Additive manufacturing cobalt-based high-temperature alloy and preparation method thereof

By using cobalt-based high-temperature alloys with specific component ratios in additive manufacturing, combined with laser cladding deposition and heat treatment technology, the problems of cracks and holes of cobalt-based high-temperature alloys during processing are solved, and high γ' phase content and Cobalt-based high-temperature alloys with low crack sensitivity significantly improve their high-temperature performance and printability.

CN118932218APending Publication Date: 2024-11-12INST OF METAL RESEARCH - CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310530675.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing additively manufactured cobalt-based high-temperature alloys are prone to cracks and holes during processing, and the γ' phase content and crack sensitivity are difficult to harmonize, resulting in low high-temperature performance, limiting its application in hot-end components such as turbines.

Method used

Using cobalt-based high-temperature alloys with specific component ratios, including C, B, Hf, Zr, Al, Ta, W, Cr, Ni and Co, the volume content of γ' phase reaches more than 70%. It is printed and carried out through laser cladding deposition process. Solid solution and aging heat treatment to optimize microstructure and mechanical properties.

Benefits of technology

Cobalt-based high-temperature alloys with high γ' phase content, low crack sensitivity and high mechanical properties have achieved, which significantly improves their high-temperature performance and printability, and is better than the comprehensive performance of existing nickel-based and cobalt-nickel-based high-temperature alloys.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932218A_ABST
    Figure CN118932218A_ABST
Patent Text Reader

Abstract

The invention provides an additive manufacturing cobalt-based high-temperature alloy and a preparation method thereof. The additive manufacturing cobalt-based high-temperature alloy is prepared from the following raw materials in percentage by weight: 0.05 to 0.2 percent of C, 0.01 to 0.05 percent of B, 0.5 to 2.0 percent of Hf, 0.01 to 0.1 percent of Zr, 3.0 to 6.0 percent of Al, 6.0 to 10.0 percent of Ta, 10.0 to 16.0 percent of W, 4.0 to 7.0 percent of Cr, 15.0 to 25.0 percent of Ni and the balance of Co. According to the additive manufacturing cobalt-based high-temperature alloy and the preparation method thereof, the volume percentage content of the gamma'phase of a sedimentary sample is as high as 70%, the crack sensitivity is low, the structure stability is good, the mechanical property is excellent, and the tensile property is superior to that of SBCoNi10. After a sedimentary sample is subjected to heat treatment, the durability at 1000 DEG C / 120 MPa is further improved to 240 h or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of additively manufactured cobalt-based high-temperature alloys, and specifically to an additively manufactured cobalt-based high-temperature alloy and a preparation method thereof. Background Art

[0002] Additive manufacturing has attracted the attention of a large number of scholars with its advantages of high precision, high design freedom and high utilization rate, especially in the preparation of complex structural parts such as turbine blades. However, due to the influence of cyclic heating and cooling during the processing, internal stress is accumulated during the forming process, which easily forms defects such as cracks and holes. Printability has become the primary factor hindering the promotion and application of additive manufacturing metal materials.

[0003] In the late stage of solidification of additively manufactured high-temperature alloys, the γ' phase precipitates rapidly, hindering the relaxation of thermal stress and leading to thermal cracks. The irreconcilable contradiction between the γ' content and crack sensitivity means that the γ' content in the high-temperature alloys currently available for additive manufacturing does not exceed 50%, resulting in low high-temperature performance, which seriously limits its application in hot end components such as turbine disks.

[0004] Co-Al-W alloys have a γ' / γ two-phase microstructure similar to that of nickel-based alloys. According to the research on traditional cobalt-based superalloys in recent years, cobalt-based superalloys have good welding performance compared with nickel-based alloys, which means that they have lower crack sensitivity than nickel-based alloys. At present, the research on γ'-strengthened cobalt-based superalloys in the field of additive manufacturing is still in its infancy.

