Supersonic spraying surface strengthening coating of finishing roll

By using alloy wear-resistant composite coating and supersonic spraying technology on the surface of the finish roll, hard metal compounds and carbides are formed, which solves the problem of easy shedding and wear of the oxide film on the surface of the finish roll, and improves wear resistance and impact resistance , extends service life and reduces production costs.

CN118932260APending Publication Date: 2024-11-12ANHUI HENGYI HARD FACE ENG CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410998804.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-12-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The friction coefficient, wear resistance, high temperature and impact resistance of existing finishing rolls are insufficient, resulting in the oxide film on the roll surface that is prone to fall off and wear, affecting rolling efficiency and product quality.

Method used

Using alloy wear-resistant composite coating, including the base layer and the working layer, the hard metal compounds and carbides are formed by introducing elements such as Ni, Cr, Co, Mo, B, V, Nb, etc., to improve the hardness and wear resistance of the coating. and through supersonic spraying technology and surface roughening path spraying technology, a stable oxide protective layer and skeleton network structure is formed.

Benefits of technology

It significantly improves the wear resistance, high temperature and impact resistance of the finish roll, enhances the bonding strength and corrosion resistance of the coating, extends the service life of the roll and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932260A_ABST
    Figure CN118932260A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of material surface strengthening, in particular to a finish roll supersonic spraying surface strengthening coating. Co is introduced into the base layer and the working layer, the Co has the valuable characteristics of excellent corrosion resistance, heat resistance, oxidation resistance and the like, and is used for forming a hard metal compound with N and / or Cr in a matrix, so that the hard metal compound is dispersed and distributed in the alloy to play a dispersion strengthening role, and after the content of the Co is accurately added, the hardness of the alloy is improved. B is combined in the working layer to promote precipitation of dispersed chromium-carbon and boron-chromium hard phases, a plastic face-centered cubic structure solid solution and promote formation of carbides at high temperature, and after comprehensive preparation, the hardness and wear resistance of the hard alloy can be improved, and excellent bonding strength is ensured; and meanwhile, the alloy still has relatively high hardness and relatively good oxidation resistance, impact resistance, thermal shock resistance and corrosion resistance at a high temperature, the spraying process performance of an alloy coating is improved, the deposition rate is increased, and the friction coefficient is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This case is a divisional application of "application number CN202311854119.0, name: Alloy wear-resistant composite coating and finishing roller supersonic spraying surface strengthening treatment process, and application date: 2023.12.29". Technical Field

[0002] The invention relates to the technical field of material surface strengthening, in particular to a finishing roll supersonic spraying surface strengthening coating. Background Art

[0003] During the rolling process of the finishing roll, the roll and the billet are subjected to high temperature and high pressure, and the roll surface oxidizes to produce iron scale. During rolling, the strip temperature is 980℃, and the roll surface quickly rises to about 600℃. After leaving the deformation zone, the roll surface temperature is affected by the cooling water of the finishing roll and drops by 40-100℃. The roll surface produces an oxide film in a complex environment of high temperature, high pressure and water vapor. In the early stage of rolling, the oxide film on the surface of the strip is thin and has poor adhesion to the roll substrate, so it is easy to fall off due to wear and press into the surface of the strip.

[0004] Chinese invention patent (CN103173713A) discloses a supersonic spraying process for the pass of a semi-steel steel roll, the steps of which are as follows: 1) Pretreatment of the pass working surface: (1) Clean the paint, iron oxide and oil stains on the pass working surface; (2) Clean the pass working surface with acetone; 2) Shot peening the pass working surface: (1) Use white corundum sand shot with a particle size of about 100 mesh to shot peen the pass working surface, the shot peening speed is 7 meters / second, the air pressure during sand blasting is 5-6kg / cm2, and the distance between the sand blasting equipment and the sand blasting surface is 120-18 0mm, and the angle with the sandblasting surface is 90°; 3) Use supersonic spraying equipment to supersonic spray the hole working surface: (1) Preheat the surface to be sprayed with oxygen to 60-80°C; (2) Powder spraying: Use spraying material to spray the hole working surface, and the spraying thickness is 0.03-0.07mm; the distance between the spray gun and the spraying surface is 100-120mm, and the angle between the spray gun and the spraying surface is ≤90°; 4) Sealing treatment of the coating: (1) Use diamond grinding to grind the sprayed surface; (2) Use silicone resin paint to seal the coating twice; (3) After sealing, use plastic film to protect the hole.

[0005] For example, a Chinese invention patent (CN104611664A) discloses a method for supersonic spray strengthening of alloy on the hole surface of a steel finishing roller. The method uses nano-scale carbide alloy powder, including: 15-20% nickel-aluminum powder, 50-70% cobalt-tungsten carbide alloy powder, 10-20% chromium-molybdenum-manganese composite powder, and 5-15% boron-tungsten composite powder. First, nickel-aluminum powder is used to prime the steel finishing roller to a thickness of 0.02 mm, and then the cobalt-tungsten carbide alloy powder, chromium-molybdenum-manganese composite powder and boron-tungsten composite powder are melted and evenly sprayed onto the roller surface. The spray layer thickness is 0.15-0.20 mm, the distance between the spray gun and the spray surface is 160-180 mm, and the angle between the spray gun and the spray surface is ≤90°.

