Beryllium-nickel alloy and preparation method thereof
Through suspension smelting technology and argon protection, the component segregation problem in Be-Ni alloy preparation is solved, the purity and performance of the alloy are improved, and the high-temperature and high-elastic alloy needs of aerospace devices are met.
Patent Information
- Application Number
- CN202411133285.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the existing Be-Ni alloy preparation methods, vacuum smelting technology cannot achieve uniform mixing of metal melts at high temperatures, resulting in serious segregation of alloy components, limiting the improvement of alloy performance. There are few domestic manufacturers, and the performance is unstable and cannot be met. Industry demand.
The suspension smelting technology is adopted to control the heating power and time to make the beryllium nickel raw material fully melt and roll evenly under the action of a magnetic field. After vacuuming, argon is added as a protective gas to reduce the oxygen content to improve the purity of the alloy.
The preparation of beryllium nickel alloy without segregation is achieved, which improves the purity and performance of the alloy and enhances its applicability in high-temperature and high-elastic applications.
Smart Images

Figure CN118932216A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of beryllium nickel alloy preparation, and in particular relates to a non-segregation beryllium nickel alloy and a preparation method thereof. Background Art
[0002] Due to its excellent electrical conductivity, high temperature resistance and elasticity, Be-Ni alloy is mainly used in aviation thermal springs, aircraft instrument mold boxes, altimeters and high temperature relays. Compared with traditional Be-Cu alloy, Be-Ni alloy can break through the temperature limit of 150℃ for Be-Cu alloy conductive components, and is more in line with the application requirements of high temperature and high elasticity alloys used in aerospace devices.
[0003] At present, there are few domestic Be-Ni alloy manufacturers, and the performance of the wires and strips they produce is extremely unstable and cannot stably meet industry demand.
[0004] The commonly used preparation method for Be-Ni alloy is vacuum melting, but the vacuum melting technology cannot effectively achieve uniform mixing of the metal melt at high temperature. During the cooling process, a phase interface is easily formed between the beryllium phase and the nickel phase, which reduces the degree of uniformity of the alloy composition and causes severe segregation during the alloy melting process. This reduces the strength and hardness of the Be-Ni alloy, limits the performance improvement of the alloy, and greatly reduces the alloy yield.
[0005] Therefore, the existing technology needs to be improved. Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides a beryllium nickel alloy without segregation and a preparation method thereof. Based on the suspension smelting technology, the beryllium nickel raw material is fully melted under the action of the magnetic field and then continuously tumbled evenly by controlling the heating power and time during suspension smelting to reduce segregation. At the same time, argon is added as a protective gas after vacuuming to reduce the oxygen content in the alloy, thereby improving the purity of the beryllium nickel alloy.
[0007] The first aspect of the present invention provides a method for preparing a beryllium-nickel alloy, wherein the mass percentage of nickel in the beryllium-nickel alloy is 98% and the balance is beryllium; the preparation method is based on suspension smelting technology and comprises the following steps:
[0008] Step S1, preparation stage, placing beryllium raw material and nickel raw material into a crucible in the order of beryllium at the bottom layer and nickel at the top layer, and evacuating to 1×10 -3 ~5×10 -3 After Pa, argon gas is filled to the preset pressure;
[0009] Step S2, in the smelting stage, the heating power increase rate of the suspension smelting is set to 20-40 kW / min, and the power is gradually increased until the beryllium raw material and the nickel raw material are completely melted, and the target power is maintained for 5-10 minutes, and then the power is reduced to 0 kW within 20-30 seconds to obtain a beryllium-nickel alloy melt;
[0010] Step S3, a cooling stage, naturally cooling the beryllium-nickel alloy melt in the crucible to room temperature to obtain a beryllium-nickel alloy ingot.
[0011] According to the method for preparing beryllium nickel alloy according to the first aspect of the present invention, in step S1, argon gas is filled into the furnace until the pressure in the furnace is 2×10 -2 ~8×10 -2 Pa.
[0012] According to the method for preparing beryllium nickel alloy described in the first aspect of the present invention, in the step S2, the target power is 150-160 kw.
