Coating for low-temperature brazing tool, tool knife and device
By applying coatings of TiC, TiCN, TiAlN, DLC and other materials on low-temperature brazing tools, the problem of insufficient bonding and strength of the low-temperature brazing layer is solved, the grinding performance and service life of the tool are improved, and high temperatures are avoided Damage to diamond during brazing.
Patent Information
- Application Number
- CN202410959790.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-12
AI Technical Summary
In low-temperature brazing technology, the bonding force and strength of the diamond brazing layer are low, resulting in insufficient grinding performance and service life of the tool, and high-temperature brazing will cause damage to the diamond crystal.
The coating is used for low-temperature brazing tools. The coating consists of main components such as TiC, TiCN, TiAlN, DLC and other additives, and tantalum, actinide, niobium and other additives. The bonding agent forms a uniform thin layer structure to enhance the bonding force and strength of the brazing layer. .
It improves the strength and stability of the diamond brazing layer with low-temperature brazing technology, extends the service life of the tool, and avoids damage to diamond crystals in high-temperature brazing.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of brazing, and in particular relates to a coating, a tool knife and a device for low-temperature brazing tools. Background Art
[0002] Diamond grinding tools are an important type of cutting equipment. The diamond brazed grinding layer structure they provide has good processability and structural stability. The diamond abrasives in it are not easy to peel off, and have good grinding performance and service life for high-hardness materials. For example, diamond needles are used clinically for tooth preparation, pit and fissure shaping, hard fillings and dental metal material cutting, etc.; diamond needles are used in denture processing factories mainly for denture grinding. Whether it is a needle used clinically or a needle used in a denture processing factory, its appearance and structure are varied. Each dentist or technician uses needles of different specifications and shapes for tooth preparation or grinding according to their own operating habits and usage methods, and finally realizes tooth preparation and denture grinding. At present, in the high-temperature brazing process, diamond is prone to structural defects such as cracks at high temperatures such as above 800°C, while in the low-temperature brazing process, the long-term grinding performance and service life of the tool will be affected due to defects such as low bonding strength.
[0003] Therefore, in view of the above technical problems, it is necessary to provide a coating, a tool knife and a device for low-temperature brazing tools.
[0004] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention
[0005] The object of the present invention is to provide a coating, a tool knife and a device for low-temperature brazing tools.
[0006] In order to achieve the above object, a technical solution provided by a specific embodiment of the present invention is as follows:
[0007] A coating for low-temperature brazing tools is formed on the surface of a diamond brazing layer. The diamond brazing layer is a grinding layer formed by fixing diamond abrasives to the tool surface through a brazing process using a brazing material. The functional raw material composition of the coating includes, by weight: 90-99.5% of the main component and the remainder of additives, wherein the main component is selected from: TiC, TiCN, TiAlN, DLC, TaC (tantalum carbide); the additives are selected from tantalum, actinium, niobium, cesium, and lanthanum. The functional raw materials form a layer structure under the action of a binder.
[0008] In one or more embodiments of the present invention, the coating has a thickness of 7-12 μm.
[0009] In one or more embodiments of the present invention, when the diamonds in the grinding layer are uniformly distributed particles of the same size, the coating is a thin layer with a uniform thickness of 7-8 μm.
[0010] In one or more embodiments of the present invention, when the diamond particles in the grinding layer are different particles of the same size, the coating is a thin layer with a uniform thickness of 9-12 μm.
[0011] In one or more embodiments of the present invention, the bonding agent is selected from nickel-chromium alloy, titanium-copper-silver-cobalt alloy.
[0012] In one or more embodiments of the present invention, the main component is a mixture of TiC, TiAlN and DLC. Preferably, the mass ratio of TiC, TiAlN and DLC in the mixture is 1:(1-2):1. Preferably, the mass ratio of TiC, TiAlN and DLC in the mixture is 1:1.25:1.
[0013] In one or more embodiments of the present invention, the additive is niobium.
[0014] In one or more embodiments of the present invention, the binder is a nickel-chromium alloy Cr20Ni35.
[0015] In one or more embodiments of the present invention, a tool knife includes a tool body having a diamond coating and a coating for low-temperature brazing tools as described above formed at least on the surface of the blade of the tool body.
[0016] In one or more embodiments of the present invention, a grinding device includes a main machine and a tool knife as described above connected to a driving device of the main machine.
