High-strength and high-heat-conductivity CuAgYSi alloy material for vapor chamber and preparation method of CuAgYSi alloy material

By preparing CuAgYSi alloy material, the shortcomings of traditional heat-smooth plate materials in high strength and high thermal conductivity are solved, and the comprehensive performance of high tensile strength, elongation and thermal conductivity are achieved, meeting the heat dissipation needs of high power equipment.

CN118932211APending Publication Date: 2024-11-12HUNAN ZHIHAOHANG PRECISION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411346975.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional heat-smoothing plate materials have shortcomings in terms of high strength and high thermal conductivity, and cannot meet the heat dissipation needs of high-power chips and other equipment.

Method used

CuAgYSi alloy material is used to mix Ag, Y, Si and Cu in a specific proportion, and undergo smelting, casting, uniform annealing and cold processing deformation treatments. Combined with multiple aging and cold processing treatments, a high tensile strength and extension are prepared. CuAgYSi alloy material with length and thermal conductivity.

Benefits of technology

The high tensile strength, elongation and thermal conductivity of CuAgYSi alloy materials are achieved, meeting the performance requirements of high strength and high thermal conductivity, and are suitable for high performance heat homogenization plate applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932211A_ABST
    Figure CN118932211A_ABST
Patent Text Reader

Abstract

The invention discloses a high-strength high-heat-conductivity CuAgYSi alloy material for a vapor chamber and a preparation method of the high-strength high-heat-conductivity CuAgYSi alloy material. The preparation method comprises the following steps of: preparing the following raw materials in percentage by mass: 1.0-5.0 wt% of Ag; y, 0.2 wt% to 0.4 wt%; si, 0.2 to 0.4 wt%; and the balance of Cu. The CuAgYSi alloy material contains Ag, Y and Si elements in a specific proportion, an AgYSi fiber phase can be formed, and precipitation of the Ag phase in the CuAgYSi alloy material is facilitated on the basis of further degassing and deoxidizing pure alloy melt through combined addition of rare earth Y and Si. The CuAgYSi alloy material prepared by the preparation method disclosed by the invention has relatively high tensile strength, elongation and thermal conductivity. The preparation method disclosed by the invention is simple, low in equipment requirement and suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of new materials, and in particular to a high-strength and high-thermal-conductivity CuAgYSi alloy material for a vapor chamber and a preparation method thereof. Background Art

[0002] A heat spreader is a plate-shaped heat transfer device that is formed by injecting a working liquid (i.e., working fluid) into a near-vacuum cavity with a capillary structure inside and can perform phase change heat transfer. Its main structures include a shell plate, a liquid wick, a liquid-filled tube, and a working fluid. The interior of the heat spreader is a near-vacuum cavity structure, which is light in weight; it does not require external force to drive it during operation, saving energy; its cavity is welded and sealed, and will not leak, making it safe and reliable; its heat transfer method is phase change heat transfer, with a high heat transfer coefficient; it can perform two-dimensional heat transfer, has a fast heat conduction speed, and can quickly and evenly transfer the heat from a point heat source and distribute it on the heat dissipation surface; its external dimensions can be designed according to the specific application scenario; the LED can be directly packaged on it, or it can be tightly fitted to the chip base to reduce contact thermal resistance.

[0003] The heat spreader is mainly used for high-speed transmission hard disk heat dissipation, high-performance microprocessor unit heat dissipation (such as CPU, graphics card, etc.), high-power LED, chip heat dissipation, high-power laser transmitter heat dissipation, satellite energy conversion unit heat dissipation and cooling of medical equipment radiation components. Because it has to withstand the pressure generated during phase change and quickly conduct heat, the heat spreader generally requires good strength and welding performance on the basis of high thermal conductivity. At present, the heat spreader material is TU2 copper or CuNiP alloy. The former has a higher thermal conductivity but insufficient strength, and the latter has acceptable strength but average thermal conductivity. As the power density of chips and other devices becomes higher and higher, the heat dissipation demand increases significantly, and traditional heat spreaders cannot meet the performance requirements of high strength and high thermal conductivity. There is an urgent need to develop new high-performance heat spreader materials. Summary of the invention

[0004] One of the purposes of the present invention is to provide a high-strength and high-thermal-conductivity CuAgYSi alloy material for a heat spreader, which has high tensile strength, elongation and thermal conductivity.