[0013] According to the method for preparing beryllium nickel alloy described in the first aspect of the present invention, in the step S3, the natural cooling time is 20 to 40 minutes.
[0014] According to the method for preparing beryllium nickel alloy described in the first aspect of the present invention, the crucible is a copper crucible.
[0015] According to the method for preparing beryllium-nickel alloy described in the first aspect of the present invention, the beryllium raw material is 3N grade metallic beryllium, and the nickel raw material is 4N grade metallic nickel.
[0016] A second aspect of the present invention provides a beryllium-nickel alloy prepared by the aforementioned method for preparing the beryllium-nickel alloy.
[0017] The solution proposed by the present invention has the following technical effects:
[0018] The present invention is based on suspension smelting technology. By controlling the heating power and time during suspension smelting, the beryllium nickel raw material is fully melted under the action of a magnetic field and then continuously tumbled evenly to reduce segregation. At the same time, argon is added as a protective gas after vacuuming to reduce the oxygen content in the alloy, thereby improving the purity of the beryllium nickel alloy.
[0019] In addition, the nickel-beryllium raw materials will experience skin effect on the surface of the material in this uneven and rapidly changing magnetic field, generating eddy currents, which will in turn generate a magnetic field in the opposite direction of the coil magnetic field. When the magnetic field force is greater than the gravity of the raw materials, the melt can be suspended to reduce material contamination caused by contact between the melt and the inner wall of the crucible, further improving the purity of the beryllium-nickel alloy. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0021] Figure 1 This is a SEM characterization picture of the beryllium nickel alloy obtained in specific example 1 of the present invention.
[0022] Figure 2 This is a line scan composition characterization diagram of the beryllium nickel alloy obtained in specific example 1 of the present invention. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] In a first aspect of this embodiment, a method for preparing a beryllium-nickel alloy is provided, wherein the mass percentage of nickel in the beryllium-nickel alloy is 98% and the balance is beryllium. The preparation method is based on suspension smelting technology and comprises the following steps:
[0025] Step S1, preparation stage, placing beryllium raw material and nickel raw material into a crucible in the order of beryllium at the bottom layer and nickel at the top layer, and evacuating to 1×10 -3 ~5×10 -3 Pa and then filled with argon to the preset pressure.
[0026] Step S2, smelting stage, setting the heating power increase rate of suspension smelting to 20-40 kW / min, gradually increasing the power until the beryllium raw material and the nickel raw material are completely melted, maintaining the target power for 5-10 minutes, and then reducing the power to 0 kW within 20-30 seconds to obtain a beryllium nickel alloy melt.
[0027] Step S3, a cooling stage, naturally cooling the beryllium-nickel alloy melt in the crucible to room temperature to obtain a beryllium-nickel alloy ingot.
[0028] In step S1, in the preparation stage, beryllium raw materials and nickel raw materials are placed in a crucible in the order of beryllium at the bottom and nickel at the top, and the crucible is evacuated to 1×10 -3 ~5×10 -3 Pa and then filled with argon to the preset pressure.
[0029] In some embodiments, in step S1, argon gas is charged to a pressure of 2×10 -2 ~8×10 -2 Pa.
[0030] In this embodiment, the introduction of argon gas after evacuation can further reduce the amount of oxidation and improve the purity of the beryllium nickel alloy.
[0031] In some embodiments, the crucible is a copper crucible.
[0032] In some embodiments, the beryllium raw material is 3N grade metallic beryllium, and the nickel raw material is 4N grade metallic nickel.
[0033] In step S2, the smelting stage, the heating power increase rate of the suspension smelting is set to 20-40 kw / min, and the power is gradually increased until the beryllium raw material and the nickel raw material are completely melted, and the target power is maintained for 5-10 minutes, and then the power is reduced to 0 kw within 20-30 seconds to obtain a beryllium nickel alloy melt.
[0034] In some embodiments, in step S2, the target power is 150-160 kw.