[0017] Compared with the prior art, the coating, tool knife and device for low-temperature brazing tools of the present invention effectively overcome the shortcomings of low bonding force and low strength of the diamond brazing layer in low-temperature brazing technology, and further avoid the problem of damage to diamond crystals during high-temperature brazing, which affects the performance and life of the product. It provides a method for further forming a coating on the surface of the brazing layer to achieve low-temperature brazing technology with higher strength and structural stability, so as to obtain higher product performance and longer service life. DETAILED DESCRIPTION
[0018] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0019] The coating for low-temperature brazing tools of the present invention can be formed on the surface of the diamond brazing layer by existing technologies such as chemical vapor deposition and physical vapor deposition. The diamond brazing layer is a grinding layer formed by fixing diamond abrasives to the tool surface through a brazing process using a brazing material to overcome the defects of the diamond brazing layer formed by low-temperature brazing, such as low bonding force and low strength.
[0020] The present invention includes but is not limited to the following embodiments, wherein the raw materials of the brazing filler metal for diamond brazing include, by mass fraction, 45 parts of copper, 9 parts of silver, 30 parts of zinc, 2.8 parts of nickel, 0.5 parts of graphene powder material with a particle size of 80 microns, 0.2 parts of magnesium carbonate, and 0.95 parts of rosin. The brazing filler metal is uniformly dispersed by a process such as sufficient mixing and melting. The number of brazing layers formed on the tool by brazing is 3, and the thickness of a single layer is 150 microns.
[0021] According to the relevant national standards (GB5319-85, Determination of transverse fracture strength of sintered metal materials), the size of the segment specimen is determined, the span spacing of the three-point bending fixture is 25mm, and the load drop speed is 1mm / min. A 30×6×10 rectangular grinding wheel segment is prepared, and the average value of the three specimens is used as the final test result to obtain the bending strength value.
[0022] Grinding test
[0023] Maximum circumferential speed of tool sample: 25m / s
[0024] Grinding fluid: 5% water-based emulsion, flow rate 90L / min
[0025] Grinding machine: creep feed surface grinder, model MMD7125
[0026] Grinding method: Plunge grinding
[0027] Table feed speed: 0.3m / min
[0028] Grinding test results: Using sample workpiece to grind Al 2 O 3 Ceramic grinding experiment, Al 2 O 3 The ceramics were subjected to a continuous grinding test, with the test endpoint being when the exposed part of the abrasive had lost 60% of its height.
[0029] Example 1
[0030] The coating for low-temperature brazing tools in this embodiment comprises the following functional raw material compositions by weight: 99% of the main component and the remainder of the additive, wherein the main component is TiC; the additive is lanthanum, and the functional raw materials are uniformly bonded to form a layer structure under the action of the binder Cr20Ni35 which accounts for 10% of the total weight of the functional material.
[0031] On the dental needle brazed with a grinding layer at a brazing temperature of 500°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer with uniform thickness of 7 μm: the three-point bending strength value of the sample block is 187 MPa, and there is no desoldering or breakage of the abrasive on the surface of the needle after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 500.
[0032] On the cutting blade with a grinding layer brazed at a brazing temperature of 500°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer of uniform thickness with a thickness of 7 μm: the three-point bending strength value of the sample block is 183 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 500.
[0033] On the dental bur brazed with a grinding layer at a brazing temperature of 500°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.6 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 9 μm: the three-point bending strength value of the sample block is 185 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 500.
[0034] On the cutting blade brazed with a grinding layer at a brazing temperature of 500°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.8 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 9 μm: the three-point bending strength value of the sample block is 182 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 550.
[0035] Example 2
[0036] The coating for low-temperature brazing tools in this embodiment comprises functional raw materials composed of wt%: 90% of the main component and the remainder of additives, wherein the main component is TiC and the additive is lanthanum. The functional raw materials are uniformly bonded to form a layer structure under the action of the binder Cr20Ni35 which accounts for 10% of the total weight of the functional material.
[0037] On the dental bur brazed with a grinding layer at a brazing temperature of 500°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer of uniform thickness with a thickness of 7 μm: the three-point bending strength value of the sample block is 151 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 350.
[0038] On the cutting blade with a grinding layer brazed at a brazing temperature of 500°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer with uniform thickness of 7 μm: the three-point bending strength value of the sample block is 155 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 350.