[0005] Therefore, how to provide an additively manufactured cobalt-based high-temperature alloy with high γ' phase content, low crack sensitivity, and high mechanical properties and a preparation method thereof has become an urgent problem that technicians in this field need to solve. Summary of the invention

[0006] Therefore, the technical problem to be solved by the present application is to provide an additively manufactured cobalt-based high-temperature alloy and a preparation method thereof, which has good high-temperature performance.

[0007] In order to solve the above problems, the present application provides an additive manufacturing cobalt-based high-temperature alloy, comprising the following raw materials in weight percentage:

[0008] C 0.05-0.2%, B 0.01-0.05%, Hf 0.5-2.0%, Zr 0.01-0.1%, Al 3.0-6.0%, Ta6.0-10.0%, W 10.0-16.0%, Cr 4.0-7.0%, Ni 15.0-25.0%, balance Co.

[0009] Furthermore, in the cobalt-based alloy, the volume percentage of the γ' phase is greater than 70%.

[0010] Furthermore, in the Co-based alloy, the size of the γ' phase is 50-100 nm.

[0011] Furthermore, the room temperature tensile strength of the cobalt-based alloy is above 1300 MPa.

[0012] Further, cobalt-based alloys are used in additive manufacturing.

[0013] According to another aspect of the present application, there is provided a method for preparing the above-mentioned cobalt-based alloy, comprising the following steps:

[0014] Step (1): weighing the raw materials as mentioned above to prepare an alloy ingot; using the raw materials to perform laser cladding deposition printing; and obtaining an alloy.

[0015] Further, the following steps are included: during the laser cladding deposition process printing, the laser power is 1100-

[0016] 1700W, scanning speed 600-1300mm / min, powder feeding amount 5-11g / min, spot diameter 2-3mm.

[0017] Furthermore, the method for preparing the cobalt-based high-temperature alloy by additive manufacturing further includes the following steps:

[0018] Step (2): performing subsequent heat treatment on the alloy obtained in step (1).

[0019] Further, the heat treatment comprises the following steps:

[0020] Step S1: solution treatment; further, the solution treatment includes: first, keeping warm at 1240-1300°C for 1-5h; then keeping warm at 1260-1310°C for 1-5h, and then cooling to room temperature.

[0021] Further, the heat treatment comprises the following steps:

[0022] Step S2: performing a first aging treatment on the alloy after the solution treatment in step S1; further, the first aging treatment includes: keeping warm at 800-1200°C for 26-50h, and then cooling to room temperature.

[0023] Further, the heat treatment comprises the following steps:

[0024] Step S3: performing a second aging treatment on the alloy after the first aging treatment in step S2; further, the second aging treatment includes: keeping at 600-800° C. for 15-35 hours, and then cooling to room temperature.

[0025] The cobalt-based alloy and preparation method provided by the present application. The present application has good high-temperature performance. The γ' phase content of the additively manufactured cobalt-based high-temperature alloy of the present application is as high as 70% or more, which is much higher than the current typical additively manufactured high-temperature alloys, and has good printability and low crack sensitivity. Compared with typical additively manufactured nickel-based, cobalt-based, and cobalt-nickel-based high-temperature alloys, the comprehensive performance of the cobalt-based high-temperature alloy of the present application is significantly excellent. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The microstructures of the additively manufactured cobalt-based high-temperature alloy in the deposited state (a, b) and after deposition + heat treatment (c, d) of Example 1;

[0027] Figure 2 Comparison of room temperature and high temperature tensile properties of the additively manufactured cobalt-based high-temperature alloys of Example 1 and Example 2 with those of typical alloys in the prior art;

[0028] Figure 3 The Larson-Miller curves of the additively manufactured cobalt-based high-temperature alloy after deposition and heat treatment of Example 1 are compared with those of the typical alloy in the prior art;

[0029] Figure 4 This is the deposited structure of the additively manufactured cobalt-based high-temperature alloy of Example 2. DETAILED DESCRIPTION

[0030] See also Figure 1-4 As shown, an additively manufactured cobalt-based high-temperature alloy includes the following raw materials in weight percentage:

[0031] C 0.05-0.2%, B 0.01-0.05%, Hf 0.5-2.0%, Zr 0.01-0.1%, Al 3.0-6.0%, Ta6.0-10.0%, W 10.0-16.0%, Cr 4.0-7.0%, Ni 15.0-25.0%, balance Co.