[0006] However, there is still room for further improvement in the friction coefficient, wear resistance, high temperature resistance and impact resistance of the finishing rollers after spraying by the above two methods. Summary of the invention

[0007] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0008] Alloy wear-resistant composite coating, including primer layer and working layer;

[0009] Alloy wear-resistant composite coating, including primer layer and working layer;

[0010] The composition of the primer layer includes Ni: 16-20, Cr: 4-6, Co: 11-23, Mo: 2-5 by weight, and the balance is Fe and trace impurities;

[0011] 1.2≤(N i+Cr) / Co≤1.5, 0.15≤Mo / N i≤0.38;

[0012] The composition of the working layer includes Cr: 20-35, B: 4.1-6.2, Co: 11-70 and trace impurities by weight;

[0013] 0.31≤Cr / (B+Co)≤0.44.

[0014] Preferably, the composition of the primer layer includes Ni: 16-20, Cr: 4-6, Co: 11-23, Mo: 2-5, and the balance is Fe and trace impurities by weight;

[0015] 1.27≤(N i+Cr) / Co≤1.34, 0.18≤Mo / N i≤0.25;

[0016] The composition of the working layer includes Cr: 20-35, B: 4.1-6.2, Co: 11-70 and trace impurities by weight;

[0017] 0.33≤Cr / (B+Co)≤0.41.

[0018] Alloy wear-resistant composite coating, including primer layer and working layer;

[0019] The components of the primer layer include Ni: 16-18, Cr: 4-6, Co: 11-22, Mo: 2-4, C: 0.4-0.8, V: 1.0-2.0, Nb: 1.0-2.0, and the balance is Fe and trace impurities;

[0020] 0.45≤Co / (Ni+Cr)≤0.77;

[0021] 0.036≤(V+Nb) / (Fe+C+Co)≤0.048;

[0022] 0.011≤C / (N i+Cr+Co)≤0.019;

[0023] 0.14≤Mo / N i≤0.31;

[0024] The composition of the working layer includes, by weight, Cr: 20-35, B: 4.1-6.2, Co: 11-65, W: 2-5, and trace impurities;

[0025] 0.31≤Cr / (B+Co)≤0.51;

[0026] 0.01≤B / (Cr+Co+W)≤0.09.

[0027] Preferably, the composition of the primer layer includes, by weight, Ni: 16-18, Cr: 4-6, Co: 11-22, Mo: 2-4, C: 0.4-0.8, V: 1.0-2.0, Nb: 1.0-2.0, and the balance is Fe and trace impurities;

[0028] 0.47≤Co / (Ni+Cr)≤0.75;

[0029] 0.041≤(V+Nb) / (Fe+C+Co)≤0.046;

[0030] 0.014≤C / (N i+Cr+Co)≤0.017;

[0031] 0.16≤Mo / N i≤0.24;

[0032] The composition of the working layer includes, by weight, Cr: 20-35, B: 4.1-6.2, Co: 11-65, W: 2-5, and trace impurities;

[0033] 0.36≤Cr / (B+Co)≤0.49;

[0034] 0.03≤B / (Cr+Co+W)≤0.07.

[0035] The surface strengthening treatment process of the finishing roller by supersonic spraying includes the following steps:

[0036] Surface purification:

[0037] Clean the sprayed surface with acetone until the roller surface reveals a fresh metal surface, then dry it until there is no water mark on the surface;

[0038] Surface roughening treatment:

[0039] The sandblasting material is white corundum sand: 80 mesh, the sandblasting distance is between 120 and 150 mm, the sandblasting angle is between 75° and 90°, and the air pressure is 0.6 to 0.7 MPa;

[0040] The roughness of the workpiece surface after sandblasting should not exceed Ra: 3.2um;

[0041] After sandblasting, orderly patterns are formed on the roller surface. The orderly patterns are grid patterns formed by two groups of spiral sandblasting paths with different rotation directions, or are composed of several sandblasting areas. The sandblasting paths of two adjacent sandblasting areas are axial and circumferential respectively.

[0042] Preheating before spraying:

[0043] Before spraying, preheat the spray surface and control the preheating temperature at 50℃~60℃;

[0044] Spraying:

[0045] The spraying is carried out using JP5000 equipment, with a spray gun distance of 250-300 mm, a gun moving speed of 150-300 mm, a rotation speed of 25-40 r / min, and a powder feeding rate of 20-30 g / min. The raw material powder of the base layer as claimed in claim 1 or 2 is first sprayed on the roller surface, and then the raw material powder of the working layer as claimed in claim 1 or 2 is sprayed on the surface of the base layer to form a composite coating on the roller surface, with a coating thickness of 50-60 um.

[0046] Post-spraying treatment:

[0047] After the surface is sprayed, it is immediately polished with an oil stone to ensure that there is no granularity, the surface roughness Ra is less than 3.2, the coating hardness is greater than 1200HV, and the bonding strength is ≥70Mpa.