[0035] In this embodiment, the coil current increases continuously during the power increase process, the magnetic field strength generated by the coil increases accordingly, and the heat generated by the skin effect on the metal surface also increases accordingly, causing the beryllium raw material and the nickel raw material to continue to melt. At the same time, due to the different Ampere forces on different parts of the molten metal under the action of the magnetic field, the molten metal continues to roll in the crucible, making the two metals more evenly mixed, thereby reducing the component segregation of the beryllium nickel alloy.
[0036] In step S3, the cooling stage, the beryllium-nickel alloy melt is naturally cooled to room temperature in the crucible to obtain a beryllium-nickel alloy ingot.
[0037] In some embodiments, in step S3, the natural cooling time is 20 to 40 minutes.
[0038] A second aspect of the present embodiment provides a beryllium-nickel alloy prepared by the aforementioned method for preparing the beryllium-nickel alloy.
[0039] Example 1
[0040] In the first step, 27 g of 3N grade beryllium and 1324.8 g of 4N grade nickel were placed in a copper crucible in the order of beryllium at the bottom and nickel at the top, and the crucible was evacuated to 3.2 × 10 -3 Pa, and then argon gas was filled into the furnace until the pressure inside the furnace reached 3.1×10 -2 Pa;
[0041] In the second step, the heating power increase rate of the suspension smelting is set to 30kw / min, and the power is gradually increased. The material in the copper crucible gradually begins to melt as the heating power increases; after 4 minutes, the heating power reaches 120kw, at which time most of the raw materials have melted, and only a small amount of block raw materials remain unmelted; the power is continued to be increased to 150kw, at which time the beryllium raw material and the nickel raw material are completely melted, and the power of 150kw is maintained for 10 minutes to make the beryllium nickel metal melt continue to roll and be fully mixed; then the power is reduced to 0kw within 20 to 30 seconds to obtain a beryllium nickel alloy melt;
[0042] The third step is to cool the beryllium nickel alloy melt to room temperature in a copper crucible to obtain a beryllium nickel alloy ingot, wherein the cooling time is about 20 minutes.
[0043] In order to determine the internal microstructure state of the beryllium nickel alloy prepared in Example 1, a SEM test was performed on the internal structure of the beryllium nickel alloy. Figure 1 As shown. Through SEM characterization, it was found that in the beryllium nickel alloy, the Be element is evenly distributed in the Ni element, and there is no segregation site, and the overall composition uniformity of the alloy is high.
[0044] To further determine the internal chemical composition of the alloy, the beryllium nickel alloy prepared in Example 1 was subjected to line scanning, and the alloy composition changes were as follows: Figure 2 As shown in Figure 2, it is found through line scanning that the Ni and Be elements always change evenly with the displacement.
[0045] Example 2
[0046] In the first step, 31.2 g of 3N grade beryllium and 1529.3 g of 4N grade nickel were placed in a copper crucible in the order of beryllium at the bottom and nickel at the top, and the crucible was evacuated to 1.6 × 10 -3 Pa, argon gas was filled into the furnace until the pressure inside the furnace reached 4.2×10 -2 Pa;
[0047] In the second step, the heating power increase rate of the suspension smelting is set to 25kw / min, and the power is gradually increased. The material in the copper crucible gradually begins to melt as the heating power increases; after 5 minutes, the heating power reaches 125kw, at which time most of the raw materials have melted, and only a small amount of block raw materials remain unmelted; the power is continued to be increased to 155kw, at which time the beryllium raw material and the nickel raw material are completely melted, and the power of 155kw is maintained for 8 minutes to make the beryllium nickel metal melt continue to roll and be fully mixed; then the power is reduced to 0kw within 20 to 30 seconds to obtain a beryllium nickel alloy melt;
[0048] The third step is to cool the beryllium nickel alloy melt to room temperature in a copper crucible to obtain a beryllium nickel alloy ingot, wherein the cooling time is about 40 minutes.
