Method for improving PVD target material utilization rate and PVD equipment

By installing a thickness gauge in the PVD equipment to monitor the target thickness in real time and adjust the sputtering power, the problem of inconsistent target utilization was solved, achieving efficient utilization of the target and cost savings.

CN118932302APending Publication Date: 2024-11-12RISEN ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411142343.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Inconsistent target utilization during PVD coating process leads to waste due to incomplete use of the target material, increasing costs.

Method used

A thickness gauge is installed on each target to monitor the target thickness in real time. The sputtering power is set according to the minimum thickness value, the total coating power is adjusted, the target utilization rate is controlled to ensure consistency, and the target is not fully used or is penetrated.

Benefits of technology

This improved the utilization rate of the target material, avoided waste, reduced production costs, and ensured the stability of battery efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932302A_ABST
    Figure CN118932302A_ABST
Patent Text Reader

Abstract

The embodiment of the invention provides a method for improving the utilization rate of a PVD target material and PVD equipment, and relates to the technical field of solar cell manufacturing. The method for improving the PVD target material utilization rate is used for conducting upper film coating and lower film coating on the surface of a battery substrate and comprises the steps that thickness detectors are installed in a plurality of first areas on each target material, and the thickness detectors are used for monitoring the thickness of the target materials in real time; obtaining thickness information output by a plurality of thickness detectors on each target material, and obtaining the minimum thickness value of each target material according to the thickness information of each target material; the sputtering power corresponding to each target material is set according to the minimum thickness value of each target material; and correspondingly performing magnetron sputtering according to the sputtering power of all the target materials. Whether the target material can be punched or not can be determined by obtaining the minimum thickness value of the target material, and the utilization rate of the target material is improved to the maximum extent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solar cell manufacturing, and in particular to a method for improving the utilization rate of PVD target materials and a PVD device. Background Art

[0002] At present, PVD coating is one of the main technologies for preparing thin film materials. Vacuum evaporation coating and magnetron sputtering coating are two widely used PVD coating methods. Vacuum evaporation coating is a technology that uses an evaporator to heat the evaporation material under vacuum conditions to vaporize it, and the evaporation particle flow is directly shot to the substrate and deposited on the substrate to form a solid film. Magnetron sputtering coating is a technology that forms a target material into a plasma state, so that positively charged gas ions collide with the target material, and metal atoms fly to form a metal film on the surface of the substrate. When PVD equipment uses magnetron sputtering to coat, due to the inconsistency of each target material, magnetic rod, target position in the chamber, and chamber atmosphere, the deposition rate of each target material is inconsistent, the target material life is inconsistent, and the target material utilization rate is inconsistent. In addition, when the target material is offline after the film formation is completed, it is easy for some targets to not be completely used up, resulting in a low utilization rate of some targets, waste of targets and increased costs.

[0003] Therefore, in the prior art, there is a technical problem that the target material is easily punctured or the target material is not completely used up during the coating process, resulting in an uneven overall utilization rate of the target material. Summary of the invention

[0004] The present invention provides a method for improving the utilization rate of PVD target materials and a PVD device, which can detect the minimum thickness of each target material, improve the utilization rate of the target material, make the utilization rate of each target material basically consistent, and reduce the cost.

[0005] The embodiments of the present invention can be implemented as follows:

[0006] An embodiment of the present invention provides a method for improving the utilization rate of a PVD target material, which is used for performing upper coating and lower coating on the surface of a battery substrate. The method for improving the utilization rate of a PVD target material includes:

[0007] A thickness detector is installed on a plurality of first regions on each target material, wherein the thickness detector is used to monitor the thickness of the target material in real time and output thickness information characterizing the target material;

[0008] Obtaining thickness information output by a plurality of thickness detectors on each target material, and obtaining a minimum thickness value of each target material according to the thickness information of each target material;

[0009] The sputtering power corresponding to each target is set according to the minimum thickness value of each target.

[0010] Optionally, the method for improving the utilization rate of the PVD target further includes:

[0011] When the minimum thickness difference exceeds the preset difference, the total power of the upper coating or the total power of the lower coating is adjusted, wherein the minimum thickness difference is:

[0012] The difference between the minimum value of the minimum thickness values ​​of all the target materials used for the upper coating and the minimum value of the minimum thickness values ​​of all the target materials used for the lower coating.