[0048] The surface strengthening treatment process of the finishing roller by supersonic spraying includes the following steps:

[0049] Surface purification:

[0050] Clean the sprayed surface with acetone until the roller surface reveals a fresh metal surface, then dry it until there is no water mark on the surface;

[0051] Surface roughening - roughening path spraying:

[0052] A grid groove structure is formed on the roller surface by turning, wherein the grid groove structure includes staggered sinusoidal grooves 1 and sine grooves 2, two groups of intersection nodes are provided between adjacent sinusoidal grooves 1 and sine grooves 2, and the depth of the sinusoidal groove 1 is greater than the depth of the sinusoidal groove 2;

[0053] Sine grooves are formed in the forward direction and roughening path spraying is completed in the reverse direction, or sinusoidal grooves are formed in the reverse direction and roughening path spraying is completed in the forward direction. The front side of the roughening path spraying point in the spraying direction is preheated, and the preheating temperature is controlled at 50-60°C;

[0054] Preheating before spraying:

[0055] Before spraying, preheat the spray surface and control the preheating temperature at 50℃~60℃;

[0056] Spraying:

[0057] Spray gun distance: 250-300mm, gun moving speed: 150-300mm, rotation speed: 25-40r / min, powder feeding rate: 20-30g / min, first spray the raw material powder of the base layer as claimed in claim 1 or 2 on the roller surface, then spray the raw material powder of the working layer as claimed in claim 1 or 2 on the surface of the base layer to form a composite coating on the roller surface, and the coating thickness is 50-60um;

[0058] Post-spraying treatment:

[0059] After the surface is sprayed, it is immediately polished with an oil stone to ensure that there is no granularity, the surface roughness Ra is less than 3.2, the coating hardness is greater than 1200HV, and the bonding strength is ≥70Mpa.

[0060] Preferably, the surface roughening-roughening path spraying step adopts an integrated molding device, which includes a clamping mechanism and a frame. The clamping mechanism is equipped with a rotating spindle, which can drive the clamping mechanism and the finishing roller to rotate. A slide rail is arranged at the bottom of the frame, and a servo motor is installed on the slide rail. The servo motor drives the frame to move along the length direction of the slide rail.

[0061] A reciprocating screw and a driving motor are installed on the frame. The driving motor is installed on the frame and is suitable for driving the reciprocating screw installed on the frame to rotate. The reciprocating screw is matched with a driving block. The driving block is suitable for lateral reciprocating motion relative to the frame. A plurality of sliders are installed on the frame. A driven ring with a notch is installed on the inner side of the plurality of sliders. The notch is suitable for the free passage of the clamping mechanism. The driven ring and the driving block are meshed by teeth. A switching structure, a coarsening structure and a spraying structure are installed on the driven ring. The switching structure is suitable for reciprocatingly switching the coarsening structure and the spraying structure to be in a working state.

[0062] Preferably, the switching mechanism includes a switching frame, which is rotatably mounted on the driven ring via an articulated seat, an angle limiting part is installed between the switching frame and the articulated seat, the switching frame completes reciprocating angle switching between the angle limiting part and the articulated seat, and a blocking structure is hoop-connected on the roller shaft head, the blocking structure is suitable for unidirectionally hindering the corresponding switching frame from moving in the opposite direction and completing the angle switching through the angle limiting part.

[0063] Preferably, the spraying structure comprises an adjusting frame and a sprayer, the adjusting frame is suitable for selectively adjusting the position relative to the switching frame, the sprayer is installed on the adjusting frame, the adjusting frame is linearly adjustable relative to the switching frame, and a pusher is installed on the switching frame, which is suitable for driving the position of the adjusting frame to be selectively adjustable, and the sprayer is provided with two powder material tubes and a supersonic spraying structure, the angles of the two powder material tubes relative to the supersonic spraying structure are adjustable, and the two powder material tubes are respectively suitable for powder feeding operations of base layer and working layer raw materials;

[0064] The roughening structure includes a driver and a tool holder installed on a switching frame. The output end of the driver is connected to the tool holder via a worm gear. The tool holder is rotatably installed on the switching frame. The driver can adjust the travel angle of the tool holder in time. A turning tool is installed on the tool holder for spiral roughening of the roller surface.

[0065] Preferably, the powder raw material sprayed on the roughening path has the same composition and ratio as the powder raw material of the base layer.

[0066] Compared with the prior art, the present invention has the following beneficial effects:

[0067] 1) By introducing Ni, Cr, Co, and Mo elements into the base layer and controlling the ratio of (Ni+Cr) / Co, they can be used to form hard metal compounds with Ni and / or Cr in the matrix, so that they are dispersed in the alloy and play a role of dispersion strengthening. The introduction of Mo can improve the valence state of Ni, thereby enhancing the dp orbital hybridization with the neighboring O, which helps to activate the lattice O. Due to the activation of O on the surface of the material, a more stable oxide protective layer can be formed, thereby resisting the erosion of the corrosive medium to the material, thereby enhancing the corrosion resistance of the material.

