Method for regulating and controlling refractory high-entropy alloy hot forging structure
Through the pretreatment and multi-stage forging technology of cast high-entropy alloys, the problem of hot forging tissue regulation of AlCrNbMoTaTiHf system has been solved, and the uniformity and recrystallization of hot forging tissue have been improved, which is suitable for a variety of application needs.
Patent Information
- Application Number
- CN202411165841.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art lacks methods for regulating hot forging structure of refractory high entropy alloys, especially the AlCrNbMoTaTiHf system, which is difficult to meet the requirements of hot forging structures under different application contexts.
Pretreatment of the cast high-entropy alloy before final forging, including high-temperature solid solution + slow-cooling treatment, isothermal forging under different initial grain structures and static recrystallization heat treatment, and finally, the second fire isothermal forging isothermal forging to regulate the difficulty of melting Hot forging structure of high entropy alloys.
It realizes effective regulation of hot forging tissue of refractory high entropy alloys, improves the uniformity and recrystallization of the tissue, and is suitable for hot forging tissue requirements under different application backgrounds.
Smart Images

Figure CN118932238A_ABST
Abstract
Description
Technical Field
[0001] The invention discloses a method for regulating the hot forging structure of a refractory high-entropy alloy. The refractory high-entropy alloy is a cast AlCrNbMoTaTiHf alloy and belongs to the technical field of metal materials. Background Art
[0002] With the increasing demand for the temperature bearing capacity of hot end components in aerospace, shipbuilding and ground-based gas turbines, it is inevitable that the high-temperature resistant materials used for hot end components must have better high-temperature performance. The refractory high-entropy alloy developed in recent years is a new type of high-temperature resistant structural material with great potential. Compared with traditional nickel-based high-temperature alloys, it has the advantages of higher melting point and hardness, higher high-temperature strength and resistance to high-temperature softening. In order to meet the mechanical property requirements of hot-forged parts, it is inevitable that the refractory high-entropy alloy structure must meet the corresponding requirements. For example, as a turbine disk material for aircraft engines, the refractory high-entropy alloy hot forging structure is required to be uniform and fine; while as a turbine disk material for large ground-based gas turbines, the grain requirements for its hot forging structure are significantly lower than those for aircraft engines. Therefore, according to different application background requirements, it is necessary to obtain a method for adjusting the hot forging structure of refractory high-entropy alloys.
[0003] AlCrNbMoTaTiHf alloy in the refractory high entropy alloy system has a very high melting point, high high temperature strength and plasticity, and high high temperature microstructure stability. It is a new high temperature resistant candidate structural material for various hot end components in different fields. In order to further improve the comprehensive performance of the refractory high entropy alloy of the AlCrNbMoTaTiHf system, it is necessary to perform hot processing. According to different application requirements, it is necessary to design corresponding appropriate hot forging parameters to obtain a microstructure state that meets the performance requirements. However, there is currently a lack of research on the hot forging of refractory high entropy alloys in the AlCrNbMoTaTiHf system, and there is even less research on regulating the hot forging microstructure of the refractory high entropy alloys in the system. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a method for regulating the hot forging structure of a refractory high entropy alloy. The method aims to solve the problem that the cast high entropy alloy is affected by the smelting and homogenization processes, and the grain structure before hot forging is not the same, that is, the grain size before hot forging is very different. Before final forging, the cast high entropy alloy is pretreated to achieve a unified "intermediate state" grain size standard, leaving a larger processing window for the subsequent final forging, so as to obtain the hot forging structure required in different application backgrounds.
[0005] The method of the present invention performs pretreatment of the cast high entropy alloy before final forging in sequence, including high temperature solid solution + slow cooling treatment, first fire isothermal forging with different parameters according to different initial grain structures, static recrystallization heat treatment after the first fire forging, and finally, the second fire isothermal forging is completed according to the hot forging structure requirements required in different application backgrounds, so as to realize the effective regulation of the hot forging structure of the refractory high entropy alloy AlCrNbMoTaTiHf.