[0013] Optionally, the step of setting the sputtering power corresponding to each target material according to the minimum thickness value of each target material includes:

[0014] The sputtering power of each target is determined according to the sputtering power calculation formula, which is:

[0015] Sputtering power = minimum thickness value / (sum of the minimum thickness values ​​of each target material used for coating) x total power; or,

[0016] Sputtering power = minimum thickness value / (sum of the minimum thickness values ​​of each target material used for the lower coating) x total power.

[0017] Optionally, the method for improving the utilization rate of the PVD target further includes:

[0018] When the minimum thickness value of any of the target materials is lower than the set thickness value, the control machine sends out an alarm and obtains the remaining sputtering power of the target material according to the minimum thickness value.

[0019] Optionally, the method for improving the utilization rate of the PVD target further includes:

[0020] After the machine issues an alarm, the time to stop and change the target is obtained based on the remaining sputtering power of the target material.

[0021] Optionally, the method for improving the utilization rate of the PVD target further includes:

[0022] Compare the minimum thickness values ​​of each target material used for upper coating to obtain the upper coating target material thickness difference, and when the upper coating target material thickness difference exceeds the upper coating target material thickness preset difference, the control machine sends out an alarm; or,

[0023] The minimum thickness value of each target material used for the lower coating is compared to obtain the thickness difference of the lower coating target material. When the thickness difference of the lower coating target material exceeds the preset thickness difference of the lower coating target material, the control machine sends out an alarm.

[0024] Optionally, the method for improving the utilization rate of the PVD target further includes:

[0025] After the machine issues an alarm, the sputtering power of the target is automatically or manually adjusted according to the minimum thickness of the target, and the hydrogen and oxygen amounts of the PVD equipment are adjusted synchronously.

[0026] Optionally, a thickness detector is installed on each of the first regions of each target material, wherein the thickness detector is used to monitor the thickness of the target material in real time, and the step of outputting information characterizing the thickness of the target material includes:

[0027] In the case where the target is sputtered from above, the thickness detector is installed at the bottom of the target; or,

[0028] When the target is sputtered downward, the thickness detector is installed on the upper part of the target.

[0029] Optionally, the first area includes at least an operating end and a pump end of the target material, and a thickness detector is installed on each of the first areas on each target material, wherein the thickness detector is used to monitor the thickness of the target material in real time, and the step of outputting information characterizing the thickness of the target material further includes:

[0030] A non-contact thickness detector is installed at the operating end and the pump end of the target material respectively.

[0031] An embodiment of the present invention further provides a PVD device, which is implemented by using a method for improving the utilization rate of PVD target materials.

[0032] The beneficial effects of the method for improving the utilization rate of PVD target and the PVD equipment according to the embodiment of the present invention include, for example:

[0033] The method for improving the utilization rate of PVD target materials is used for performing upper and lower coating on the surface of a battery substrate, and the method for improving the utilization rate of PVD target materials comprises: installing thickness detectors on several first areas on each target material, wherein the thickness detectors are used to monitor the thickness of the target material in real time and output information characterizing the thickness of the target material; obtaining thickness information output by several thickness detectors on each target material, and obtaining the minimum thickness value of each target material according to the thickness information of each target material; and setting the sputtering power corresponding to each target material according to the minimum thickness value of each target material. When in use, since several first areas on the target material are areas with the smallest target material thickness, thickness detectors are installed in several first areas on the target material to monitor the minimum thickness of the target material in real time, thereby obtaining the minimum thickness value of the target material, thereby clarifying whether the target material can be penetrated, avoiding the impact on battery efficiency, and avoiding the phenomenon of unutilized target material, thereby maximizing the utilization rate of the target material, and the sputtering power corresponding to each target material can be set according to the minimum thickness value of each target material, and then magnetron sputtering is performed accordingly, so that the minimum thickness of each target material is basically the same, thereby making the utilization rate of each target material basically the same.

[0034] The PVD equipment is realized by using a method to improve the utilization rate of PVD target materials, which can maximize the utilization rate of target materials while avoiding affecting battery efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0036] Figure 1 A schematic diagram of the installation of the thickness detector and the target material provided in this embodiment;

[0037] Figure 2 A flow chart of the method for improving PVD target utilization provided in this embodiment.

[0038] Icon: 10-target material; 20-thickness tester. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0040] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.