[0068] 2) Introduce Cr, B, and Co elements into the base layer. Co is used to form hard metal compounds with Ni and / or Cr in the matrix, so that it is dispersed in the alloy to play a role in dispersion strengthening. After ensuring the precise addition of Co content, B will be combined with B in the working layer to promote the precipitation of dispersed chromium-carbon, boron-chromium hard phase, plastic face-centered cubic structure solid solution, and promote the formation of carbides at high temperatures. After comprehensive configuration, the hardness and wear resistance of cemented carbide can be improved, and excellent bonding strength can be ensured. At the same time, it still has high hardness and good oxidation resistance, impact resistance, thermal shock resistance and corrosion resistance at high temperatures, improving the spraying process performance of the alloy coating and increasing the deposition rate.

[0069] 3) Co is introduced into the base layer and working layer. Co has excellent corrosion resistance, heat resistance and oxidation resistance. Co is used to form hard metal compounds with Ni and / or Cr in the matrix, so that it is dispersed in the alloy and plays a role of dispersion strengthening. After ensuring the precise addition of Co content, B will be combined with B in the working layer to promote the precipitation of dispersed chromium-carbon, boron-chromium hard phase, plastic face-centered cubic structure solid solution and promote the formation of carbides at high temperature. After comprehensive configuration, the hardness and wear resistance of cemented carbide can be improved, and excellent bonding strength can be ensured. At the same time, it still has high hardness and good oxidation resistance, impact resistance, thermal shock resistance and corrosion resistance at high temperature, improves the spraying process performance of alloy coating, increases deposition rate and reduces friction coefficient.

[0070] 4) V and Nb are introduced into the base layer, and they are precisely adjusted to meet the above-mentioned ratio range, so that a nano-scale carbide second phase is formed inside it, which significantly reduces the overheating sensitivity of the coating, refines the grains, and has high toughness; because the grain refinement effect inside the coating will be slightly affected after the Co content is precisely formulated, and a variety of metal compound phases are formed inside it due to the introduction of V and Nb, such as: VCo5, ​​VCo3, NbCo2, NbCo5, VNb2, VNb5. During the solidification process of the alloy, the metal compound phase can serve as the core of non-uniform nucleation, promote the nucleation and growth of grains, thereby obtaining fine grains. The metal compound phase can also further refine the grains by hindering the growth of grains and inhibiting the movement of grain boundaries, and has high strength, impact resistance, good corrosion resistance and high temperature stability.

[0071] 5) Rationally introduce Cr, Co, B, and W into the working layer and precisely control their addition amounts, form tungsten-cobalt-boron intermetallic compounds and boron-chromium alloy phases, plastic face-centered cubic structure solid solutions, and promote the formation of borides at high temperatures in the working layer. After being equipped, the hardness and wear resistance of the cemented carbide can be improved, and excellent bonding strength can be ensured. At the same time, it still has high hardness and good oxidation resistance and corrosion resistance at a high temperature of 960°C, improves the spraying process performance of the alloy coating, increases the deposition rate, and reduces the friction coefficient.

[0072] 6) The surface of the finishing roller is first shot peened with 80 meshes by using supersonic spraying process to form orderly lines on the surface, thereby ensuring the roughness of the roller surface. The number of shot peening meshes should not be too large, otherwise the rough finishing roller quality will be low. If it is too small, it is difficult to obtain a roughened surface and effective bonding between layers cannot be ensured. Perform necessary preheating treatment before spraying to prevent the formation of a brittle layer structure on the surface due to large temperature differences.

[0073] 7) Surface roughening - roughening path spraying process, through the surface spiral roughening treatment, the roughening path spray cladding is carried out immediately after the roughening to obtain a skeleton network with consistent base layer components. The two grooves of the skeleton network have different depths. The skeleton network can improve the axial impact resistance, and at the same time can effectively improve the contact area between the coating and the roller body as well as the impact resistance and high temperature resistance. After the spraying is completed, the alloy in the groove is completely clad as a whole, and then the base layer spraying and the working layer spraying are carried out on the outer layer.

[0074] 8) Surface roughening - The roughening path spraying adopts a new structural design, which can spray along the path immediately after the roughening is completed. During spraying, preheating treatment is performed before the spraying path to prevent the occurrence of a brittle layer structure. The preheating treatment here can be laser preheating or flame or plasma preheating treatment. BRIEF DESCRIPTION OF THE DRAWINGS

[0075] Figure 1 This is a diagram showing the surface coating structure of a finishing roller according to an embodiment of the present invention.

[0076] Figure 2 It is a schematic diagram of the overall structure of the integrated molding equipment of the present invention.

[0077] Figure 3 for Figure 2 Enlarged view of the internal structure of the middle frame.

[0078] Figure 4 for Figure 2 Schematic diagram of the overall structure of the switching rack.

[0079] Figure 5 for Figure 4 Schematic diagram of the right side structure of the center switching rack.

[0080] Figure 6 for Figure 3 Schematic diagram of the structure of the angle limiting part between the middle articulated seat and the switching frame.