[0006] To achieve the above purpose, the technical solution of the present invention is as follows:
[0007] In the method for controlling the hot forging structure of a refractory high entropy alloy of the present invention, the refractory high entropy alloy is a cast AlCrNbMoTaTiHf alloy, characterized in that: the molar expression of the AlCrNbMoTaTiHf alloy is Al a Cr b Nb c Mo d Ta e Ti f Hf g , wherein: a=2-6, b=2-4, c=18-28, d=4-8, e=6-10, f=30-40, g=15-23, a+b+c+d+e+f+g=100; characterized in that the steps of the method are as follows:
[0008] Step 1, placing the refractory high entropy alloy AlCrNbMoTaTiHf as-cast billet in a heat treatment furnace, heating it to 1170-1230°C, keeping it warm for 1-3h, then slowly cooling it to 1000-1050°C and then cooling it to room temperature in the furnace, the slow cooling rate being 30-60°C / h;
[0009] Step 2: After sandblasting and lubricating the surface of the refractory high entropy alloy AlCrNbMoTaTiHf cast blank obtained after the heat treatment in step 1, the blank is placed in a heating furnace for heating, and then quickly transferred to a hydraulic press for first-fire isothermal forging. After a deformation amount of 45% to 55%, a refractory high entropy alloy AlCrNbMoTaTiHf forging blank is obtained. The process parameters of the first-fire isothermal forging are as follows:
[0010] When the grain size of the refractory high entropy alloy AlCrNbMoTaTiHf as-cast billet after heat treatment in step 1 is ASTM 3.0-5.0, the first isothermal forging temperature is 1130-1170°C, and the strain rate is controlled at 0.5-3s -1 ;
[0011] When the grain size of the refractory high entropy alloy AlCrNbMoTaTiHf as-cast billet after heat treatment in step 1 is ASTM 6.0-8.0, the first isothermal forging temperature is 1110-1140°C, and the strain rate is controlled at 0.01-0.1s -1 ;
[0012] When the grain size of the refractory high entropy alloy AlCrNbMoTaTiHf as-cast billet after heat treatment in step 1 is finer than ASTM8.0 grade, the first isothermal forging temperature is 1090-1140°C, and the strain rate is controlled at 0.001-0.08s -1 ;
[0013] Step 3: placing the refractory high entropy alloy AlCrNbMoTaTiHf forging blank obtained after the treatment in step 2 in a heat treatment furnace, performing a heat treatment at 1080-1130° C. for 0.5-1.5 h, and then cooling the furnace to room temperature;
[0014] Step 4: After sandblasting and lubricating the surface of the refractory high entropy alloy AlCrNbMoTaTiHf forging blank obtained after the treatment in step 3, the blank is heated in a heating furnace and quickly transferred to a hydraulic press for second isothermal forging to obtain the final forging after a deformation of 40% to 60%.
[0015] During implementation, the heating and holding time before the first isothermal forging in step 2 and the second isothermal forging in step 4 is 1 to 2 hours.
[0016] During the implementation, during the first isothermal forging in step 2 and the second isothermal forging in step 4, the reduction in the ambient temperature in the mold should be controlled to be no greater than 300°C.
[0017] In addition, the process parameters of the second isothermal forging in step 4 are:
[0018] When the final forging grain structure is required to be finer than the uniform structure of ASTM grade 8, the grain size of the refractory high entropy alloy AlCrNbMoTaTiHf forging blank obtained after step 3 should be controlled to be no coarser than ASTM grade 6.0; the forging temperature is 1080-1120°C, and the strain rate is 0.001-0.5s -1 ;
[0019] When the final forging grain structure is required to be a uniform structure of ASTM 5 to 7, the forging temperature is 1110 to 1140°C and the strain rate is 0.005 to 0.03s -1 ;
[0020] When the final forging grain structure is required to be a uniform structure of ASTM grade 2 to 4, the forging temperature is 1140 to 1170°C and the strain rate is 0.05 to 0.1s -1.
[0021] During implementation, after the second isothermal forging in step 4, the final forging is covered with asbestos felt after it is taken out of the furnace, and then subjected to slow cooling treatment.