[0042] In the description of the present invention, it should be noted that if the terms "upper", "lower", "inside", "outside", etc. appear to indicate an orientation or position relationship, they are based on the orientation or position relationship shown in the accompanying drawings, or are the orientation or position relationship in which the product of the invention is usually placed when used. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0043] In addition, the terms “first”, “second”, etc., if used, are merely used to distinguish between the descriptions and should not be understood as indicating or implying relative importance.

[0044] It should be noted that, in the absence of conflict, the features in the embodiments of the present invention may be combined with each other.

[0045] At present, PVD coating is one of the main technologies for preparing thin film materials. Vacuum evaporation coating and magnetron sputtering coating are two widely used PVD coating methods. Vacuum evaporation coating is a technology that uses an evaporator to heat the evaporation material under vacuum conditions to vaporize it, and the evaporation particle flow is directly shot to the substrate and deposited on the substrate to form a solid film. Magnetron sputtering coating is a technology that forms a target material into a plasma state, so that positively charged gas ions collide with the target material, and metal atoms fly to form a metal film on the surface of the substrate. When PVD equipment uses magnetron sputtering to coat, due to the inconsistency of each target material, magnetic rod, target position in the chamber, and chamber atmosphere, the deposition rate of each target material is inconsistent, the target material life is inconsistent, and the target material utilization rate is inconsistent. In addition, when the target material is offline after the film formation is completed, it is easy for some targets to not be completely used up, resulting in a low utilization rate of some targets, waste of targets and increased costs.

[0046] At present, the existing technology mainly uses the kilowatt life test value of the target material as the basis for the target material to go offline. Since the observation window of the PVD target is coated with a film layer at the end of the target material, the state of the target material cannot be well observed. Therefore, if the empirical value of the target material life is used, it is impossible to determine whether the target material is penetrated, resulting in low target material utilization when it is not penetrated, and the battery efficiency is affected when it is severely penetrated.

[0047] Based on this, this embodiment provides a PVD device, which is implemented by a method of improving the utilization rate of PVD target materials, and the surface of the battery substrate is coated with an upper film and a lower film by the method of improving the utilization rate of the PVD target materials.

[0048] Please refer to Figure 1-Figure 2 , the method for improving the utilization rate of PVD target material includes:

[0049] S1: A thickness detector 20 is installed at a plurality of first regions on each target material 10 , wherein the thickness detector 20 is used to monitor the thickness of the target material 10 in real time and output information representing the thickness of the target material 10 .

[0050] Specifically, when the target 10 is sputtered from above, the thickness detector 20 is installed at the bottom of the target 10 ; or when the target 10 is sputtered from below, the thickness detector 20 is installed at the top of the target 10 .

[0051] In the present embodiment, the first region at least includes the two ends of the target material 10, namely the operating end and the pump end. During the sputtering coating process of the target material 10, the etching speed at the two ends of the target material 10 is faster than that at other positions of the target material 10, and the thickness at the two ends of the target material 10 is thinner than that at other positions of the target material 10. Therefore, the thickness detector 20 is set at the first region of the target material 10, namely, the two ends of the target material 10. Of course, the first region can also include other positions on the target material 10 except the two ends. Specifically, a non-contact thickness detector is installed at the operating end and the pump end of the target material 10 respectively. The non-contact thickness detector can detect the thickness of the target material 10 in real time and transmit the information characterizing the thickness of the target material 10 to the machine host computer for display. Among them, the non-contact thickness detector adopts an X-ray fluorescence spectrometry thickness gauge or a non-contact ultrasonic thickness gauge.

[0052] S2: Obtain thickness information output by a plurality of thickness detectors 20 on each target material 10 , and obtain a minimum thickness value of each target material 10 according to the thickness information of each target material 10 .

[0053] It should be noted that when an X-ray fluorescence spectrometry thickness gauge is used to detect the thickness of the target material 10, the primary X-rays generated by the X-ray tube are irradiated onto the target material 10, which will excite the atoms of the elements in the target material 10, causing their inner electrons to be expelled to form holes. At this time, the outer electrons will jump to fill the inner holes, thereby releasing characteristic X-rays (fluorescent X-rays) with specific energy. The intensity of the characteristic X-rays is proportional to the content of the element; when measuring the thickness of the target material 10, the X-rays will be attenuated due to the absorption of the target material 10 during the process of passing through the target material 10. By measuring the intensity of the emitted X-ray fluorescence, combined with known parameters such as the absorption coefficient of the element to X-rays, a mathematical model between intensity and thickness can be established, thereby calculating the thickness of the target material 10.