[0081] Figure 7 The schematic diagram of the structure inside the frame of the present invention (relative to Figure 2 The vertical direction of the middle frame);

[0082] Figure 8 It is a structural schematic diagram of the blocking structure in the present invention;

[0083] Fig. 9 It is a structural diagram of the present invention when the coating is changed from spraying to roughening;

[0084] Fig.10 It is a structural diagram of the present invention when the roughening is changed to the spraying working condition. DETAILED DESCRIPTION

[0085] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0086] In the description of the present invention, it is necessary to understand that the terms "upper", "lower", "front", "back", "left", "right", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0087] Embodiment: The surface strengthening treatment process of the finishing roller by supersonic spraying comprises the following steps:

[0088] 1. Inspection: Check the appearance of the roller. If there are no bumps, scratches, cracks, pits, etc., proceed to the next process;

[0089] 2. Surface purification: Use acetone to thoroughly remove the oil, paint, oxides, etc. attached to the spray surface, and wipe and clean it. The roller surface should show a fresh metal surface. Except for the spray surface, the journal part should be cleaned with a shovel, kerosene, etc. and wiped clean with a rag;

[0090] 3. Dehumidification: Bake the roller surface to remove the moisture adsorbed on the roller surface and the rust on the roller surface until there is no water mark.

[0091] 4. Shot peening:

[0092] 1)2) The sandblasting material is white corundum sand: 80 mesh, the sandblasting distance is between 120 and 150 mm, the sandblasting angle is between 75° and 90°, and the air pressure is 0.6 to 0.7 MPa;

[0093] 3) The roughness of the workpiece surface after sandblasting should not exceed Ra: 3.2um (detected by roughness sample block); or visually observe the sandblasting surface from all angles under strong light with the naked eye, and it is qualified if it is grayish white, the roller surface is uniform, and there is no reflective bright spot;

[0094] 4) After sandblasting, orderly lines are formed on the roller surface. After spraying, orderly lines are formed on the roller surface. The orderly lines are grid lines formed by two sets of spiral sandblasting paths with different rotation directions, or are composed of several sandblasting areas. The sandblasting paths of two adjacent sandblasting areas are axial and circumferential respectively. For example:

[0095] One-shot sandblasting

[0096] Fix two templates on the surface of the roller, and make the right end faces of the two templates flush with the right end faces of the roller section that needs to be sprayed, rotate the roller manually, and use a sandblasting gun to blast along the spiral gap between the two templates, and the roughness is controlled between Ra5.5 and Ra6.5; sandblast a total of n times according to the above method, n = the number of equally divided sections of the circumference of the roller section that needs to be sprayed;

[0097] Secondary sandblasting

[0098] Turn over the two templates and fix them on the surface of the roller that has been sandblasted once, and make the left end faces of the two templates flush with the left end faces of the roller section that needs to be sprayed. Manually rotate the roller, and the sandblasting gun sandblasts along the spiral gap between the two templates. The roughness is controlled between Ra5.5 and Ra6.5. Sandblast a total of n times according to the above method, n = the number of equally divided sections of the roller section that needs to be sprayed;

[0099] Several left spiral lines and several right spiral lines are sandblasted, that is, a diamond pattern is sandblasted on the approximate vertical stripe pattern, and the roughness is controlled at Ra5.5-Ra6.5. Several patterns in the present invention are combined together to form a honeycomb basic structure, so that after supersonic spraying, the bonding strength between the coating and the substrate is greatly enhanced, and a strong anti-wear effect can be achieved. Therefore, the present invention solves the problem that the surface of the roller repaired now is not wear-resistant, and a supersonic spraying layer with high bonding strength and super wear resistance can be obtained, thereby extending the service life of the roller and reducing production costs.

[0100] The entire surface of the pre-sprayed roller is sandblasted once, and then the diamond pattern is sandblasted on this basis, so the surface hardness of the entire pre-sprayed roller is uniform; while the existing sandblasting technology does not form a pattern skeleton and cannot make the spray layer have sufficient wear resistance, which will lead to local wear and some parts are not worn, but the entire roller does need to be repaired, which greatly wastes time and materials. At the same time, when the outermost diamond pattern of the present invention is subjected to rolling impact force, the impact force will be dispersed to the surroundings along the edge of the diamond, thereby reducing the impact force and extending the overall service life of the roller.

[0101] 5. Preheating before spraying: The spraying surface should be preheated before powder is sent to spraying. The preheating temperature is generally controlled at around 50℃~60℃.

[0102] 6. Spraying: JP5000 equipment is used for spraying, spray gun distance: 280mm, gun moving speed: 200mm, rotation speed: 30r / min, powder feeding rate: 23g / min. The spraying parameters are as follows:

[0103]

[0104]

[0105] The composition of the primer layer includes Ni: 16, Cr: 4, Co: 15, Mo: 3 by weight, and the balance is Fe and trace impurities;

[0106] 1.27≤(Ni+Cr) / Co≤1.34, 0.18≤Mo / N i≤0.25.

[0107] The composition of the working layer includes Cr: 24.5, B: 4.8, Co: 68.7 and trace impurities by weight;

[0108] 0.33≤Cr / (B+Co)≤0.41.

[0109] Finally, a coating with a thickness of 50 to 60 μm is obtained;

[0110] 8. Post-spraying treatment: After spraying, the surface is polished with oilstone to make sure there is no graininess, surface roughness Ra<3.2, coating hardness>1200HV, and bonding strength≥70Mpa.