[0022] The technical solution of the present invention is characterized in that the precipitation phase in the AlCrNbMoTaTiHf refractory high entropy alloy is first dissolved back by high-temperature solid solution back-dissolution + slow cooling before final forging to form a supersaturated solid solution, and then a large number of coarse Hf-rich phases are precipitated by slow cooling, which effectively increases the ability of the Hf-rich phase to hinder dislocation movement, thereby greatly improving the nucleation ability of the dynamic recrystallization of the refractory high entropy alloy during hot forging, and then refining the forging structure and effectively improving the uniformity of the forging structure. Further, the technical solution of the present invention studies the organizational evolution law of the AlCrNbMoTaTiHf refractory high entropy alloy during hot forging under different initial grain structure conditions, and on this basis establishes the response relationship between the initial grain structure-forging parameters (temperature, strain rate, deformation)-hot forging structure, which provides technical guarantee for obtaining a hot forging structure with moderate grain size and relatively uniform distribution of recrystallized and non-recrystallized grains after the first fire isothermal forging, and forms an applicable range of process parameters.
[0023] In addition, due to the limited deformation amount of the AlCrNbMoTaTiHf refractory high entropy alloy during the first isothermal forging, the alloy cannot be completely recrystallized, while some non-recrystallized grains can undergo static recrystallization through heat treatment, thereby effectively improving the recrystallization degree of the alloy after the first isothermal forging, and making organizational preparations for obtaining a uniform grain structure in the second isothermal forging. Through a lot of research in the early stage of the present invention, it was obtained that static recrystallization can occur under the conditions of 1080-1130°C and 0.5-1.5h, and it was statistically obtained that the recrystallization degree of the alloy under this condition is not less than 85%. This measure forms step three of the technical solution of the present invention.
[0024] For the second fire isothermal forging, the technical solution of the present invention carries out the correlation between the second fire isothermal forging parameters and the grain structure of the forging according to the different requirements of the grain structure of the forging under different application background requirements, so as to finally realize the effective regulation of the hot forging structure under different application requirements. The specific contents are:
[0025] The technical solution of the present invention proposes a corresponding final forging process window, and provides process guidance specifications for the development of forgings for different application directions. When implemented, the final forging temperature is 1080-1120°C and the strain rate is 0.001-0.5s for the uniform structure of the turbine disk for aircraft engines that is finer than ASTM 8.0. -1 For the uniform structure of ASTM 5.0-7.0 required for the turbine disk of ship gas turbine, the final forging temperature is 1110-1140℃ and the strain rate is 0.005-0.03s-1 For the uniform structure of ASTM 2 to 4 required for the turbine disk of large ground gas turbines, the final forging temperature is 1140 to 1170°C and the strain rate is 0.05 to 0.1s -1 .
[0026] The beneficial effects of the technical solution of the present invention are:
[0027] 1. The present invention pretreats the precipitated phase of the AlCrNbMoTaTiHf refractory high entropy alloy by high-temperature solid solution dissolution+slow cooling, thereby improving the recrystallization degree of the alloy billet, which is beneficial to the subsequent grain refinement and improvement of organizational uniformity.
[0028] 2. The present invention adopts different targeted first-fire forgings due to differences in initial grain structures, combined with heat treatment that can produce static recrystallization and uniform grain structures after the first-fire forging, to prepare for the final second-fire forging to obtain uniform grain structures; through the study of the correlation between the second-fire forging parameters and the grain structure of the forgings, the effective regulation of the hot forging structure under different application requirements is ultimately achieved.
[0029] 3. The method for controlling the hot forging structure of the present invention is applicable to the control of the hot forging structure of metallurgical cast refractory high entropy alloys, and is also applicable to the control of the hot forging structure of powder metallurgy and additive manufacturing refractory high entropy alloys. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figures 1 to 4 They are the final forging microstructure diagrams of the AlCrNbMoTaTiHf refractory high entropy alloys obtained in Examples 1 to 4 of the present invention respectively. DETAILED DESCRIPTION
[0031] The technical solution of the present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments:
[0032] Example 1
[0033] The molar expression of the AlCrNbMoTaTiHf high entropy alloy is Al5Cr2Nb 24 Mo6Ta8Ti 36 Hf 19 The refractory high entropy alloy ingot is melted by four times of turning in an electromagnetic suspension melting furnace, and then extruded to obtain ASTM 5.0 grade refractory high entropy alloy rods.
