Ceramic coating for surface of aero-engine compressor and preparation method of ceramic coating

By adding an AlCrSi layer to the TiBN coating and forming an AlCrSiTiBN antioxidant coating, the problem of insufficient oxidation resistance and sudden drop in hardness of the compressor blade coating at high temperature is solved, and the high coating is achieved under 800°C Strength and high toughness significantly improve protection performance in high-temperature service environments.

CN118932305AActive Publication Date: 2024-11-12UNIV OF SCI & TECH BEIJING

Patent Information

Application Number
CN202410952955.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-12
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

The existing compressor blade coatings lack oxidation resistance in high temperature environments, resulting in deterioration of protective performance. The introduction of antioxidant elements will cause the coating hardness to drop sharply, making it difficult to have both high hardness and oxidation resistance.

Method used

A high-strength, tough, high-temperature oxidation-resistant ceramic coating for the surface of titanium alloy of aero engine compressor was designed. By adding an AlCrSi layer to the TiBN coating, a pure Ti transition layer was formed on the substrate by magnetron sputtering method and AlCrSiTiBN antioxidant coating ensures that the coating maintains high strength and toughness at high temperatures.

Benefits of technology

It effectively improves the oxidation resistance and hardness of the coating, avoids the problem of sudden hardness drop, and allows the coating to maintain high strength and high toughness under 800°C, significantly improving the protective performance in high-temperature service environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932305A_ABST
    Figure CN118932305A_ABST
Patent Text Reader

Abstract

The invention provides a high-toughness high-temperature-oxidation-resistant ceramic coating applied to the titanium alloy surface of an aero-engine compressor and a preparation method of the high-toughness high-temperature-oxidation-resistant ceramic coating, and relates to the field of coating preparation, and the preparation method comprises the steps that S1, a base body is pretreated and fixed to a substrate table; s2, the target materials are placed on the target positions respectively; s3, the substrate is subjected to bias cleaning through ionized inert gas; s4, a pure Ti transition layer with the thickness of 80-100 nm is sputtered on the surface of the base body; and S5, a layer of AlCrSiTiBN anti-oxidation coating is formed on the pure Ti transition layer. According to the coating disclosed by the invention, the problem that the coating is easy to oxidize and lose efficacy at high temperature is solved on the basis of keeping excellent mechanical properties, and a new thought is provided for application of the protective coating on the titanium alloy surface of the aero-engine compressor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of high-strength, tough, and high-temperature resistant protective coating preparation, and in particular to a high-strength, tough, and high-temperature oxidized ceramic coating applied to the surface of titanium alloy of an aero-engine compressor and a preparation method thereof. Background Art

[0002] With the continuous development of aviation engine and gas turbine technology and the continuous improvement of usage requirements, their operating temperatures are gradually increasing. The service environment of compressor blades is also tending to be high temperature, complex stress, and high corrosion. The blades need to be able to withstand oxidation, corrosion, high-speed airflow erosion, high-temperature creep and thermomechanical fatigue for a long time without failure. Preparing a suitable protective coating on the blades is an effective and feasible way.

[0003] The outlet temperature of domestic compressors is generally between 400℃ and 600℃, and the outlet temperature of advanced engines has exceeded 650℃. The main problem is high-temperature oxidation, and there is little research on the adaptability of compressor coatings in this temperature range. In addition, as its thrust-to-weight ratio continues to increase, it is expected that the outlet temperature of the fifth-generation aircraft engine compressor will reach about 800℃. In the harsh working environment of high temperature, high pressure and high speed, the performance of the protective coating will often deteriorate sharply and make the protective performance ineffective. Therefore, a coating with both excellent mechanical properties and high-temperature oxidation resistance is the guarantee of high-performance compressor blades, and improving its wear resistance, hardness and oxidation resistance is the key.