[0111] 9. Sealing: Use silicone resin to seal the sprayed surface.

[0112] 10. After sealing the holes, wrap the roller surface with plastic film.

[0113] Embodiment 2, which is different from Embodiment 1, is that the composition of the primer layer includes Ni: 18, Cr: 5, Co: 18, Mo: 4 by weight, and the balance is Fe and trace impurities;

[0114] 1.27≤(Ni+Cr) / Co≤1.34, 0.18≤Mo / N i≤0.25.

[0115] The composition of the working layer includes Cr: 26.8, B: 5.4, Co: 67.8 and trace impurities by weight;

[0116] 0.33≤Cr / (B+Co)≤0.41.

[0117] Embodiment 3, which is different from Embodiment 1, is that the composition of the primer layer includes Ni: 20, Cr: 6, Co: 21, Mo: 5 by weight, and the balance is Fe and trace impurities;

[0118] 1.27≤(Ni+Cr) / Co≤1.34, 0.18≤Mo / N i≤0.25.

[0119] The composition of the working layer includes Cr: 28.4, B: 5.8, Co: 65.8 and trace impurities by weight;

[0120] 0.33≤Cr / (B+Co)≤0.41.

[0121] The product performance indicators of Examples 1 to 3 are as follows:

[0122]

[0123] Embodiment 4, which is different from Embodiment 1, is that the composition of the primer layer includes Ni: 16, Cr: 4, Co: 15, Mo: 3, C: 0.5, V: 1.6, Nb: 1.6, and the balance is Fe and trace impurities;

[0124] 0.47≤Co / (Ni+Cr)≤0.75;

[0125] 0.041≤(V+Nb) / (Fe+C+Co)≤0.046;

[0126] 0.014≤C / (N i+Cr+Co)≤0.017;

[0127] 0.16≤Mo / N i≤0.24;

[0128] The composition of the working layer includes, by weight, Cr: 31.6, B: 4.3, Co: 61.5, W: 2.6, and trace impurities;

[0129] 0.36≤Cr / (B+Co)≤0.49;

[0130] 0.03≤B / (Cr+Co+W)≤0.07.

[0131] Example 5, which is different from Example 1, is that the composition of the primer layer includes Ni: 17, Cr: 5, Co: 14, Mo: 4, C: 0.6, V: 1.5, Nb: 1.5, and the balance is Fe and trace impurities;

[0132] 0.47≤Co / (Ni+Cr)≤0.75;

[0133] 0.041≤(V+Nb) / (Fe+C+Co)≤0.046;

[0134] 0.014≤C / (N i+Cr+Co)≤0.017;

[0135] 0.16≤Mo / N i≤0.24;

[0136] The composition of the working layer includes, by weight, Cr: 28.3, B: 4.8, Co: 63.6, W: 3.3, and trace impurities;

[0137] 0.36≤Cr / (B+Co)≤0.49;

[0138] 0.03≤B / (Cr+Co+W)≤0.07.

[0139] Example 6, which is different from Example 1, is that the composition of the primer layer includes Ni: 18, Cr: 5, Co: 11, Mo: 3, C: 0.6, V: 1.6, Nb: 1.6, and the balance is Fe and trace impurities;

[0140] 0.47≤Co / (Ni+Cr)≤0.75;

[0141] 0.041≤(V+Nb) / (Fe+C+Co)≤0.046;

[0142] 0.014≤C / (N i+Cr+Co)≤0.017;

[0143] 0.16≤Mo / N i≤0.24;

[0144] The composition of the working layer includes, by weight, Cr: 25.8, B: 5.6, Co: 64.5, W: 4.1, and trace impurities;

[0145] 0.36≤Cr / (B+Co)≤0.49;

[0146] 0.03≤B / (Cr+Co+W)≤0.07.

[0147] The product performance indicators of Examples 4 to 6 are as follows:

[0148]

[0149] In order to increase the number of times the finishing high-speed steel rolls are used, reduce roll consumption, and meet the rolling plans of pickled plates, automotive panels and other steel types with thin specifications and high surface quality requirements, combined with the company's requirements for reducing consumption, improving quality and increasing efficiency, through full communication, the high-speed steel finishing roll surface spraying technology developed by our company was tried out on the F2 stand of the 1580 line of the Fourth Steel Rolling Plant of a certain company. The usage data is as follows

[0150]

[0151]

[0152] The surface strengthening treatment process of the finishing roller by supersonic spraying includes the following steps:

[0153] Surface purification:

[0154] Clean the sprayed surface with acetone until the roller surface reveals a fresh metal surface, then dry it until there is no water mark on the surface;

[0155] Surface roughening - roughening path spraying:

[0156] A grid groove structure is formed on the roller surface by turning, wherein the grid groove structure includes staggered sinusoidal grooves 1 and sine grooves 2, two groups of intersection nodes are provided between adjacent sinusoidal grooves 1 and sine grooves 2, and the depth of the sinusoidal groove 1 is greater than the depth of the sinusoidal groove 2;