[0034] The steps of the method for controlling the hot forging structure of a refractory high entropy alloy using the present invention are as follows:
[0035] Step 1: Al5Cr2Nb 24 Mo6Ta8Ti 36 Hf 19The refractory high entropy alloy bar is placed in a heat treatment furnace, heated to 1190°C, kept at this temperature for 2 hours, then slowly cooled to 1020°C at a cooling rate of 60°C / h, and then cooled to room temperature in the furnace;
[0036] Step 2: After the surface of the refractory high entropy alloy billet in step 1 is sandblasted and lubricated, the billet is placed in a heating furnace, and the high entropy alloy billet is heated to 1150° C. and kept warm for 1.5 hours before being used for the first fire forging;
[0037] Step 3: Take the high entropy alloy billet from step 2 out of the heating furnace and quickly transfer it to a hydraulic press. -1 After forging and deforming by 53% at a strain rate, the forging blank is obtained. During forging, the reduction of the ambient temperature in the mold furnace should be controlled to be no more than 300°C.
[0038] Step 4: Take the forging blank out of the hydraulic press, place the refractory high entropy alloy forging blank in a heat treatment furnace, perform heat treatment at 1100°C for 1 hour, and then cool the furnace to room temperature;
[0039] Step 5: placing the forging blank after the heat treatment in step 4 in a heating furnace for heating, heating the high entropy alloy forging blank to 1110° C., keeping the temperature for 1.5 hours, and then using it for the second fire forging;
[0040] Step 6: After the forging billet in step 5 is heat-insulated, it is taken out and quickly transferred to the hydraulic press for forging at a temperature of 1110°C and a strain rate of 0.05s -1 After forging deformation of 50%, the forging is obtained. During forging, the reduction of the ambient temperature in the mold furnace should be controlled to be no more than 300°C;
[0041] Step 7: After the forging is taken out, it is covered with asbestos felt, and finally the forging structure with an average grain size of ASTM 8.0 is obtained, such as Figure 1 shown.
[0042] Example 2
[0043] The molar expression of the AlCrNbMoTaTiHf high entropy alloy is Al4Cr3Nb 22 Mo6T 10 Ti 35 Hf 20 The refractory high entropy alloy ingot is melted by three times of turning in an electromagnetic suspension melting furnace, and then extruded to obtain ASTM 7.0 grade refractory high entropy alloy rods.
[0044] The steps of the method for controlling the hot forging structure of a refractory high entropy alloy using the present invention are as follows:
[0045] Step 1: Al4Cr3Nb 22 Mo6T 10 Ti 35 Hf20 The refractory high entropy alloy bar is placed in a heat treatment furnace, heated to 1200°C, kept at this temperature for 1.5 hours, then slowly cooled to 1000°C at a cooling rate of 50°C / h, and then cooled to room temperature in the furnace;
[0046] Step 2: After the surface of the refractory high entropy alloy billet in step 1 is sandblasted and lubricated, the billet is placed in a heating furnace, the high entropy alloy billet is heated to 1130° C., kept warm for 1 hour, and then used for the first fire forging;
[0047] Step 3: Take the high entropy alloy billet from step 2 out of the heating furnace and quickly transfer it to a hydraulic press. -1 After forging and deforming by 50% at a strain rate, the forging blank is obtained. During forging, the reduction of the ambient temperature in the mold furnace should be controlled to be no more than 300°C.
[0048] Step 4: Take the forging blank out of the hydraulic press, place the refractory high entropy alloy forging blank in a heat treatment furnace, perform heat treatment at 1110°C for 1.2h, and then cool the furnace to room temperature;
[0049] Step 5: placing the forging blank after the heat treatment in step 4 in a heating furnace for heating, heating the high entropy alloy forging blank to 1160° C., keeping the temperature for 1 hour, and then using it for the second fire forging;
[0050] Step 6: After the forging billet in step 5 is heat-insulated, it is taken out and quickly transferred to the hydraulic press for forging at a temperature of 1160°C and a strain rate of 0.1s -1 After forging deformation of 48%, the forging is obtained. During forging, the reduction of the ambient temperature in the mold furnace should be controlled to be no more than 300°C;
[0051] Step 7: After the forging is taken out, it is covered with asbestos felt, and finally the forging structure with an average grain size of ASTM 3.0 is obtained, such as Figure 2 shown.
[0052] Example 3
[0053] The molar expression of the AlCrNbMoTaTiHf high entropy alloy is Al4Cr2Nb 26 Mo6Ta7Ti 34 Hf 21 The refractory high entropy alloy ingot is melted by five turns in an electromagnetic suspension melting furnace, and then extruded to obtain ASTM 9.0 grade refractory high entropy alloy rods.