[0004] Previous research was mainly limited to binary and ternary nitride coatings. For example, TiBN is a ternary coating formed by adding the element B to TiN. The addition of B can refine the coating grains and significantly increase the hardness. According to previous studies, although the TiBN coating has good mechanical strength, its oxidation resistance is far from meeting the service requirements of the compressor, and the addition of elements with good oxidation resistance will cause the hardness of the coating to drop sharply. With the further increase in service temperature, higher requirements are also placed on the oxidation resistance of the protective coating. Therefore, it is urgent to develop a new system that combines hardness and oxidation resistance to adapt to more demanding service environments. Summary of the invention

[0005] In order to solve the deficiencies in the prior art, the present invention improves on the original TiBN coating and designs a new type of high-strength, tough, high-temperature oxidation-resistant ceramic coating for the surface of titanium alloy in aircraft engine compressors. While retaining the high hardness of the TiBN coating, the oxidation resistance of the TiBN coating is improved, avoiding the phenomenon of a sudden drop in the hardness of the coating due to the introduction of antioxidant elements in the past, thereby improving the problem of failure and degradation of the protective performance of traditional nitride coatings in high-temperature service environments. Specifically:

[0006] A method for preparing a ceramic coating on the surface of an aero-engine compressor, comprising:

[0007] Step S1, polishing the substrate, then washing it with an organic solvent and deionized water in sequence, fixing the dried substrate on a substrate table, and finally placing it in a chamber of a coating device;

[0008] Step S2, placing the AlCrSi target, the Ti target, and the TiB2 target on the target positions respectively;

[0009] Step S3: evacuate the chamber until the vacuum degree reaches 1.8×10 -3 Pa, then raise the chamber temperature to the deposition temperature of 300°C-400°C, introduce inert gas to adjust the chamber pressure to 1Pa, set the bias voltage of the substrate stage to -950V, and etch for 10-20min; this step uses ionized inert gas to bias clean the substrate;

[0010] Step S4, controlling the Ti target power between 400-480W, adjusting the flow rate of the inert gas Ar to stabilize the chamber pressure between 0.18-0.21Pa, and sputtering a layer of 80-100nm thick pure Ti transition layer on the surface of the substrate, the transition layer is mainly used to achieve adhesion between the substrate and the anti-oxidation coating to prevent stratification and shedding of the coating;

[0011] Step S5, further introduce inert gas and turn on the N2 flow controller switch, control the chamber pressure to 0.18-0.21Pa, set the substrate stage bias to -110V, the rotation speed to 23rpm, control the power of the AlCrSi target to 160 to 240W, the power of the TiB2 target to 65-85W, deposit at the deposition temperature for 2-3h, and form a layer of AlCrSiTiBN anti-oxidation coating on the pure Ti transition layer.

[0012] Preferably, in step S1, the organic solvent is selected from acetone and alcohol; and the cleaning method is selected from ultrasonic cleaning.

[0013] Preferably, in step S1, the substrate is selected from one of single crystal Si, single crystal Al2O3, and 304 stainless steel.

[0014] Preferably, in step S2, the AlCrSi target is placed on the RF target position, and the chemical composition ratio of Al, Cr, and Si in the target is 1:1:1; the Ti target and the TiB2 target are placed on the DC target position; the purity of the target material reaches 99.99%, and the target size is φ76.2×5 mm. Generally speaking, a metal target with good conductivity is placed on the target position of the DC target, and a material with poor conductivity is placed on the RF target. Generally speaking, the sputtering efficiency of the DC target is higher than that of the RF target.

[0015] Preferably, in step S3, the inert gas is selected from argon.

[0016] Preferably, in step S5, 30 sccm of Ar and 10 sccm of N2 are introduced in a ratio of 3:1 to stabilize the gas pressure at 0.18 Pa, and the power of the AlCrSi target is controlled at 200 W, and the power of the TiB2 target is controlled at 80 W, and deposition is performed at the deposition temperature for 3 hours.

[0017] Furthermore, the present invention also provides a ceramic coating, including a substrate, a pure Ti transition layer, and an AlCrSiTiBN anti-oxidation coating. The ceramic coating can resist oxidation at 800°C and maintain high strength and high toughness.