[0054] S3: setting the sputtering power corresponding to each target material 10 according to the minimum thickness value of each target material 10 .

[0055] Specifically, when the PVD equipment performs upper and lower coating on the battery substrate, there are multiple coating target positions and target materials 10, respectively, and a fixed value of the total power of the upper coating or the total power of the lower coating is set according to the film thickness of the battery substrate. In other words, the sum of the sputtering powers of all the target materials 10 used for the upper coating is a fixed value, and the sum of the sputtering powers of all the target materials 10 used for the lower coating is also a fixed value. The smaller the thickness of the target material 10, the lower the set sputtering power, and the lower the etching rate. When the total power is fixed, the sputtering power of each target material 10 is adjusted according to the minimum thickness value of each target material 10, so as to balance the utilization rate of each target material 10 in magnetron sputtering, so that the utilization rate of each target material 10 can be maximized.

[0056] Specifically, the sputtering power of each target material 10 needs to be determined according to the sputtering power calculation formula, and the sputtering power calculation formula is:

[0057] Sputtering power = minimum thickness value / (sum of minimum thickness values ​​of each target material 10 used for coating) x total power; or,

[0058] Sputtering power = minimum thickness value / (sum of minimum thickness values ​​of each target material 10 used for lower coating) x total power.

[0059] S4: When the minimum thickness difference exceeds the preset difference, adjust the total power of the upper coating or the total power of the lower coating, wherein the minimum thickness difference is:

[0060] The difference between the minimum value of the minimum thickness values ​​of all the targets 10 used for the upper coating and the minimum value of the minimum thickness values ​​of all the targets 10 used for the lower coating.

[0061] Specifically, when the minimum thickness difference exceeds the preset difference, the total power of the upper coating or the total power of the lower coating is too large, and the target material 10 is easily penetrated. Therefore, it is necessary to reduce the total power of the upper coating or the total power of the lower coating according to the actual situation, so that the thickness of the target material 10 used for the upper coating and the thickness of the target material 10 used for the lower coating are basically the same, thereby ensuring that the overall thickness of all target materials 10 is basically the same, so that all target materials 10 can basically achieve maximum utilization and save costs.

[0062] In this embodiment, the preset difference refers to a minimum thickness difference artificially set according to actual coating conditions.

[0063] S5: When the minimum thickness value of any target material 10 is lower than the set thickness value, the control machine sends out an alarm and obtains the remaining sputtering power according to the minimum thickness value.

[0064] Specifically, the sputtering power corresponding to each target material 10 can be obtained according to the sputtering power calculation formula in step S3. As the coating work continues, each target material 10 has an accumulated power after use. The sputtering power corresponding to each target material 10 is compared with the accumulated power after use, and the difference obtained is the remaining sputtering power of each target material 10.

[0065] S6: After the machine sends out an alarm, the time for stopping the machine and changing the target is obtained according to the remaining sputtering power of the target material 10 .

[0066] Specifically, the remaining sputtering power of the target material 10 can be obtained according to step S5, and the remaining working time of the target material 10 can be estimated manually according to the obtained remaining sputtering power of the target material 10, and the target material 10 is stopped and replaced after the time is reached.

[0067] For example, according to the sputtering power calculation formula in step S3, the sputtering power corresponding to a target material 10 is 10KW. As the coating work progresses, the cumulative power of the target material 10 after use is 6KW. The sputtering power corresponding to the target material 10 is compared with the cumulative power after use, and the difference is 4KW, that is, the remaining sputtering power of the target material 10 is 4KW. According to the remaining sputtering power of the target material 10, it is estimated that the target material 10 can continue to work for 10s, and the target is stopped after 10s.

[0068] S7: Compare the minimum thickness values ​​of each target material 10 used for upper coating to obtain the upper coating target material thickness difference. When the upper coating target material thickness difference exceeds the upper coating target material thickness difference preset, the control machine sends out an alarm;

[0069] Or the minimum thickness value of each target material 10 used for the lower coating is compared to obtain the lower coating target material thickness difference. When the lower coating target material thickness difference exceeds the lower coating target material thickness preset difference, the control machine sends out an alarm.