[0054] The steps of the method for controlling the hot forging structure of a refractory high entropy alloy using the present invention are as follows:
[0055] Step 1: Al4Cr2Nb 26 Mo6Ta7Ti 34 Hf 21The refractory high entropy alloy bar is placed in a heat treatment furnace, heated to 1210°C, kept at this temperature for 2 hours, then slowly cooled to 1050°C at a cooling rate of 30°C / h, and then furnace cooled to room temperature;
[0056] Step 2: After the surface of the refractory high entropy alloy billet in step 1 is sandblasted and lubricated, the billet is placed in a heating furnace, the high entropy alloy billet is heated to 1100° C., kept warm for 2 hours, and then used for the first fire forging;
[0057] Step 3: Take the high entropy alloy billet from step 2 out of the heating furnace and quickly transfer it to a hydraulic press. -1 After forging and deforming by 52% at a strain rate, the forging blank is obtained. During forging, the reduction of the ambient temperature in the mold furnace should be controlled to be no more than 300°C.
[0058] Step 4: Take the forging blank out of the hydraulic press, place the refractory high entropy alloy forging blank in a heat treatment furnace, perform heat treatment at 1090°C for 1h, and then cool the furnace to room temperature;
[0059] Step 5: placing the forging blank after the heat treatment in step 4 in a heating furnace for heating, heating the high entropy alloy forging blank to 1110° C., keeping the temperature for 1.5 hours, and then using it for the second fire forging;
[0060] Step 6: After the forging billet in step 5 is heat-insulated, it is taken out and quickly transferred to the hydraulic press for forging at a forging temperature of 1080°C and a strain rate of 0.05s -1 After forging deformation of 45%, the forging is obtained. During forging, the reduction of the ambient temperature in the mold furnace should be controlled to be no more than 300°C;
[0061] Step 7: After the forging is taken out, it is covered with asbestos felt, and finally the forging structure with an average grain size of ASTM 10.0 is obtained, such as Figure 3 shown.
[0062] Example 4
[0063] The molar expression of the AlCrNbMoTaTiHf high entropy alloy is Al6Cr2Nb 22 Mo8Ta8Ti 32 Hf 22 The refractory high entropy alloy ingot is melted by four turns in an electromagnetic suspension melting furnace, and then extruded to obtain ASTM 6.0 grade refractory high entropy alloy rods.
[0064] The steps of the method for controlling the hot forging structure of a refractory high entropy alloy using the present invention are as follows:
[0065] Step 1: Al6Cr2Nb 22 Mo8Ta8Ti 32 Hf 22The refractory high entropy alloy bar is placed in a heat treatment furnace, heated to 1220°C, kept at this temperature for 1 hour, then slowly cooled to 1040°C at a cooling rate of 40°C / h, and then cooled to room temperature in the furnace;
[0066] Step 2: After the surface of the refractory high entropy alloy billet in step 1 is sandblasted and lubricated, the billet is placed in a heating furnace, and the high entropy alloy billet is heated to 1140° C. and kept warm for 1.5 hours before being used for the first fire forging;
[0067] Step 3: Take the high entropy alloy billet from step 2 out of the heating furnace and quickly transfer it to a hydraulic press. -1 The forging blank is obtained after forging deformation of 56% at a strain rate. The reduction of the ambient temperature in the mold furnace during forging should be controlled to be no more than 300°C.
[0068] Step 4: Take the forging blank out of the hydraulic press, place the refractory high entropy alloy forging blank in a heat treatment furnace, perform heat treatment at 1110°C for 1 hour, and then cool the furnace to room temperature;
[0069] Step 5: placing the forging blank after the heat treatment in step 4 in a heating furnace for heating, heating the high entropy alloy forging blank to 1150° C., keeping the temperature for 1 hour, and then using it for the second fire forging;
[0070] Step 6: After the forging billet in step 5 is heat-insulated, it is taken out and quickly transferred to the hydraulic press for forging at a temperature of 1150°C and a strain rate of 0.08s -1 After forging deformation of 50%, the forging is obtained. During forging, the reduction of the ambient temperature in the mold furnace should be controlled to be no more than 300°C;
[0071] Step 7: After the forging is taken out, it is covered with asbestos felt, and finally the forging structure with an average grain size of ASTM 4.0 is obtained, such as Figure 4 shown.