[0005] A second object of the present invention is to provide a method for preparing a high-strength and high-thermal-conductivity CuAgYSi alloy material for a heat spreader. The CuAgYSi alloy material prepared by the method has high tensile strength, elongation and thermal conductivity.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] On the one hand, the present invention provides a high-strength and high-thermal-conductivity CuAgYSi alloy material for a heat spreader, which is composed of the following raw materials by mass fraction: Ag, 1.0-5.0wt%; Y, 0.2-0.4wt%; Si, 0.2-0.4wt%; and the balance is Cu.

[0008] On the other hand, a method for preparing a high-strength and high-thermal-conductivity CuAgYSi alloy material for a vapor chamber is provided, comprising the following steps:

[0009] S10, mixing Ag, Y, Si, and Cu according to mass fractions and performing smelting treatment to obtain a molten copper alloy;

[0010] S20, casting the molten copper alloy to obtain a copper alloy ingot;

[0011] S30, performing homogenization annealing treatment on the copper alloy ingot;

[0012] S40, performing cold working deformation treatment on the copper alloy ingot after homogenization annealing treatment, and then performing multiple aging treatments and multiple cold working deformation treatments alternately to obtain a CuAgYSi alloy material.

[0013] As a preferred solution of the method for preparing a high-strength and high-thermal-conductivity CuAgYSi alloy material for a vapor chamber, in step S10, Ag, Y, and Si are added in the form of pure elements, and Cu is added in the form of electrolytic copper.

[0014] As a preferred solution for the preparation method of high-strength and high-thermal-conductivity CuAgYSi alloy material for heat spreader, step S10 is specifically as follows: first, Cu and Ag are mixed and heated to melt, and then Si and Y are added in sequence. After sufficient stirring under inert gas protection, the slag is skimmed to obtain a pure melt, the furnace temperature is controlled to be 1450-1500°C, and the molten copper alloy is obtained after melting.

[0015] As a preferred solution of the method for preparing the high-strength and high-thermal-conductivity CuAgYSi alloy material for the heat spreader, in step S20, the casting temperature is 1250-1350°C.

[0016] As a preferred solution for the preparation method of high-strength and high-thermal-conductivity CuAgYSi alloy material for heat spreader, step S30 is specifically: subjecting the copper alloy ingot to homogenization annealing treatment in a nitrogen atmosphere at a temperature of 950-980° C. for 4-8 hours.

[0017] As a preferred solution of the method for preparing the high-strength and high-thermal-conductivity CuAgYSi alloy material for the vapor chamber, step S40 specifically includes the following steps:

[0018] S40a, subjecting the homogenized copper alloy ingot to cold working deformation treatment, so that the deformation amount is greater than 75%;

[0019] S40b, performing aging treatment and cold working deformation treatment on the copper alloy treated in step S40a in sequence, so that the deformation amount is greater than 75%;

[0020] S40c, performing aging treatment and cold working deformation treatment on the copper alloy treated in step S40b in sequence, so that the deformation amount is greater than 60%;

[0021] S40d, performing three-level aging and cold working deformation treatments on the copper alloy treated in step S40c in sequence, so that the deformation amount is 50%;

[0022] S40e, annealing the copper alloy treated in step S40d to obtain a CuAgYSi alloy material.

[0023] As a preferred solution for the preparation method of the high-strength and high-thermal-conductivity CuAgYSi alloy material for the vapor chamber, the aging treatment in step S40b is carried out under a nitrogen protective atmosphere at a temperature of 500-650° C. for 1-2 h.

[0024] As a preferred solution for the preparation method of the high-strength and high-thermal-conductivity CuAgYSi alloy material for the heat spreader, the aging treatment in step S40c is carried out under a nitrogen protective atmosphere at a temperature of 450-650° C. for 1-2 hours.

[0025] As a preferred solution for the preparation method of the high-strength and high-thermal-conductivity CuAgYSi alloy material for the heat spreader, the aging treatment in step S40d is carried out under a nitrogen protective atmosphere at a temperature of 420-480°C for 1-2 hours.

[0026] As a preferred solution of the method for preparing the high-strength and high-thermal-conductivity CuAgYSi alloy material for the heat spreader, in step S40e, the annealing temperature is 950-980°C and the time is 4-8h.

[0027] Beneficial effects of the present invention:

[0028] 1) The CuAgYSi alloy material of the present invention contains Ag, Y, and Si elements in a specific ratio, which can form an AgYSi fiber phase. The combined addition of rare earth Y and Si is more conducive to the precipitation of the Ag phase in the CuAgYSi alloy material on the basis of further degassing and deoxidation of the purified alloy melt.

[0029] 2) The CuAgYSi alloy material prepared by the present invention has high tensile strength, elongation and thermal conductivity.