[0070] S8: After the machine sends out an alarm, the sputtering power of the target material 10 is automatically or manually adjusted according to the minimum thickness value of the target material 10, and the hydrogen and oxygen amounts of the PVD equipment are adjusted synchronously.

[0071] In summary, an embodiment of the present invention provides a method and a PVD device for improving the utilization rate of PVD target materials. The method for improving the utilization rate of PVD target materials is used to perform upper and lower coating on the surface of a battery substrate. The method for improving the utilization rate of PVD target materials includes: a thickness detector 20 is installed in several first areas on each target material 10, wherein the thickness detector 20 is used to monitor the thickness of the target material 10 in real time and output information characterizing the thickness of the target material 10; the thickness information output by several thickness detectors 20 on each target material 10 is obtained, and the minimum thickness value of each target material 10 is obtained according to the thickness information of each target material 10; and the sputtering power corresponding to each target material 10 is set according to the minimum thickness value of each target material 10. When in use, since several first areas on the target material 10 are areas with the smallest thickness of the target material 10, the thickness detector 20 is installed in several first areas on the target material 10 to monitor the minimum thickness of the target material 10 in real time, thereby obtaining the minimum thickness value of the target material 10, thereby clarifying whether the target material 10 can be penetrated, avoiding the impact on the battery efficiency, and avoiding the phenomenon of unutilized target material 10, thereby maximizing the utilization rate of the target material 10, and the sputtering power corresponding to each target material 10 can be set according to the minimum thickness value of each target material 10, and then magnetron sputtering is performed accordingly, so that the minimum thickness of each target material 10 is basically the same, thereby making the utilization rate of each target material 10 basically the same.

[0072] The PVD device is implemented by using a method for improving the utilization rate of the PVD target material, which can maximize the utilization rate of the target material 10 while avoiding affecting the battery efficiency.

[0073] Example 1

[0074] In this embodiment, taking the target material 10 for upper coating as an example, the number of target materials 10 for upper coating is set to 8, and the total power of upper coating of the battery substrate is set to 81.6KW, that is, the sputtering power of each target material 10 should be 10.2KW, and thickness detectors 20 are installed in several first areas on each target material 10. The minimum thickness values ​​detected by each thickness detector 20 are 1.02mm, 1mm, 0.98mm, 0.97mm, 1.05mm, 1.09mm, 0.95mm and 0.99mm, respectively. The minimum thickness value of each target material 10 is substituted into the sputtering power calculation formula to determine the sputtering power of each target material 10, and the actual sputtering powers of each target material 10 are calculated to be 10.3KW, 10.1KW, 9.9KW, 9.8KW, 10.6KW, 11KW, 9.6KW and 10KW, respectively. After the actual sputtering power of each target material 10 is obtained, it is adjusted accordingly according to the actual sputtering power, and then each target material 10 performs sputtering work under the corresponding actual sputtering power.

[0075] Example 2

[0076] In this embodiment, taking the target material 10 for upper coating as an example, the number of target materials 10 for upper coating is set to 8, the total power of upper coating of the battery substrate is set to 81.6KW, the preset difference of the upper coating target material thickness of all target materials 10 for upper coating is set to 0.5mm, and thickness detectors 20 are installed in several first areas on each target material 10. The minimum thickness values ​​detected by each thickness detector 20 are 1.01mm, 0.84mm, 0.95mm, 0.91mm, 1.03mm, 1.09mm, 0.58mm and 0.79mm respectively. The above-mentioned minimum thickness values ​​are compared to obtain the upper coating target material thickness. The thickness difference is 0.51mm, and the obtained upper coating target thickness difference of 0.51mm exceeds the preset thickness difference of 0.5mm. At this time, the control machine issues an alarm. After receiving the alarm, the operator adjusts the process parameters according to the actual situation, and automatically or manually adjusts the sputtering power of each target 10 to 11.4KW, 9.5KW, 10.8KW, 10.3KW, 11.7KW, 12.4KW, 6.6KW and 9KW according to the thickness ratio, and synchronously adjusts the process hydrogen and oxygen amounts, which can reduce the process oxygen corresponding to the target 10 with a minimum thickness of 0.58mm by 4sccm and the hydrogen by 2sccm.