[0032] The cobalt-based alloy of the present application is an additively manufactured cobalt-based high-temperature alloy.

[0033] In the present application, a high Ta content (6.0-10.0%) and an appropriate Ni content (15.0-25.0%) are used to ensure that the additively manufactured cobalt-based high-temperature alloy has an ultra-high γ' phase volume fraction and a γ' phase morphology with excellent cubicity.

[0034] In the present application, the C content is 0.05-0.2%, the Hf content is 0.5-2.0%, and the B content is 0.01-0.05%, which can ensure carbide precipitation strengthening and grain boundary strengthening.

[0035] In this application of additive manufacturing of cobalt-based high-temperature alloys:

[0036] W is an important γ' phase forming element. The reduction of W content will lead to a decrease in the mismatch between γ' / γ phases, making the γ' phase morphology tend to be spherical. However, the increase of W content will lead to an increase in alloy density. Therefore, the W content in this alloy is controlled at 10-16%.

[0037] As the content of Ni increases, the morphology of the γ' phase changes from spherical to cubic, and the mismatch stress of the alloy also increases, which will eventually lead to an increase in yield strength, while Ni has little effect on the volume fraction of the γ' phase. By studying the effect of Ni on the segregation behavior of the Co-Al-W ternary system elements in the γ / γ' phase, it is found that with the increase of Ni content, the segregation degree of W in the γ' and γ phases gradually decreases. Therefore, the content range of Ni in this alloy is controlled in 15.0-25.0%.

[0038] Ta is a γ' phase-forming element. The addition of Ta can increase the volume fraction of the γ' phase in the alloy, and at the same time increase the mismatch between the γ' / γ phases, increase the interface mismatch stress, and part of Ta can be dissolved in the γ phase to increase the strength of the γ phase, that is, the solid solution resistance is also increased. First-principle calculations show that the addition of Ta can increase the stacking fault energy of the γ' phase. The addition of Ta can reduce the solid-liquid phase temperature of the alloy and increase the solidification temperature range. The addition of Ta to the Co-Al-W ternary system can increase the dissolution temperature of the γ' phase, but Ta can lead to an increase in the growth rate of the γ' phase in the alloy, that is, an increase in the coarsening rate of the γ' phase. Therefore, the Ta content range is set at Ta6.0-10.0%.

[0039] C is a carbide-forming element, which is concentrated at the grain boundary, strengthens the grain boundary, and is conducive to the improvement of high temperature performance. Too high C will combine with other carbide-forming elements to form large-sized irregular carbides, causing stress concentration, becoming a crack source, and reducing printability. Therefore, the C content in this alloy is 0.05-0.2%.

[0040] B is mainly added to polycrystalline alloys as a grain boundary strengthening element. B has a certain effect on improving the high-temperature oxidation resistance of cobalt-based high-temperature alloys. Adding B and Cr elements can promote the formation of a continuous Al2O3 layer on the surface of the Co-Al-W-based high-temperature alloy matrix. Similar to the C element, when the B content is too high, some large-sized hard borides will be formed during the additive manufacturing process, inducing cracking. Therefore, in this alloy, the B content is 0.01-0.05%.

[0041] Hf element can increase the dissolution temperature of γ' phase to a certain extent and stabilize γ' phase, but the negative impact is that it increases the possibility of forming Laves phase. In the alloy design, the content of Hf element is determined to be in the range of 0.5-2.0%.

[0042] Zr is usually concentrated in grain boundaries and carbides, inhibiting the diffusion of grain boundaries and playing a role in grain boundary strengthening. It is beneficial to improve creep resistance. In addition, due to its high oxygen affinity, too much Zr will combine with oxygen to form oxides with high melting point and high hardness, which will induce thermal cracks and be detrimental to printability. Therefore, the content of Zr in the alloy of this application is in the range of 0.01-0.1%.