[0030] 3) The preparation method of the present invention is simple, has low equipment requirements, and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a photo of the as-cast structure of the copper alloy ingot described in Example 1 of the present invention. DETAILED DESCRIPTION

[0032] The technical solution of the present invention is further illustrated below through specific implementation methods.

[0033] Unless otherwise specified, various raw materials of the present invention can be purchased commercially or prepared according to conventional methods in the art.

[0034] Example 1

[0035] The preparation method of the high-strength and high-thermal-conductivity CuAgYSi alloy material for the heat spreader of this embodiment is as follows:

[0036] Electrolytic copper is mixed with pure silver, pure silicon, and pure yttrium in the following proportions: Ag: 2.0wt%, Si: 0.3wt%, Y: 0.3wt%, and the balance is Cu. Electrolytic copper and silver are heated and melted in a graphite crucible using an induction furnace, silicon is added, and finally the rare earth element yttrium is added. Under a nitrogen protective atmosphere, the mixture is fully stirred and then slag is removed again to obtain a pure melt. The furnace temperature is controlled at 1450-1500°C. The molten copper alloy is cooled to 1250°C and then cast to obtain a copper alloy ingot. The cast structure photo of the copper alloy ingot is shown in FIG. Figure 1 shown.

[0037] The copper alloy ingot was homogenized and annealed at 950℃ for 8h in a protective atmosphere; the homogenized ingot was cold-worked and deformed by 80% deformation; the alloy was aged at 600℃ for 1h in a nitrogen protective atmosphere; and then cold-deformed by 80% deformation. Then, the aging treatment was carried out in a nitrogen protective atmosphere at a temperature of 500℃ for 2h; the aged alloy was cold-deformed by 50% deformation again, and then a three-level aging treatment was carried out in a nitrogen protective atmosphere at a temperature of 450℃ for 2h; the aged plate was cold-worked by 50% deformation again, and finally annealed at 300℃ for 4h to obtain the CuAgYSi alloy material.

[0038] Example 2

[0039] Electrolytic copper is mixed with pure silver, pure silicon and pure yttrium in the proportion of Ag: 5.0wt%, Si: 0.4wt%, Y: 0.4wt% and the balance is Cu. Electrolytic copper and silver are heated and melted in a graphite crucible using an induction furnace, silicon is added, and finally rare earth element yttrium is added. Under a nitrogen protective atmosphere, the mixture is fully stirred and then slag is removed again to obtain a pure melt, and the furnace temperature is controlled at 1450-1500°C. The molten copper alloy is cast when the temperature is cooled to 1250°C.

[0040] The copper alloy ingot was homogenized and annealed at 950℃ for 8h in a nitrogen protective atmosphere; the homogenized ingot was cold deformed with 80% deformation; the alloy was aged at 600℃ for 1h in a nitrogen protective atmosphere; and then cold deformed with 80% deformation. Then, the aging treatment was carried out in a nitrogen protective atmosphere at a temperature of 500℃ for 2h; the aged alloy was cold deformed again with 50% deformation, and then a three-level aging treatment was carried out in a nitrogen protective atmosphere at a temperature of 450℃ for 2h; the aged plate was cold deformed again with 50% deformation, and finally annealed at 300℃ for 4h to obtain the CuAgYSi alloy material.

[0041] Example 3

[0042] Electrolytic copper is mixed with pure silver, pure silicon and pure yttrium in the proportion of Ag: 3.0wt%, Si: 0.25wt%, Y: 0.25wt%, and the balance is Cu. Electrolytic copper and silver are heated and melted in a graphite crucible using an induction furnace, silicon is added, and finally rare earth element yttrium is added. Under a nitrogen protective atmosphere, the slag is skimmed again after sufficient stirring to obtain a pure melt, and the furnace temperature is controlled at 1450-1500°C. The molten copper alloy is cast when the temperature is cooled to 1250°C.

[0043] The copper alloy ingot was homogenized and annealed at 950℃ for 8h in a nitrogen protective atmosphere; the homogenized ingot was cold-worked and deformed by 80% deformation; the alloy was aged at 600℃ for 1h in a nitrogen protective atmosphere; and then cold-deformed by 80% deformation. Then, the aging treatment was carried out in a nitrogen protective atmosphere at a temperature of 500℃ for 2h; the aged alloy was cold-deformed by 50% deformation again, and then a three-level aging treatment was carried out in a protective atmosphere at a temperature of 450℃ for 2h; the aged plate was cold-worked by 50% deformation again, and finally annealed at 300℃ for 4h to obtain the CuAgYSi alloy material.