[0157] Sine grooves are formed in the forward direction and roughening path spraying is completed in the reverse direction, or sinusoidal grooves are formed in the reverse direction and roughening path spraying is completed in the forward direction. The front side of the roughening path spraying point in the spraying direction is preheated, and the preheating temperature is controlled at 50-60°C;

[0158] Preheating before spraying:

[0159] Before spraying, preheat the spray surface and control the preheating temperature at 50℃~60℃;

[0160] Spraying:

[0161] Spray gun distance: 250-300mm, gun moving speed: 150-300mm, rotation speed: 25-40r / min, powder feeding rate: 20-30g / min, first spray the raw material powder of the primer layer as described above on the roller surface, then spray the raw material powder of the working layer as described above on the surface of the primer layer to form a composite coating on the roller surface, and the coating thickness is 50-60um;

[0162] Post-spraying treatment:

[0163] After the surface is sprayed, it is immediately polished with an oil stone to ensure that there is no granularity, the surface roughness Ra is less than 3.2, the coating hardness is greater than 1200HV, and the bonding strength is ≥70Mpa.

[0164] like Figures 1 to 7 As shown, the surface roughening-roughening path spraying step adopts an integrated molding device, which includes a clamping mechanism 12 and a frame 13. The clamping mechanism 12 is equipped with a rotating spindle, which can drive the clamping mechanism 12 and the finishing roller to rotate. A slide rail 131 is arranged at the bottom of the frame 13, and a servo motor 132 is installed on the slide rail 131. The servo motor 132 drives the frame 13 to move along the length direction of the slide rail 131.

[0165] like Figure 7As shown, a reciprocating screw 15 and a driving motor 14 are installed on the frame 13. The driving motor 14 is installed on the frame 13 and is suitable for driving the reciprocating screw 15 installed on the frame 13 to rotate. The reciprocating screw 15 is matched with a driving block 16. The driving block 16 is suitable for lateral reciprocating motion relative to the frame 13. A plurality of sliders 18 are installed on the frame 13. A driven ring 17 with a notch is installed on the inner side of the plurality of sliders 18. The notch is suitable for the clamping mechanism 12 to pass freely. The driven ring 17 and the driving block 16 are meshed with teeth. A switching structure, a coarsening structure and a spraying structure are installed on the driven ring 17. The switching structure is suitable for reciprocatingly switching the coarsening structure and the spraying structure to be in a working state.

[0166] like Figures 4 to 6 As shown, the switching mechanism includes a switching frame 19, which is rotatably mounted on the driven ring 17 via an articulated seat 111, and an angle limiting portion 110 is installed between the switching frame 19 and the articulated seat 111. The switching frame 19 completes the reciprocating angle switching between the angle limiting portion 110 and the articulated seat 111. A blocking structure 112 is hooped on the shaft head of the roller body. The blocking structure 112 includes multiple single parts that are installed on the stepped shaft of the roller body through a steel belt hoop. The blocking structure 112 is suitable for unidirectionally blocking the corresponding switching frame 19 from moving in the opposite direction and completing the angle switching through the angle limiting portion 110. Figure 8 As shown, the monomer structure of the blocking structure 112 is a unidirectional rotating structure, for example, the main body 1121 and the blocking body 1122 rotatably mounted on the top of the main body, a torsion spring (not shown) is installed at the rotation node of the two, and a limit plate 1123 is installed on the top of the main body 1121 to limit the reverse deflection angle of the blocking body 1122 after reset, that is, the blocking body 1122 remains in a vertical state after reset. Figure 6 As shown, the angle limiting part 110 includes a guide groove 1101 arranged on the hinge seat 111 and positioning grooves located at both ends of the guide groove 1101 (not shown in the figure), and an elastic positioning pin 1102 installed on the switching frame 19, and the elastic positioning pin 1102 is suitable for rotating along the guide groove 1101 and being adapted and fixed in the positioning groove. When the blocking structure 112 hinders the switching frame 19, it can release the positioning groove and the elastic positioning pin 1102 so that it rotates to another positioning groove to complete the angle limitation.

[0167] like Figure 4 , Figure 5 and Figure 8As shown, the switching frame 19 is in the middle position to facilitate the understanding of the present solution by those skilled in the art, and the switching frame 19 cannot be specifically stabilized in this position during the whole process, and the locating grooves at the end points of the guide groove 1101 are used to limit the stability of the switching frame 19. The coating structure includes an adjustment frame 113 and a sprayer, and the adjustment frame 113 is suitable for selectively adjusting the position relative to the switching frame 19, and the sprayer is installed on the adjustment frame 113. The adjustment frame 113 is linearly adjustable relative to the switching frame 19, and a pusher ( Figure 5 The top position of the sprayer may be a cylinder, which drives the adjustment frame 113 to selectively adjust the position. Two powder pipes ( Figure 5 The two powder tubes are respectively suitable for powder delivery processing of powder one and powder two.

[0168] like Figure 5 and Figure 8 As shown, the roughening structure includes a driver 115 and a tool holder 114 mounted on the switching frame 19. The output end of the driver 115 is connected to the tool holder 114 via a worm gear, and the tool holder 114 is rotatably mounted on the switching frame 19. The driver 115 adopts a servo motor, which can adjust the travel angle of the tool holder 114 in time. A turning tool is installed on the tool holder 114 for spiral roughening of the roller surface.