[0043] Cr is the most effective alloying element for improving the oxidation resistance and corrosion resistance of γ' phase strengthened cobalt-based high-temperature alloys. However, the addition of Cr will also seriously reduce the γ' phase stability of the alloy and promote the precipitation of secondary phases. Therefore, the Cr content in the alloy of the present application is 4.0-7.0%.

[0044] Al can form a dense protective Al2O3 layer on the surface of the alloy matrix to improve the high-temperature oxidation resistance of the alloy. Too much Al will lead to the formation of β phase. Therefore, the Al content in the alloy of the present application is 3.0-6.0%.

[0045] The additively manufactured cobalt-based high-temperature alloy of the present application replaces part of the W element in the Co-Al-W ternary alloy by adding alloying elements such as Ni, thereby reducing the proportion of W in the alloy and thus reducing the alloy density. Secondly, grain boundary strengthening elements such as C, B, Zr, and Hf are added to strengthen the grain boundaries and improve room temperature and high temperature performance. Finally, Ta and Ni improve the high-temperature stability of the γ' phase while ensuring sufficient volume fraction as γ' phase-forming elements. In addition, the addition of Ni and Ta can increase the mismatch between the γ / γ' phases, obtain a structure with excellent cubicity, and improve high-temperature performance. The additively manufactured cobalt-based high-temperature alloy of the present application can solve the problems of high density, low dissolution temperature of the γ' phase, poor stability, and unsatisfactory high-temperature performance of traditional Co-Al-W ternary alloys.

[0046] The types of raw materials and weight proportions of the additively manufactured cobalt-based high-temperature alloy of the present application are adjusted so that the cobalt-based alloy of the present application has excellent printability. A reasonable printing process and post-processing process are adopted so that the tensile properties and durability of the alloy are better than the mature additively manufactured high-temperature alloys that have been published so far.

[0047] The additively manufactured cobalt-based high-temperature alloy of the present application has good printability and low crack sensitivity. By rationally regulating the content of Ta, W, and Al, the synergistic effect of each component obtains a γ' phase with excellent cubicity and high volume fraction. At the same time, the metallurgical bonding is good, and a crack-free block sample is obtained.

[0048] The cobalt-based alloy of the present application is an additively manufactured cobalt-based high-temperature alloy.

[0049] The present application also discloses some embodiments, in which the volume percentage of the γ′ phase in the additively manufactured cobalt-based alloy is higher than 70%.

[0050] The present application also discloses some embodiments, in which the size of the γ' phase in the additively manufactured cobalt-based alloy is 50-100 nm.

[0051] The present application also discloses some embodiments, and the room temperature tensile strength of the cobalt-based alloy of the present application is above 1300 MPa.

[0052] The present application also discloses some embodiments, wherein the cobalt-based alloy of the present application is used for additive manufacturing.

[0053] Furthermore, the cobalt-based alloy of the present application is used for turbine working blades and guide vanes.

[0054] According to another aspect of the present application, there is provided a method for preparing the above-mentioned cobalt-based alloy, comprising the following steps:

[0055] Step (1): weighing the raw materials as mentioned above to prepare an alloy ingot; using the raw materials to perform laser cladding deposition printing; and obtaining an alloy.

[0056] Specifically, in step (1): weigh the raw materials as mentioned above to prepare an alloy ingot, prepare powder by gas atomization, screen the powder with a particle size in the range of 100-325 meshes for laser cladding deposition printing, and obtain a deposited alloy.

[0057] The present application also discloses some embodiments, including the following steps: in the laser cladding deposition process printing, the laser power is 1100-1700W, the scanning speed is 600-1300mm / min, the powder feeding amount is 5-11g / min, and the spot diameter is 2-3mm. Preferably, the laser power is 1600-1700W, the scanning speed is 1100-1400mm / min, and the powder feeding amount is 10-11g / min.

[0058] After printing by laser cladding deposition process, the present invention obtains a nearly crack-free micro-columnar structure, in which the volume percentage of γ' phase is as high as 70%, the cubic degree is excellent, and the size is nanometer-level 50-100nm. The tensile performance test shows that the room temperature tensile strength of the deposited structure reaches more than 1300MPa, which is much higher than other reported deposited high-temperature alloys, and the high-temperature mechanical properties are excellent.