[0049] Example 3
[0050] In the first step, 40 g of 3N grade beryllium and 1960 g of 4N grade nickel were placed in a copper crucible in the order of beryllium at the bottom and nickel at the top, and the crucible was evacuated to 4.8 × 10 -3 Pa, and then argon gas was filled into the furnace until the pressure inside the furnace reached 5.5×10 -2 Pa;
[0051] In the second step, the heating power increase rate of the suspension smelting is set to 40kw / min, and the power is gradually increased. The material in the copper crucible gradually begins to melt as the heating power increases; after 3 minutes, the heating power reaches 120kw, at which time most of the raw materials have melted, and only a small amount of block raw materials remain unmelted; the power is continued to be increased to 160kw, at which time the beryllium raw material and the nickel raw material are completely melted, and the power of 160kw is maintained for 5 minutes to make the beryllium nickel metal melt continue to roll and be fully mixed; then the power is reduced to 0kw within 20 to 30 seconds to obtain a beryllium nickel alloy melt;
[0052] The third step is to cool the beryllium nickel alloy melt naturally to room temperature in a copper crucible to obtain a beryllium nickel alloy ingot, wherein the cooling time is about 30 minutes.
[0053] In summary, the solution proposed by the present invention has the following technical effects:
[0054] The present invention is based on suspension smelting technology. By controlling the heating power and time during suspension smelting, the beryllium nickel raw material is fully melted under the action of a magnetic field and then continuously tumbled evenly to reduce segregation. At the same time, argon is added as a protective gas after vacuuming to reduce the oxygen content in the alloy, thereby improving the purity of the beryllium nickel alloy.
[0055] In addition, the nickel-beryllium raw materials will experience skin effect on the surface of the material in this uneven and rapidly changing magnetic field, generating eddy currents, which will in turn generate a magnetic field in the opposite direction of the coil magnetic field. When the magnetic field force is greater than the gravity of the raw materials, the melt can be suspended to reduce material contamination caused by contact between the melt and the inner wall of the crucible, further improving the purity of the beryllium-nickel alloy.
[0056] Please note that the technical features of the above embodiments can be combined arbitrarily. In order to make the description concise, all possible combinations of the technical features in the above embodiments are not described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. The above embodiments only express several implementation methods of the present application, and their descriptions are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present application, several variations and improvements can be made, which all belong to the scope of protection of the present application. Therefore, the scope of protection of the patent in this application shall be based on the attached claims.
Claims
1. A method for preparing a beryllium nickel alloy, It is characterized in that The mass percentage of nickel in the beryllium-nickel alloy is 98%, and the balance is beryllium; the preparation method is based on suspension smelting technology and includes the following steps: Step S1, preparation stage, placing beryllium raw material and nickel raw material into a crucible in the order of beryllium at the bottom layer and nickel at the top layer, and evacuating to 1×10 -3 ~5×10 -3 After Pa, argon gas is filled to the preset pressure; Step S2, in the smelting stage, the heating power increase rate of the suspension smelting is set to 20-40 kW / min, and the power is gradually increased until the beryllium raw material and the nickel raw material are completely melted, and the target power is maintained for 5-10 minutes, and then the power is reduced to 0 kW within 20-30 seconds to obtain a beryllium-nickel alloy melt; Step S3, a cooling stage, naturally cooling the beryllium-nickel alloy melt in the crucible to room temperature to obtain a beryllium-nickel alloy ingot.
2. The method for preparing beryllium nickel alloy according to claim 1, It is characterized in that In step S1, argon gas is charged into the furnace until the pressure in the furnace is 2×10 -2 ~8×10 -2 Pa.
3. The method for preparing beryllium nickel alloy according to claim 1, It is characterized in that In the step S2, the target power is 150-160kw.
4. The method for preparing beryllium nickel alloy according to claim 1, It is characterized in that In step S3, the natural cooling time is 30 to 40 minutes.
5. The method for preparing beryllium nickel alloy according to claim 1, It is characterized in that The crucible is a copper crucible.
6. The method for preparing beryllium nickel alloy according to claim 1, It is characterized in that The beryllium raw material is 3N grade metallic beryllium, and the nickel raw material is 4N grade metallic nickel.
7. A beryllium-nickel alloy prepared by the method for preparing a beryllium-nickel alloy according to any one of claims 1 to 6.