[0044] Comparative Example 1

[0045] Electrolytic copper is mixed with pure silver, pure silicon and pure lanthanum according to the ratio of Ag: 2.0wt%, Si: 0.3wt%, La: 0.3wt% and the balance is Cu. Electrolytic copper and silver are heated and melted in a graphite crucible using an induction furnace, silicon is added, and finally rare earth element lanthanum is added. Under a nitrogen protective atmosphere, the mixture is fully stirred and then slag is removed again to obtain a pure melt, and the furnace temperature is controlled at 1450-1500°C. The molten copper alloy is cast when the temperature is cooled to 1250°C.

[0046] The copper alloy ingot was homogenized and annealed at 950℃ for 8h in a nitrogen protective atmosphere; the homogenized ingot was cold-worked and deformed by 80% deformation; the alloy was aged at 600℃ for 1h in a nitrogen protective atmosphere; and then cold-deformed by 80% deformation. Then, the aging treatment was carried out in a nitrogen protective atmosphere at a temperature of 500℃ for 2h; the aged alloy was cold-deformed by 50% deformation again, and then a three-level aging treatment was carried out in a nitrogen protective atmosphere at a temperature of 450℃ for 2h; the aged plate was cold-worked by 50% deformation again, and finally annealed at 300℃ for 4h to obtain the CuAgLaSi alloy material.

[0047] Comparative Example 2

[0048] Electrolytic copper is mixed with pure silver, pure silicon and pure cerium in the proportion of Ag: 2.0wt%, Si: 0.3wt%, Ce: 0.3wt% and the balance is Cu. Electrolytic copper and pure Ag are heated and melted in a graphite crucible using an induction furnace, silicon is added, and finally rare earth element cerium is added. Under a nitrogen protective atmosphere, the mixture is fully stirred and then slag is removed again to obtain a pure melt, and the furnace temperature is controlled at 1450-1500°C. The molten copper alloy is cast when the temperature is cooled to 1250°C.

[0049] The copper alloy ingot was homogenized and annealed at 950℃ for 8h in a nitrogen protective atmosphere; the homogenized ingot was cold-worked and deformed by 80% deformation; the alloy was aged at 600℃ for 1h in a nitrogen protective atmosphere; and then cold-deformed by 80% deformation. Then, the aging treatment was carried out in a nitrogen protective atmosphere at a temperature of 500℃ for 2h; the aged alloy was cold-deformed by 50% deformation again, and then a three-level aging treatment was carried out in a nitrogen protective atmosphere at a temperature of 450℃ for 2h; the aged plate was cold-worked again by 50% deformation, and finally annealed at 300℃ for 4h to obtain the CuAgCeSi alloy material.

[0050] Comparative Example 3

[0051] Electrolytic copper is mixed with pure nickel, pure zinc and pure phosphorus according to the ratio of Ni: 5.0wt%, P: 0.4wt%, Zn: 0.4wt%, and the balance is Cu. Electrolytic copper and pure nickel are heated and melted in a graphite crucible using an induction furnace, zinc is added, and finally pure phosphorus is added. Under a nitrogen protective atmosphere, the slag is skimmed again after sufficient stirring to obtain a pure melt, and the furnace temperature is controlled at 1450-1500°C. The molten copper alloy is cast when the temperature is cooled to 1250°C.

[0052] The copper alloy ingot was homogenized and annealed at 950℃ for 8h in a nitrogen protective atmosphere; the homogenized ingot was cold deformed with 80% deformation; the alloy was aged at 600℃ for 1h in a nitrogen protective atmosphere; and then cold deformed with 80% deformation. Then, the aging treatment was carried out in a nitrogen protective atmosphere at a temperature of 500℃ for 2h; the aged alloy was cold deformed again with 50% deformation, and then a three-level aging treatment was carried out in a nitrogen protective atmosphere at a temperature of 450℃ for 2h; the aged plate was cold deformed again with 50% deformation, and finally annealed at 300℃ for 4h to obtain the CuNiPZn alloy material.

[0053] The tensile strength and elongation of the copper alloy materials of the above-mentioned embodiments 1-3 and comparative examples 1-3 were tested in accordance with "GB / T228.1-2010 Tensile test of metal materials Part 1: Room temperature test method"; the thermal conductivity of the copper alloy materials of the above-mentioned embodiments 1-3 and comparative examples 1-3 was tested in accordance with "GB / T3651-2008 Measurement method of high temperature thermal conductivity of metals", and the test results are shown in Table 1.