[0059] The laser cladding deposition process can be used to print a fine columnar structure with an orientation of

[001] , a γ' phase content of more than 70%, a size of 50-100nm, and excellent cubicity.

[0060] The present application also discloses some embodiments, wherein the method for preparing the cobalt-based alloy further comprises the following steps:

[0061] Step (2): heat treating the alloy obtained in step (1).

[0062] The present application also discloses some embodiments, wherein the heat treatment comprises the following steps:

[0063] Step S1: solution treatment; the present application also discloses some embodiments, the solution treatment comprises: firstly keeping warm at 1240-1300°C for 1-5h; then keeping warm at 1260-1310°C for 1-5h, and then cooling to room temperature.

[0064] The present application also discloses some embodiments, wherein the heat treatment comprises the following steps:

[0065] Step S2: performing a first aging treatment on the alloy after the solution treatment in step S1; the present application also discloses some embodiments, and the first aging treatment includes: keeping warm at 800-1200°C for 26-50h, and then cooling to room temperature.

[0066] The present application also discloses some embodiments, wherein the heat treatment comprises the following steps:

[0067] Step S3: performing a second aging treatment on the alloy after the first aging treatment in step S2; the present application also discloses some embodiments, and the second aging treatment includes: keeping warm at 600-800°C for 15-35h, and then cooling to room temperature.

[0068] After solution treatment and two-stage aging treatment, the 1000℃ / 120MPa endurance performance is further improved to more than 240h.

[0069] The additively manufactured cobalt-based high-temperature alloy in this application showed excellent performance in both tensile tests and endurance tests.

[0070] The tensile properties of the cobalt-based superalloy manufactured by deposition additive manufacturing in this application:

[0071] Room temperature: σ b ≥1300MPa,σ 0.2 ≥750MPa, A≥10%;

[0072] 900℃:σ b ≥630MPa,σ 0.2 ≥450MPa, A≥10%;

[0073] 1000℃:σ b ≥300MPa,σ 0.2 ≥250MPa, A≥10%;

[0074] The long-lasting properties of the cobalt-based superalloy manufactured by deposition additive manufacturing in this application:

[0075] 980℃ / 150MPa, t≥120h, A≥25%;

[0076] 980℃ / 235MPa, t≥10h, A≥25%;

[0077] 1000℃ / 120MPa, t≥130h, A≥30%;

[0078] The deposition-based additively manufactured cobalt-based high-temperature alloy of the present application has significantly improved high-temperature endurance performance after heat treatment, and the endurance life at 1000°C / 120MPa reaches more than 240h.

[0079] Tensile properties of heat-treated additively manufactured cobalt-based superalloy:

[0080] Room temperature: σ b ≥1230MPa,σ 0.2 ≥650MPa, A≥10%;

[0081] 900℃:σ b ≥720MPa,σ 0.2 ≥580MPa, A≥10%;

[0082] 1000℃:σ b ≥350MPa,σ 0.2 ≥250MPa, A≥30%;

[0083] Long-lasting properties of heat-treated additively manufactured cobalt-based high-temperature alloys:

[0084] 980℃ / 150MPa, t≥150h, A≥25%;

[0085] 980℃ / 235MPa, t≥10h, A≥30%;

[0086] 1000℃ / 120MPa, t≥240h, A≥20%.

[0087] In this application, the impact on crack sensitivity is mainly divided into three categories:

[0088] (1) Elements affecting γ' phase content and morphology:

[0089] Al, W, and Ta are γ' phase-forming elements. As the content of these elements increases, the γ' phase content increases accordingly, and the high-temperature performance improves. However, when the γ' phase content is too high, aging cracks will occur.

[0090] Ni and Ta are elements that affect the γ' phase morphology. The increase of Ta and Ni elements is conducive to obtaining a γ' phase with excellent cubicity, which will lead to an increase in the γ / γ' mismatch. This morphology is conducive to the improvement of mechanical properties, but a large mismatch will also induce aging cracks.