[0039] On the dental bur brazed with a grinding layer at a brazing temperature of 500°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.6 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 9 μm: the three-point bending strength value of the sample block is 153 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 350.
[0040] On the cutting blade brazed with a grinding layer at a brazing temperature of 500°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.8 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 9 μm: the three-point bending strength value of the sample block is 155 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 350.
[0041] Example 3
[0042] The coating for low-temperature brazing tools in this embodiment comprises the following functional raw materials: 99.5% of the main component and the remainder of the additives, wherein the main component is TiC and the additive is lanthanum. The functional raw materials are uniformly bonded to form a layer structure under the action of the binder Cr20Ni35 which accounts for 10% of the total weight of the functional material.
[0043] On the dental bur brazed with a grinding layer at a brazing temperature of 500°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer of uniform thickness with a thickness of 7 μm: the three-point bending strength value of the sample block is 182 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 450.
[0044] On the cutting blade with a grinding layer brazed at a brazing temperature of 500°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer with uniform thickness of 7 μm: the three-point bending strength value of the sample block is 178 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 450.
[0045] On the dental bur brazed with a grinding layer at a brazing temperature of 500°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.6 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 9 μm: the three-point bending strength value of the sample block is 175 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 450.
[0046] On the cutting blade brazed with a grinding layer at a brazing temperature of 500°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.8 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 9 μm: the three-point bending strength value of the sample block is 180 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 450.
[0047] Example 4
[0048] The only difference between this embodiment and embodiment 1 is that the binder is Cr15Ni60.
[0049] On the dental bur brazed with a grinding layer at a brazing temperature of 500°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer of uniform thickness with a thickness of 7 μm: the three-point bending strength value of the sample block is 182 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 500.
[0050] On the cutting blade with a grinding layer brazed at a brazing temperature of 500°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer with uniform thickness of 7 μm: the three-point bending strength value of the sample block is 180 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 500.
[0051] On the dental bur brazed with a grinding layer at a brazing temperature of 500°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.6 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 9 μm: the three-point bending strength value of the sample block is 182 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 500.
[0052] On the cutting blade brazed with a grinding layer at a brazing temperature of 500°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.8 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 9 μm: the three-point bending strength value of the sample block is 180 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 500.
[0053] Example 5
[0054] The coating for low-temperature brazing tools in this embodiment comprises the following functional raw materials: 99% of the main component and the remainder of the additive, wherein the main component is a mixture of TiC, TiAlN and DLC in a mass ratio of 1:2:1; the additive is niobium, and the functional raw materials are uniformly bonded to form a layer structure under the action of the binder Cr20Ni35 accounting for 10% of the total mass of the functional material.
[0055] On the dental bur brazed with a grinding layer at a brazing temperature of 500°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer of uniform thickness with a thickness of 7 μm: the three-point bending strength value of the sample block is 185 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 500.
[0056] On the cutting blade with a grinding layer brazed at a brazing temperature of 500°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer with uniform thickness of 7 μm: the three-point bending strength value of the sample block is 187 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 500.
[0057] On the dental bur brazed with a grinding layer at a brazing temperature of 500°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.6 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 9 μm: the three-point bending strength value of the sample block is 185 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 500.
[0058] On the cutting blade brazed with a grinding layer at a brazing temperature of 500°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.8 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 9 μm: the three-point bending strength value of the sample block is 186 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 500.
[0059] Example 6
[0060] The only difference between this embodiment and embodiment 5 is that the main components are a mixture of TiC, TiAlN and DLC in a mass ratio of 1:1:1.
[0061] On the dental needle brazed with a grinding layer at a brazing temperature of 500°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer of uniform thickness with a thickness of 7 μm: the three-point bending strength value of the sample block is 188 MPa, and there is no desoldering or breakage of the abrasive on the surface of the needle after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 500.
[0062] On the cutting blade with a grinding layer brazed at a brazing temperature of 500°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer with uniform thickness of 7 μm: the three-point bending strength value of the sample block is 189 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 500.
[0063] On the dental bur brazed with a grinding layer at a brazing temperature of 500°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.6 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 9 μm: the three-point bending strength value of the sample block is 192 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 500.
[0064] On the cutting blade brazed with a grinding layer at a brazing temperature of 500°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.8 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 9 μm: the three-point bending strength value of the sample block is 190 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 500.