[0018] The beneficial effects brought about by the technical solution provided by the embodiment of the present invention include at least:

[0019] The present invention adopts a magnetron sputtering method to design a ceramic coating with a substrate, a pure Ti transition layer and an AlCrSiTiBN layer, so that the coating material has excellent characteristics of high strength, high toughness and high-temperature oxidation resistance. On the basis of maintaining the mechanical properties of the ceramic coating, it effectively solves the problem of easy oxidation failure of the coating at high temperature (it can still maintain high strength and high toughness at a high temperature of 800°C). BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0021] Figure 1 It is a schematic diagram of the internal structure of the chamber of the magnetron sputtering coating instrument of the present invention;

[0022] Figure 2 is a schematic diagram of the structure of the ceramic coating of the present invention;

[0023] FIG3( a) is a cross-sectional SEM morphology of the TiBN coating prepared in Comparative Example 1;

[0024] FIG3( b ) is a cross-sectional SEM morphology comparison diagram of the AlCrSiTiBN anti-oxidation coating prepared in Example 1;

[0025] FIG4( a ) is a cross-sectional SEM morphology of the TiBN coating prepared in Comparative Example 1 after oxidation at 400° C. for 10 h;

[0026] FIG4( b ) is a cross-sectional SEM morphology of the AlCrSiTiBN anti-oxidation coating prepared in Example 1 after oxidation at 400° C. for 10 h;

[0027] Figure 5 This is a comparison chart of the oxide film thickness generated by the coatings prepared under different preparation conditions and oxidized at 800℃ for 3h;

[0028] FIG6( a ) is a cross-sectional SEM image of the TiBN coating prepared in Comparative Example 1 after oxidation at 800° C. for 3 h;

[0029] FIG6( b ) is a cross-sectional SEM image of the AlCrSiTiBN anti-oxidation coating prepared in Example 1 after oxidation at 800° C. for 3 h;

[0030] Figure 7 This is a diagram of the mechanical properties of the AlCrSiTiBN anti-oxidation coating prepared in Example 2;

[0031] Among them: 1-AlCrSi RF target, 2-Ti DC target, 3-TiB2 DC target, 4-substrate stage, 5-AlCrSiTiBN anti-oxidation coating, 6-pure Ti transition layer, 7-substrate. DETAILED DESCRIPTION

[0032] The technical solution of the present invention is described below in conjunction with the accompanying drawings.

[0033] In the embodiments of the present invention, words such as "exemplarily" and "for example" are used to indicate examples, illustrations or explanations. Any embodiment or design described as "example" in the present invention should not be interpreted as being more preferred or more advantageous than other embodiments or designs. Specifically, the use of the word "example" is intended to present the concept in a specific way. In addition, in the embodiments of the present invention, the meaning expressed by "and / or" can be both, or it can be either of the two.

[0034] In the embodiments of the present invention, "image" and "picture" can sometimes be used interchangeably. It should be noted that when the difference between them is not emphasized, the meanings they want to express are the same. "of", "corresponding" and "corresponding" can sometimes be used interchangeably. It should be noted that when the difference between them is not emphasized, the meanings they want to express are the same.

[0035] In the embodiments of the present invention, sometimes a subscript such as W1 may be mistakenly written as a non-subscript such as W1. When the difference is not emphasized, the meanings to be expressed are consistent.

[0036] In order to make the technical problems, technical solutions and advantages to be solved by the present invention more clear, a detailed description will be given below with reference to the accompanying drawings and specific embodiments.

[0037] like Figure 1As shown, the internal structure of the chamber of the magnetron sputtering coating apparatus used in the present invention is shown in the figure, 1 represents the AlCrSi RF target position, 2 represents the Ti DC target position, 3 represents the TiB2 target DC target position, and 4 represents the substrate stage with adjustable rotation speed. By using the magnetron sputtering coating apparatus, a pure Ti transition layer is first plated on the substrate, and then a layer of AlCrSiTiBN is plated.