[0091] The present application rationally regulates these four elements, balances the contradiction between this performance and crack sensitivity, and obtains the highest possible content of γ' phase with excellent cubicity.

[0092] (2) Solid solution elements: Cr, Ni, can strengthen the γ phase matrix and reduce the tendency to crack.

[0093] (3) Carbide / boride forming elements: C, B, Hf, Ta, Zr. Carbides / borides, which are high melting point precipitation phases, are the crack source of solidification cracks; therefore, the content should be kept as low as possible. On the other hand, carbides are pinned to the grain boundaries, hindering dislocation movement and grain boundary sliding, and improving high temperature performance. These carbide / boride forming elements are indispensable. Therefore, the present application reasonably regulates the content of carbides and the size and morphology of carbides to reduce the cracking tendency and strengthen the grain boundaries.

[0094] Example

[0095] Embodiment 1:

[0096] The composition of Example 1 of the present application is shown in Table 1 below; the mechanical properties of Example 1 after being printed by laser cladding deposition process are shown in Table 2 below; the mechanical properties of Example 1 after being printed by laser cladding deposition process and then heat treated are shown in Table 3 below. Several typical alloys used for additive manufacturing in the prior art are used for comparison: cobalt-based (GH5188), cobalt-nickel-based (SBCoNi10), nickel-based (ABD-850M, CM247LC, IN738LC, Alloy1), and the specific compositions are shown in Table 1 below.

[0097] Table 1 Composition of typical additive manufacturing alloys in Example 1 and prior art

[0098]

[0099] Table 2

[0100]

[0101] Table 3

[0102]

[0103] Example 1 Alloy deposited structure as shown Figure 1 As shown in (ab). After laser cladding deposition printing, a crack-free, well-metallurgically bonded structure was obtained. Fine carbide particles were observed between dendrites, with a volume percentage of γ' phase as high as 77%, excellent cubicity, and a nanoscale size of about 50nm. After heat treatment, the size of the γ' phase grew to about 100nm, and no aging cracks were generated by the precipitation and growth of the γ' phase. It can be seen that the internal stress of the deposited structure was reasonably released.

[0104] Table 2 shows the tensile properties and rupture properties of the alloy in Example 1. The printed samples exhibit excellent mechanical properties both at room temperature and at high temperature.

[0105] Table 3 shows the tensile properties and endurance properties of the alloy after deposition and heat treatment of Example 1. Compared with the deposited state, the tensile properties are still relatively high after heat treatment, and the endurance properties are significantly improved under the conditions of 1000°C / 120MPa.

[0106] Figure 2 The room temperature tensile mechanical properties of the alloys of Example 1, Example 2, and Example 3 as deposited are compared with the typical additive manufacturing high temperature alloys of the prior art. The mechanical properties are significantly better than those of typical additive manufacturing high temperature alloys such as IN738 (nickel-based), GH5188 (cobalt-based), and SBCoNi10 (cobalt-nickel-based).

[0107] Figure 3 The durability performance of the heat-treated Example 1 alloy is compared with several typical additively manufactured nickel-based high-temperature alloys in the prior art. Similarly, the Example 1 alloy of the present application also shows obvious performance advantages.

[0108] Embodiment 2:

[0109] The composition of Example 2 is shown in Table 4 below; the mechanical properties of the cobalt-based high-temperature alloy of Example 2 printed by the laser cladding deposition process are shown in Table 5 below.

[0110] Table 4

[0111]

[0112] Table 5

[0113] Test conditions Yield strength (MPa) Tensile strength(MPa) Elongation(%) 20℃ 762 1400 16.2 900℃ 611 760 14.8 1000℃ 354 471 11.5

[0114] The deposited structure of Example 2 of the present application is as follows Figure 4 As shown in the figure. After laser cladding deposition printing, a crack-free, well-metallurgically bonded structure was obtained. The dendrite size is small, the volume fraction of the γ' phase reaches 70%, with good cubicity and a size of about 75-80nm.