Claims
1. A method for regulating the hot forging structure of a refractory high entropy alloy, wherein the refractory high entropy alloy is a cast AlCrNbMoTaTiHf alloy, characterized in that: The molar expression of the AlCrNbMoTaTiHf alloy is Al a Cr b Nb c Mo d Ta e Ti f Hf g , wherein: a=2-6, b=2-4, c=18-28, d=4-8, e=6-10, f=30-40, g=15-23, a+b+c+d+e+f+g=100; characterized in that the steps of the method are as follows: Step 1, placing the refractory high entropy alloy AlCrNbMoTaTiHf as-cast billet in a heat treatment furnace, heating it to 1170-1230°C, keeping it warm for 1-3h, then slowly cooling it to 1000-1050°C and then cooling it to room temperature in the furnace, the slow cooling rate being 30-60°C / h; Step 2: After sandblasting and lubricating the surface of the refractory high entropy alloy AlCrNbMoTaTiHf cast blank obtained after the heat treatment in step 1, the blank is placed in a heating furnace for heating, and then quickly transferred to a hydraulic press for first-fire isothermal forging. After a deformation amount of 45% to 55%, a refractory high entropy alloy AlCrNbMoTaTiHf forging blank is obtained. The process parameters of the first-fire isothermal forging are as follows: When the grain size of the refractory high entropy alloy AlCrNbMoTaTiHf as-cast billet after heat treatment in step 1 is ASTM 3.0-5.0, the first isothermal forging temperature is 1130-1170°C, and the strain rate is controlled at 0.5-3s -1 ; When the grain size of the refractory high entropy alloy AlCrNbMoTaTiHf as-cast billet after heat treatment in step 1 is ASTM 6.0-8.0, the first isothermal forging temperature is 1110-1140°C, and the strain rate is controlled at 0.01-0.1s -1 ; When the grain size of the refractory high entropy alloy AlCrNbMoTaTiHf as-cast billet after heat treatment in step 1 is finer than ASTM8.0 grade, the first isothermal forging temperature is 1090-1140°C, and the strain rate is controlled at 0.001-0.08s -1 ; Step 3: placing the refractory high entropy alloy AlCrNbMoTaTiHf forging blank obtained after the treatment in step 2 in a heat treatment furnace, performing a heat treatment at 1080-1130° C. for 0.5-1.5 h, and then cooling the furnace to room temperature; Step 4: After sandblasting and lubricating the surface of the refractory high entropy alloy AlCrNbMoTaTiHf forging blank obtained after the treatment in step 3, the blank is heated in a heating furnace and quickly transferred to a hydraulic press for second isothermal forging to obtain the final forging after a deformation of 40% to 60%.
2. The method for controlling the hot forging structure of a refractory high entropy alloy according to claim 1, characterized in that: The heating and holding time before the first isothermal forging in step 2 and the second isothermal forging in step 4 is 1 to 2 hours.
3. The method for controlling the hot forging structure of a refractory high entropy alloy according to claim 1, characterized in that: During the first isothermal forging in step 2 and the second isothermal forging in step 4, the reduction in the ambient temperature in the mold should be controlled to be no greater than 300°C.
4. The method for controlling the hot forging structure of a refractory high entropy alloy according to claim 1, characterized in that: The process parameters of the second isothermal forging in step 4 are: When the final forging grain structure is required to be finer than the uniform structure of ASTM grade 8, the forging temperature is 1080-1120°C and the strain rate is 0.001-0.5s -1 ; When the final forging grain structure is required to be a uniform structure of ASTM 5 to 7, the forging temperature is 1110 to 1140°C and the strain rate is 0.005 to 0.03s -1 ; When the final forging grain structure is required to be a uniform structure of ASTM grade 2 to 4, the forging temperature is 1140 to 1170°C and the strain rate is 0.05 to 0.1s -1 .
5. The method for controlling the hot forging structure of a refractory high entropy alloy according to claim 4, characterized in that: The grain size of the refractory high entropy alloy AlCrNbMoTaTiHf forging blank obtained after the treatment in step 3 should be controlled to be no coarser than ASTM grade 6.
0.
6. The method for controlling the hot forging structure of a refractory high entropy alloy according to claim 1, characterized in that: After the second isothermal forging in step 4, the final forging is covered with asbestos felt after it is taken out of the furnace and subjected to slow cooling treatment.