[0077] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.

Claims

1. A method for improving the utilization rate of PVD target materials, used for coating the surface of a battery substrate with upper and lower coatings, characterized in that: The method for improving the utilization rate of the PVD target comprises: A thickness detector (20) is installed on a plurality of first regions on each target material (10), wherein the thickness detector (20) is used to monitor the thickness of the target material (10) in real time and output thickness information characterizing the target material (10); Obtaining thickness information output by a plurality of thickness detectors (20) on each target material (10), and obtaining a minimum thickness value of each target material (10) based on the thickness information of each target material (10); The sputtering power corresponding to each target material (10) is set according to the minimum thickness value of each target material (10).

2. The method for improving the utilization rate of PVD target according to claim 1, characterized in that: The method for improving the utilization rate of the PVD target material further comprises: When the minimum thickness difference exceeds the preset difference, the total power of the upper coating or the total power of the lower coating is adjusted, wherein the minimum thickness difference is: The difference between the minimum value of the minimum thickness values ​​of all target materials (10) used for the upper coating and the minimum value of the minimum thickness values ​​of all target materials (10) used for the lower coating.

3. The method for improving the utilization rate of PVD target according to claim 1, characterized in that: The step of respectively setting the sputtering power corresponding to each target material (10) according to the minimum thickness value of each target material (10) comprises: The sputtering power of each target material (10) is determined according to a sputtering power calculation formula, wherein the sputtering power calculation formula is: Sputtering power = minimum thickness value / (sum of minimum thickness values ​​of each target material (10) used for coating) x total power; or, Sputtering power = minimum thickness value / (sum of minimum thickness values ​​of each target material (10) used for lower coating) x total power.

4. The method for improving the utilization rate of PVD target according to claim 1, characterized in that: The method for improving the utilization rate of the PVD target material further comprises: When the minimum thickness value of any one of the target materials (10) is lower than the set thickness value, the control machine sends out an alarm and obtains the remaining sputtering power of the target material (10) according to the minimum thickness value.

5. The method for improving the utilization rate of PVD target according to claim 4, characterized in that: The method for improving the utilization rate of the PVD target material further comprises: After the machine sends out an alarm, the time for stopping the machine and changing the target is obtained according to the remaining sputtering power of the target material (10).

6. The method for improving the utilization rate of PVD target according to claim 1 or 4, characterized in that: The method for improving the utilization rate of the PVD target material further comprises: Comparing the minimum thickness value of each target material (10) used for upper coating to obtain a thickness difference of the upper coating target material, and when the thickness difference of the upper coating target material exceeds a preset thickness difference of the upper coating target material, the control machine sends an alarm; or, The minimum thickness value of each target material (10) used for the lower coating is compared to obtain a lower coating target material thickness difference value, and when the lower coating target material thickness difference value exceeds a preset lower coating target material thickness difference value, the control machine sends out an alarm.

7. The method for improving the utilization rate of PVD target according to claim 6, characterized in that: The method for improving the utilization rate of the PVD target material further comprises: After the machine issues an alarm, the sputtering power of the target material (10) is automatically or manually adjusted according to the minimum thickness value of the target material (10), and the hydrogen and oxygen amounts of the PVD equipment are adjusted synchronously.

8. The method for improving the utilization rate of PVD target according to claim 1, characterized in that: The plurality of first regions on each target material (10) are each provided with a thickness detector (20), wherein the thickness detector (20) is used to monitor the thickness of the target material (10) in real time and output information characterizing the thickness of the target material (10), the steps comprising: When the target (10) is sputtered upward, the thickness detector (20) is installed at the bottom of the target (10); or, When the target material (10) is sputtered downward, the thickness detector (20) is installed on the upper part of the target material (10).

9. The method for improving the utilization rate of PVD target according to claim 1, characterized in that: The first area at least includes an operating end and a pump end of the target material (10), and each of the first areas on the target material (10) is equipped with a thickness detector (20), wherein the thickness detector (20) is used to monitor the thickness of the target material (10) in real time, and the step of outputting information characterizing the thickness of the target material (10) further includes: A non-contact thickness detector is installed at the operating end and the pump end of the target material (10), respectively.

10. A PVD device, characterized in that: This is achieved by using the method for improving the utilization rate of PVD target materials as described in any one of claims 1 to 9.