[0115] Table 6 above shows the tensile properties of the alloy in Example 2 as deposited. The printed samples exhibit excellent mechanical properties both at room temperature and at high temperature.

[0116] Embodiment 3:

[0117] The composition of Example 3 is shown in Table 6 below; the mechanical properties of the cobalt-based high-temperature alloy of Example 3 printed by the laser cladding deposition process are shown in Table 7 below.

[0118] Table 6

[0119]

[0120] Table 7

[0121] Test conditions Yield strength (MPa) Tensile strength(MPa) Elongation(%) 20℃ 806 1339 18.2 900℃ 460 632 32 1000℃ 258 328 28.5

[0122] Table 7 above shows the tensile properties of the alloy of Example 3 in the deposited state. The printed samples show excellent mechanical properties both at room temperature and at high temperature.

[0123] It is easy for those skilled in the art to understand that, under the premise of no conflict, the above-mentioned advantageous methods can be freely combined and superimposed.

[0124] The above are only preferred embodiments of the present application and are not intended to limit the present application. Any modifications, equivalent replacements and improvements made within the spirit and principles of the present application shall be included in the protection scope of the present application. The above are only preferred implementations of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and variations can be made without departing from the technical principles of the present application, and these improvements and variations should also be regarded as the protection scope of the present application.

Claims

1. An additively manufactured cobalt-based high-temperature alloy, characterized in that: The raw materials include the following weight percentages: C 0.05-0.2%, B 0.01-0.05%, Hf 0.5-2.0%, Zr 0.01-0.1%, Al 3.0-6.0%, Ta6.0-10.0%, W 10.0-16.0%, Cr 4.0-7.0%, Ni 15.0-25.0%, balance Co.

2. The cobalt-based alloy according to claim 1, characterized in that: In the additively manufactured cobalt-based high-temperature alloy, the volume percentage of the γ' phase is higher than 70%.

3. The additively manufactured cobalt-based high-temperature alloy according to claim 1, characterized in that: In the additively manufactured cobalt-based high-temperature alloy, the size of the γ' phase is 50-100 nm.

4. The additively manufactured cobalt-based high-temperature alloy according to claim 1, characterized in that: The room temperature tensile strength of the additively manufactured cobalt-based alloy is above 1300 MPa.

5. A method for preparing a cobalt-based high-temperature alloy by additive manufacturing as claimed in any one of claims 1 to 4, characterized in that: The steps include: Step (1): weighing the raw material as described in claim 1; performing laser cladding deposition printing; and obtaining an alloy.

6. The method for preparing a cobalt-based high-temperature alloy by additive manufacturing according to claim 5, characterized in that: The method comprises the following steps: the parameters of the laser cladding deposition process printing include: laser power 1100-1700W, scanning speed 600-1300mm / min, powder feeding amount 5-11g / min, and spot diameter 2-3mm.

7. The method for preparing a cobalt-based high-temperature alloy by additive manufacturing according to claim 5, characterized in that: The additive manufacturing method for preparing a cobalt-based high-temperature alloy further comprises the following steps: Step (2): heat treating the alloy obtained in step (1).

8. The method for preparing a cobalt-based high-temperature alloy by additive manufacturing according to claim 7, characterized in that: The heat treatment comprises the following steps: Step S1: solution treatment; further, the solution treatment comprises: firstly keeping warm at 1240-1300°C for 1-5h; then keeping warm at 1260-1310°C for 1-5h, and then cooling to room temperature.

9. The method for preparing a cobalt-based high-temperature alloy by additive manufacturing according to claim 8, characterized in that: The heat treatment comprises the following steps: Step S2: performing a first aging treatment on the alloy after the solution treatment in step S1; further, the first aging treatment includes: keeping warm at 800-1200°C for 26-50h, and then cooling to room temperature.

10. The method for preparing a cobalt-based high-temperature alloy by additive manufacturing according to claim 9, characterized in that: The heat treatment comprises the following steps: Step S3: performing a second aging treatment on the alloy after the first aging treatment in step S2; further, the second aging treatment includes: keeping warm at 600-800°C for 15-35h, and then cooling to room temperature.