[0065] Example 7
[0066] The only difference between this embodiment and embodiment 5 is that the main components are a mixture of TiC, TiAlN and DLC in a mass ratio of 1:1.25:1.
[0067] On the dental bur brazed with a grinding layer at a brazing temperature of 500°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer of uniform thickness with a thickness of 7 μm: the three-point bending strength value of the sample block is 200 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 550.
[0068] On the cutting blade with a grinding layer brazed at a brazing temperature of 500°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer with uniform thickness of 7 μm: the three-point bending strength value of the sample block is 198 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 550.
[0069] On the dental bur brazed with a grinding layer at a brazing temperature of 500°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.6 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 9 μm: the three-point bending strength value of the sample block is 205 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 550.
[0070] On the cutting blade brazed with a grinding layer at a brazing temperature of 500°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.8 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 9 μm: the three-point bending strength value of the sample block is 203 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 550.
[0071] Example 8
[0072] The only difference between this embodiment and embodiment 7 is that the additive is tantalum.
[0073] On the dental bur brazed with a grinding layer at a brazing temperature of 500°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer with uniform thickness of 7 μm: the three-point bending strength value of the sample block is 192 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 530.
[0074] On the cutting blade with a grinding layer brazed at a brazing temperature of 500°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer with uniform thickness of 7 μm: the three-point bending strength value of the sample block is 195 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 530.
[0075] On the dental bur brazed with a grinding layer at a brazing temperature of 500°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.6 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 9 μm: the three-point bending strength value of the sample block is 198 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 530.
[0076] On the cutting blade brazed with a grinding layer at a brazing temperature of 500°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.8 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 9 μm: the three-point bending strength value of the sample block is 193 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 530.
[0077] Example 9
[0078] The only difference between this embodiment and embodiment 7 is that the coating thickness is different.
[0079] On the dental bur brazed with a grinding layer at a brazing temperature of 500°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer with uniform thickness of 8 μm: the three-point bending strength value of the sample block is 201 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 550.
[0080] On the cutting blade with a grinding layer brazed at a brazing temperature of 500°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer with uniform thickness of 8 μm: the three-point bending strength value of the sample block is 197 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 550.
[0081] On the dental bur brazed with a grinding layer at a brazing temperature of 500°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.6 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 12 μm: the three-point bending strength value of the sample block is 203 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 550.
[0082] On the cutting blade brazed with a grinding layer at a brazing temperature of 500°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.8 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 12 μm: the three-point bending strength value of the sample block is 204 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 550.
[0083] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
[0084] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A coating for low-temperature brazing tools, which is formed on the surface of a diamond brazing layer, wherein the diamond brazing layer is a grinding layer formed by fixing diamond abrasives to the tool surface through a brazing process using a brazing material, characterized in that: The functional raw material composition of the coating includes, by weight: 90-99.5% of the main component and the remainder of additives, wherein the main component is selected from: TiC, TiCN, TiAlN, DLC, TaC; the additive is selected from: tantalum, actinium, niobium, cesium, lanthanum, and the functional raw material forms a layer structure under the action of a binder.
2. The coating for low temperature brazing tools according to claim 1, characterized in that: The coating has a thickness of 7-12 μm.
3. The coating for low temperature brazing tools according to claim 2, characterized in that: When the diamonds in the grinding layer are uniformly distributed particles of the same size, the coating is a thin layer with uniform thickness, and the thickness is 7-8 μm.
4. The coating for low temperature brazing tools according to claim 2, characterized in that: When the diamonds in the grinding layer are particles of different sizes, the coating is a thin layer with uniform thickness, and the thickness is 9-12 μm.
5. The coating for low temperature brazing tools according to claim 1, characterized in that: The binder is selected from nickel-chromium alloy, titanium-copper-silver-cobalt alloy.
6. The coating for low temperature brazing tools according to claim 1, characterized in that: The main component is a mixture of TiC, TiAlN and DLC.
7. The coating for low temperature brazing tools according to claim 1, characterized in that: The additive is niobium.
8. The coating for low temperature brazing tools according to claim 5, characterized in that: The binder is a nickel-chromium alloy Cr20Ni35.
9. A tool knife comprising a tool body having a diamond coating and the coating for low-temperature brazing tools according to any one of claims 1 to 8 formed at least on the surface layer of the blade of the tool body.
10. A grinding device comprising a main machine and the utility knife according to claim 9 connected to a driving device of the main machine.