[0038] The ceramic coating structure prepared by the present invention is as follows Figure 2 As shown, 5 represents the AlCrSiTiBN anti-oxidation coating deposited on the top layer, 7 represents the substrate, and a transition layer 6 is arranged between the AlCrSiTiBN anti-oxidation coating 5 and the substrate 7. The transition layer 6 is a pure Ti coating with a thickness of 80 to 100 nm.

[0039] Example 1

[0040] With Al2O3 sheets as the matrix, the AlCrSiTiBN anti-oxidation coating is prepared by adopting the preparation process designed by the invention.

[0041] The atomic ratio of AlCrSi target is 1:1:1. AlCrSi target is placed in the RF target position, and Ti target and TiB2 target are placed in the DC target position. Their purity is 99.99%.

[0042] First, the substrate was polished, then ultrasonically cleaned with acetone, alcohol, and deionized water for 10 minutes in sequence, fixed on the substrate table after drying, and placed in the chamber of the coating instrument.

[0043] The chamber was evacuated to a vacuum degree of 1.8×10 -3 Pa, then heat the chamber to the deposition temperature of 400°C, introduce inert gas Ar to adjust the chamber pressure to 1Pa, set the bias voltage of the substrate stage to -950V, and etch for 10-20min; this step uses ionized inert gas to bias clean the substrate.

[0044] The Ti target power was controlled at 450 W, the flow rate of the inert gas Ar was adjusted to stabilize the chamber pressure between 0.18 and 0.21 Pa, and a pure Ti transition layer with a thickness of 80 to 100 nm was sputtered on the substrate surface.

[0045] Further introduce inert gas and turn on the N2 flow controller switch, introduce 10sccm of N2 and 30sccm of Ar to control the chamber pressure to 0.18-0.21Pa, set the substrate stage bias to -110V and the rotation speed to 23rpm, control the power of the AlCrSi target at 200W, and the power of the TiB2 target at 80W, and deposit at the deposition temperature for 3h to form a layer of AlCrSiTiBN anti-oxidation coating on the pure Ti transition layer.

[0046] Example 2

[0047] The difference from Example 1 is that the substrate is single crystal Si.

[0048] Comparative Example 1

[0049] With Al2O3 sheet as substrate, substrate pretreatment and ion etching process refer to Example 1, the difference between Example 1 and Example 1 is that only Ti target and TiB2 target are used during coating deposition. The comparative coating deposition process is: after ion etching for 10 minutes, the chamber pressure is controlled to 0.21Pa, the bias voltage is set to -110V, the substrate stage speed is 23rpm, the Ti target power is set to 450W, the TiB2 target power is set to 80W, and the deposition is carried out for 2-3 hours.

[0050] Comparative Example 2

[0051] The difference from Comparative Example 1 is that the substrate is single crystal Si.

[0052] Comparative Example 3

[0053] With Al2O3 sheet as substrate, AlCrSiTiBN anti-oxidation coating is prepared by the preparation process designed by the present invention. With Al2O3 sheet as substrate, substrate pretreatment and ion etching process refer to Example 1, the difference between it and Example 1 is that during coating deposition, the power of AlCrSi target is controlled at 160W. The comparative coating deposition process is: after 10 minutes of ion etching, the chamber pressure is controlled to 0.21Pa, the bias voltage is set to -110V, the substrate stage speed is 23rpm, the Ti target power is set to 450W, the TiB2 target power is set to 80W, the AlCrSi target power is set to 160W, and the deposition is 3h.