[0169] The surface roughening-roughening path spraying treatment steps are as follows:

[0170] The finishing roller is hoisted and fixed by a clamping mechanism 12, and the clamping mechanism 12 is equipped with a rotating spindle, which can drive the clamping mechanism 12 and the finishing roller to rotate;

[0171] A blocking structure 112 is hooped on the roller shaft head, and the servo motor 132 drives the frame 13 to move along the slide rail 131 to the surface roughening-roughening path spraying to the working station. Under the action of the switching frame 19, the blocking structure 112, and the angle limiting part 110, the roughening structure is in a working state, and the driving motor 14 drives the reciprocating screw 15 to rotate and drives the slider 18 thereon to reciprocate, thereby driving the driven ring 17 to reciprocate and deflect, and the driver 115 on the roughening structure drives the tool holder 114 to deflect in time, and at the same time, the servo motor 132 drives the frame 13 to move along the axis direction of the finishing roller, and finally a sinusoidal groove 1 is processed on the roller surface, such as Fig. 9 As shown, the switching frame 19 passes through the blocking structure 112 without changing its angle. After completely passing through, as shown in FIG. Fig.10As shown, the servo motor 132 works in the reverse direction, the switching frame 19 completes the angle switching under the blocking effect of the blocking structure 112, and completes the restriction through the angle limiting part 110, the spraying structure is in the working state, the supersonic spraying structure and one of the powder material pipes work, and the powder material of the base layer is sprayed along the sinusoidal groove 1 to obtain the groove coating 1;

[0172] like Fig.10 As shown, when the switching frame 19 passes through the blocking structure 112 at the other end, the clamping mechanism 12 drives the finishing roller to rotate at a reasonable angle, such as Fig. 9 As shown, the servo motor 132 works in the reverse direction again, the switching frame 19 completes the angle switching under the action of the blocking structure 112, and completes the restriction through the angle limiting part 110, the coarsening structure is in working state, and the driver 115 on the coarsening structure drives the tool holder 114 to deflect in time, and finally a sinusoidal groove 2 is processed on the roller surface. After the switching frame 19 passes through the blocking structure 112, the servo motor 132 works in the reverse direction again, the switching frame 19 completes the angle switching under the action of the blocking structure 112, and completes the restriction through the angle limiting part 110, the supersonic spraying structure and one of the powder tubes work, and the powder for the base layer is sprayed along the coarse sinusoidal groove 2 to obtain the groove coating 2; preheating is required along the coarsening path spraying process, and arc preheating or laser preheating can be used.

[0173] Remove the blocking structure 112, the rotating spindle of the clamping mechanism 12 works, the spraying structure is still in working state, and the other powder pipe is opened to work together with the supersonic spraying structure. By adjusting the position of the adjusting frame 113 and the powder feeding position and direction of the working layer, the spraying operation of the working layer is carried out until it is completed, and the roller body can be removed after grinding with an oilstone.

[0174] The powder raw material sprayed on the roughening path has the same composition and ratio as the powder raw material of the base layer.

[0175] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. The replacement may be a replacement of a part of the structure, device, method step, or a complete technical solution. The spraying structure is in an unsprayed state when spraying outside the side end of the roller body. Any equivalent replacement or change according to the technical solution and inventive concept of the present invention shall be covered within the protection scope of the present invention.

Claims

1. Finishing roller supersonic spraying surface strengthening coating, It is characterized in that Including base layer and working layer; The components of the primer layer include Ni: 16-18, Cr: 4-6, Co: 11-22, Mo: 2-4, C: 0.4-0.8, V: 1.0-2.0, Nb: 1.0-2.0, and the balance is Fe and trace impurities; 0.45≤Co / (Ni+Cr)≤0.77; 0.036≤(V+Nb) / (Fe+C+Co)≤0.048; 0.011≤C / (Ni+Cr+Co)≤0.019; 0.14≤Mo / Ni≤0.31; The composition of the working layer includes, by weight, Cr: 20-35, B: 4.1-6.2, Co: 11-65, W: 2-5, and trace impurities; 0.31≤Cr / (B+Co)≤0.51; 0.01≤B / (Cr+Co+W)≤0.

09.

2. The finishing roll supersonic spraying surface strengthening coating according to claim 1, It is characterized in that The components of the primer layer include, by weight, Ni: 16-18, Cr: 4-6, Co: 11-22, Mo: 2-4, C: 0.4-0.8, V: 1.0-2.0, Nb: 1.0-2.0, and the balance is Fe and trace impurities; 0.47≤Co / (Ni+Cr)≤0.75; 0.041≤(V+Nb) / (Fe+C+Co)≤0.046; 0.014≤C / (Ni+Cr+Co)≤0.017; 0.16≤Mo / Ni≤0.24; The composition of the working layer includes, by weight, Cr: 20-35, B: 4.1-6.2, Co: 11-65, W: 2-5, and trace impurities; 0.36≤Cr / (B+Co)≤0.49; 0.03≤B / (Cr+Co+W)≤0.07.