[0054] Table 1. Test results of tensile strength, elongation and thermal conductivity of copper alloy materials

[0055] Test Parameters Tensile strength / MPa Elongation / % Thermal conductivity / W / (m·K) Example 1 563 9.3 308 Example 2 727 7.1 385 Example 3 592 6.8 342 Comparative Example 1 445 4.8 285 Comparative Example 2 424 5.2 293 Comparative Example 3 519 8.5 255

[0056] It can be seen from Table 1 that the CuAgYSi copper alloy material prepared by the method of this embodiment can have relatively high tensile strength, elongation and thermal conductivity.

[0057] The above embodiments are only used to illustrate the detailed methods of the present invention. The present invention is not limited to the above detailed methods, that is, it does not mean that the present invention must rely on the above detailed methods to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A high-strength and high-thermal-conductivity CuAgYSi alloy material for a heat spreader, characterized in that: The invention is composed of the following raw materials by mass fraction: Ag, 1.0-5.0wt%; Y, 0.2-0.4wt%; Si, 0.2-0.4wt%; and the balance is Cu.

2. A method for preparing the high-strength and high-thermal-conductivity CuAgYSi alloy material for a heat spreader according to claim 1, characterized in that: The following steps are involved: S10, mixing Ag, Y, Si, and Cu according to mass fractions and performing smelting treatment to obtain a molten copper alloy; S20, casting the molten copper alloy to obtain a copper alloy ingot; S30, performing homogenization annealing treatment on the copper alloy ingot; S40, performing cold working deformation treatment on the copper alloy ingot after homogenization annealing treatment, and then performing multiple aging treatments and multiple cold working deformation treatments alternately to obtain a CuAgYSi alloy material.

3. The method for preparing the high-strength and high-thermal-conductivity CuAgYSi alloy material for a heat spreader according to claim 2, characterized in that: In step S10, Ag, Y, and Si are added in the form of pure elements, and Cu is added in the form of electrolytic copper.

4. The method for preparing the high-strength and high-thermal-conductivity CuAgYSi alloy material for a vapor chamber according to claim 3, characterized in that: Step S10 is specifically as follows: firstly, Cu and Ag are mixed, heated and melted, and then Si and Y are added in sequence. After being fully stirred under the protection of inert gas, the slag is skimmed to obtain a pure melt, and the furnace temperature is controlled to be 1450-1500° C., and a molten copper alloy is obtained after melting.

5. The method for preparing the high-strength and high-thermal-conductivity CuAgYSi alloy material for a vapor chamber according to claim 2, characterized in that: In step S20, the casting temperature is 1250-1350°C.

6. The method for preparing the high-strength and high-thermal-conductivity CuAgYSi alloy material for a vapor chamber according to claim 2, characterized in that: Step S30 specifically includes: subjecting the copper alloy ingot to homogenization annealing treatment in a nitrogen atmosphere at a temperature of 950-980° C. for 4-8 hours.

7. The method for preparing the high-strength and high-thermal-conductivity CuAgYSi alloy material for a heat spreader according to claim 2, characterized in that: Step S40 specifically includes the following steps: S40a, subjecting the homogenized copper alloy ingot to cold working deformation treatment, so that the deformation amount is greater than 75%; S40b, performing aging treatment and cold working deformation treatment on the copper alloy treated in step S40a in sequence, so that the deformation amount is greater than 75%; S40c, performing aging treatment and cold working deformation treatment on the copper alloy treated in step S40b in sequence, so that the deformation amount is greater than 60%; S40d, performing three-level aging and cold working deformation treatments on the copper alloy treated in step S40c in sequence, so that the deformation amount is 50%; S40e, annealing the copper alloy treated in step S40d to obtain a CuAgYSi alloy material.

8. The method for preparing the high-strength and high-thermal-conductivity CuAgYSi alloy material for a heat spreader according to claim 7, characterized in that: The aging treatment in step S40b is carried out under a nitrogen protective atmosphere at a temperature of 500-650° C. for a time of 1-2 h.

9. The method for preparing the high-strength and high-thermal-conductivity CuAgYSi alloy material for a vapor chamber according to claim 7, characterized in that: The aging treatment in step S40c is carried out under a nitrogen protective atmosphere at a temperature of 450-650° C. for a time of 1-2 h.

10. The method for preparing the high-strength and high-thermal-conductivity CuAgYSi alloy material for a vapor chamber according to claim 7, characterized in that: The aging treatment in step S40d is carried out under a nitrogen protective atmosphere at a temperature of 420-480°C for a time of 1-2 hours.