[0054] Comparative Example 4

[0055] With Al2O3 sheet as substrate, AlCrSiTiBN anti-oxidation coating is prepared by the preparation process designed by the present invention. With Al2O3 sheet as substrate, substrate pretreatment and ion etching process refer to Example 1, the difference between it and Example 1 is that during coating deposition, the power of AlCrSi target is controlled at 240W. The comparative coating deposition process is: after 10 minutes of ion etching, the chamber pressure is controlled to 0.21Pa, the bias voltage is set to -110V, the substrate stage speed is 23rpm, the Ti target power is set to 450W, the TiB2 target power is set to 80W, the AlCrSi target power is set to 240W, and the deposition is carried out for 3 hours. For the samples prepared in the embodiment and the comparative example, the cross-sectional morphology of the coating and the oxide layer is observed and analyzed using a scanning electron microscope; the coating on the Al2O3 substrate is subjected to oxidation experiments at 400℃ for 10 hours and 800℃ for 3 hours using a muffle furnace; the hardness of the coating on the Si substrate is measured using nanoindentation.

[0056] Figure 3(a) is a cross-sectional SEM morphology of the TiBN coating of Comparative Example 1; Figure 3(b) is a cross-sectional SEM morphology of the AlCrSiTiBN anti-oxidation coating prepared in Example 1. As can be seen from Figure 3(a), the TiBN coating is a columnar crystal structure, which provides a channel for the diffusion of oxygen along the grain boundary. As can be seen from Figure 3(b), after the AlCrSi element is doped, the columnar crystal structure of the coating disappears, becoming more dense and uniform. The coating thickness is relatively thicker with the same deposition time, and it is well bonded to the substrate.

[0057] Figure 4(a) is a cross-sectional SEM morphology of the TiBN coating prepared in Comparative Example 1 after oxidation at 400°C for 10 hours; Figure 4(b) is a cross-sectional SEM morphology of the AlCrSiTiBN anti-oxidation coating prepared in Example 1 after oxidation at 400°C for 10 hours. It can be seen from Figures 4(a) and 4(b) that under the same conditions, the AlCrSiTiBN anti-oxidation coating is almost not oxidized, while the TiBN coating generates an oxide layer of about 60 nm.

[0058] Figure 5 The statistics of the oxide films generated by comparative examples 1, 3, and 4 at 800°C for 3 hours show that with the increase of the AlCrSi target power, the thickness of the oxide layer shows a trend of first decreasing and then increasing. When the power is 200 W, the coating oxide film thickens the least, indicating that its oxidation resistance is the best.

[0059] Figure 6(a) is a cross-sectional SEM morphology of the TiBN coating prepared in Comparative Example 1 after oxidation at 800°C for 3h; Figure 6(b) is a cross-sectional SEM morphology of the AlCrSiTiBN anti-oxidation coating prepared in Example 1 after oxidation at 800°C for 3h. It can be seen from Figures 6(a) and 6(b) that under the same conditions, the thickness of the oxide film generated by the AlCrSiTiBN anti-oxidation coating is about 210nm, while TiBN is completely oxidized to form loose and porous TiO2. The AlCrSiTiBN anti-oxidation coating prepared by the present invention exhibits more excellent oxidation resistance, mainly because the addition of Al and Cr elements forms a dense Al2O3 and Cr2O3 oxide layer in the coating, which hinders the further diffusion of O along the grain boundaries. At the same time, the addition of Si element refines the grains, and the formed amorphous encapsulated nanocrystalline structure not only helps to hinder the diffusion of oxygen along the grain boundaries, but also helps to maintain its mechanical properties. When the power of the AlCrSi target is 200W, the composition of the coating is Al 6.4 Cr 6.8 Si 4.5The oxidation resistance of the coating is best when TiBN is added. The addition of Cr inhibits the transformation of metastable TiO2 to a stable state during oxidation, thereby improving its oxidation resistance. The incorporation of Si hinders the growth of TiN columnar crystals, refines the film structure, and improves the hardness and oxidation resistance. However, when the Si content is further increased, the excessive formation of amorphous phase will reduce the hardness of the coating. The maximum value of Al in the coating is between 0.64 and 0.7. When it is less than this value, the coating is a face-centered cubic structure. The coating grains are refined with increasing Al content, and the hardness and oxidation resistance are improved. When the content is greater than 0.7, the cubic AlN phase transforms into the hexagonal AlN phase, and the hardness and bonding strength are reduced. The Al content should be increased as much as possible while avoiding the appearance of h-AlN, so the 200W coating has the best oxidation resistance.

