and the refining time is 30-50min.
6. The method for controlling the morphology of nickel-based high-temperature alloy carbides according to claim 1, characterized in that: After the intermediate alloy of La and Ce is added to the S2, the temperature of the molten steel is ≤1500°C, the vacuum degree is ≤5 Pa, and the pouring temperature is ≤1450°C.
7. The method for controlling the morphology of nickel-based high-temperature alloy carbides according to claim 1, characterized in that: The melting rate range in the consumable melting process in S4 is 2.8-3.5 kg / min, the droplet range is 2-101 / s, and the cooling gas pressure is ≥1000 Pa.