[0060] Figure 7 Figure 2 is a graph showing the mechanical properties of the AlCrSiTiBN anti-oxidation coating prepared in Example 2 and Comparative Example 2. Figure 7 It can be seen that after the addition of AlCrSi element, the hardness of the AlCrSiTiBN coating is still maintained at 39.39 GPa, and the elastic modulus is 381.26 GPa, indicating that the coating has both excellent antioxidant properties and high hardness.

[0061] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A method for preparing a ceramic coating on the surface of an aircraft engine compressor, It is characterized in that include: Step S1, polishing the substrate, then washing it with an organic solvent and deionized water in sequence, fixing the dried substrate on a substrate table, and finally placing it in a chamber of a coating device; Step S2: AlCrSi target, Ti target, TiB 2 The targets are placed on the target positions respectively; Step S3: evacuate the chamber until the vacuum degree reaches 1.8×10 -3 Pa, then heat the chamber to the deposition temperature of 300°C-400°C, introduce inert gas to adjust the chamber pressure to 1Pa, set the substrate stage bias to -950V, and etch for 10-20min; Step S4, controlling the Ti target power between 400-480 W, adjusting the flow rate of the inert gas Ar to stabilize the chamber pressure between 0.18-0.21 Pa, and sputtering a pure Ti transition layer with a thickness of 80-100 nm on the surface of the substrate; Step S5: further introduce inert gas and open N 2 The flow controller is switched on and off to control the chamber pressure to 0.18-0.21Pa, the substrate stage bias is set to -110V, the rotation speed is 23rpm, the power of the AlCrSi target is controlled to 160 to 240W, and the power of the TiB 2 The power of the target material is 65-85W, and the deposition is carried out for 2-3 hours at the deposition temperature to form an AlCrSiTiBN anti-oxidation coating on the pure Ti transition layer.

2. The method according to claim 1, It is characterized in that In step S1, the organic solvent is selected from acetone and alcohol; and the cleaning method is selected from ultrasonic cleaning.

3. The method according to claim 1, It is characterized in that In step S1, the substrate is selected from single crystal Si, single crystal Al 2 O 3 , one of 304 stainless steel.

4. The method according to claim 1, It is characterized in that In step S2, the AlCrSi target is placed on the RF target position, and the chemical composition ratio of Al, Cr, and Si in the target is 1:1:1; the Ti target and TiB 2 The target material is placed in the DC target position; the purity of the target material reaches 99.99%, and the target size is φ76.2×5 mm.

5. The method according to claim 1, It is characterized in that In step S3, the inert gas is selected from argon.

6. The method according to claim 1, It is characterized in that In step S5, Ar and N are introduced 2 , the flow ratio is 3:1, the gas pressure is stabilized at 0.18Pa, and the power of the AlCrSi target is controlled at 200W, TiB 2 The target power was 80 W, and the deposition was carried out at the deposition temperature for 3 h.

7. A ceramic coating prepared according to the method according to any one of claims 1 to 6, It is characterized in that It includes a substrate, a pure Ti transition layer, and an AlCrSiTiBN anti-oxidation coating. The ceramic coating can resist oxidation at 800°C and maintain high strength and high toughness.

Citation Information

Patent Citations

  • AlCrSiVN nano-composite coating and preparation method thereof

    CN107557736A

  • Compact titanium diboride coating, preparation method of compact titanium diboride coating and application of compact titanium diboride coating

    CN110484881A

  • Preparation process of AlCrSiN / AlCrN / AlCrON / AlCrN multilayered nano composite coating

    CN111621752A

  • Preparation process of AlCrTiSiN / AlCrTiSiON multilayer composite coating

    CN111647856A

  • Preparation process of Zr-Ti-B-N nano composite coating in reducing atmosphere

    CN111647859A

Cited By

  • High-performance diamond grinding wheel and preparation method thereof

    CN119952621A