Full-deep-sea eight-component aluminum alloy sacrificial anode and preparation method thereof
By adding elements such as Zn, In, Ga, Mg, Ti, Ca and Mn to the sacrificial anode of aluminum alloy, forming micron-level precipitation phases and galvanic pairs, the problem of self-corrosion of the anode in a deep sea environment of 10,000 meters is solved, and high Current efficiency and stable electrochemical properties are suitable for deep sea environments of 0 to 10,000 meters.
Patent Information
- Application Number
- CN202410988637.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-23
AI Technical Summary
The existing deep-sea aluminum alloy sacrificial anode in a deep-sea environment is accelerated due to the high hydrostatic pressure, which intensifies self-corrosion and decreases current efficiency, which cannot meet the protection needs of metal equipment in a deep-sea environment of 3,000 to 10,000 meters.
Design a sacrificial anode of a full-deep sea 8-member aluminum alloy, add alloying elements such as Zn, In, Ga, Mg, Ti, Ca and Mn, and destroy the surface oxidation of Al matrix through solid solution, dissolution, redeposition and oxide formation volume effect The layer suppresses self-corrosion, and forms a micron-scale corrosion galvanized pair activated surface by Ti and Ca, Mn balances the impurity Fe, and the preparation method includes heating melting, stirring and mixing, and casting.
Maintain high activity and high current efficiency in a deep sea environment of 0 to 10,000 meters, stable working potential, current efficiency reaches 90 to 95%, uniform surface dissolution, corrosion products are prone to falling off, significantly improving the scope of application and performance of the anode.
Smart Images

Figure HDA0004958235810000011 
Figure HDA0004958235810000012 
Figure HDA0004958235810000013
Abstract
Description
Technical field:
[0001] The present invention belongs to the technical field of corrosion protection of metal materials, and specifically relates to an aluminum alloy sacrificial anode with full-sea-depth high activity and a preparation method thereof, which can maintain high activity and high current efficiency in an extreme deep-sea environment of 10,000 meters and avoid self-passivation of the anode. Background technology:
[0002] The development of deep-sea engineering towards the deep-sea environment of 10,000 meters is unstoppable, but the serious deep-sea corrosion problem has always restricted the rapid development of deep-sea engineering equipment. Sacrificial anode protection is the most effective method for corrosion protection of marine engineering equipment. In the existing technology, aluminum alloy anodes used in shallow waters will have problems such as surface crusting, reduced current efficiency, and severe self-corrosion due to the "dissolution-redeposition" difficulties of active alloying elements such as In and Zn in the high-pressure, low-temperature, and low-oxygen environment of the deep sea. It cannot meet the protection requirements of metal equipment in deep-sea environments, let alone the protection requirements of metal equipment in extremely deep sea areas with a depth of more than 10,000 meters such as the Mariana Trench. Based on this, the development of sacrificial anode materials with high activity, synergistic effects of multiple alloying elements, uniform microstructure, high current efficiency, and suitable for deep-sea environments has become an urgent problem to be solved.
[0003] The deep-sea sacrificial anodes on the market are mainly aluminum alloy sacrificial anodes. For example, Chinese Patent No. 201610211695.7 discloses a method for preparing a high-performance aluminum alloy sacrificial anode for deep-sea environment. The obtained aluminum alloy sacrificial anode is suitable for deep-sea environment with high pressure, low temperature and low oxygen, and has the characteristics of stable working potential, easy shedding of corrosion products, uniform corrosion morphology, environmentally friendly formula, high capacitance and high current efficiency, and good casting performance; the aluminum alloy sacrificial anode is prepared by melting and casting with aluminum as the matrix, zinc, indium, tin and gallium elements added, and the obtained aluminum alloy sacrificial anode is prepared by melting and casting. In a simulated deep-sea environment (hydrostatic pressure of 30MPa, temperature of 4°C, dissolved oxygen content of 2.5-3mg / L) has a current efficiency higher than 90%, a working potential of 1.10 to -1.06 V (Ag / AgCl), and a capacitance greater than 2600 Ah / kg; Chinese patent 202310318260.2 discloses an aluminum alloy sacrificial anode for a deep-sea environment, the chemical composition of which includes aluminum, zinc, indium and silicon, the mass fraction of zinc is 4.95 to 5.35%, the mass fraction of indium is 0.017 to 0.018%, the mass fraction of silicon is 0.08 to 0.09%, and the balance is aluminum; its working potential in a simulated deep-sea environment with a temperature of 4°C and a dissolved oxygen content of 2.7 mg / L is ≤-1.05 V, and its electrochemical capacity is ≥2500 Ah / kg. Chinese patent 201810529402.9 discloses a seven-element aluminum alloy sacrificial anode material for deep-sea environment, which contains the following components by mass percentage: 5-6% zinc, 0.02-0.08% indium, 0.05-0.2% silicon, 0.1-0.6% cerium, 0.01-0.07% titanium, 0.5-2.0% magnesium, the balance is aluminum, and the impurity iron is <0.1%; its working potential in a simulated deep-sea environment with a temperature of 10±1°C, a hydrostatic pressure of 10MPa, and a dissolved oxygen content of 2mg / L is -0.94~-1.09V, a capacitance of 2365.3~2500.3Ah / kg, and a current efficiency of 83.4~88.1%. Chinese patent 201110085962.8 discloses a sacrificial anode for deep-sea environment, which uses aluminum as raw material and is added with elements of zinc, indium and silicon. The weight percentage of each component is as follows: zinc 3.0-5.0%, indium 0.01-0.02%, silicon 0.10-0.20%; the total amount of impurities is ≤0.16%, of which the impurity iron is ≤0.13%, and the impurity copper is ≤0.006%; the balance is aluminum; its working potential in a simulated deep-sea low-temperature environment (temperature is 10°C, deoxygenated) is -1.12 to -1.05V, the current efficiency is >93%, and the capacitance is >2600Ah / kg.Chinese patent 201510418356.1 discloses a high-efficiency aluminum alloy sacrificial anode for deep sea use, which uses electrolytic aluminum liquid as raw material, and the alloy composition content is: zinc 5-6wt%, indium 0.02-0.025wt%, magnesium 1.5-2.0wt%, titanium 0.05-0.06wt%, iron 0.08-0.15wt%, aluminum balance; its working potential in a simulated deep sea low temperature environment (temperature is 4°C, dissolved oxygen content is 4mg / L) is -1.069~-1.092V, current efficiency is 93.1~93.7%, and capacitance is 2662~2675Ah / kg. Chinese patent 200810249621.8 discloses an aluminum alloy sacrificial anode suitable for deep sea environment, which uses A00 aluminum as the main raw material, and adds the elements zinc, indium, magnesium, titanium, gallium, and manganese. The weight percentage of each component is as follows: zinc 2.0-5.5%, indium 0.03-0.08%, magnesium 0.5-2.0%, titanium 0.05-0.2%, gallium 0.05-0.55%, manganese 0.02-1.2%, and the total amount of impurities is ≤0.30%, wherein the impurities iron+copper+nickel ≤0.15%, silicon+calcium ≤0.15%, and the balance is aluminum; the working potential thereof is -1.05--1.10V and the current efficiency is 90.2-91.8% in a simulated 800-meter deep sea low temperature environment (temperature is 4°C, dissolved oxygen content is 4mg / L, and hydrostatic pressure is 8MPa) . Chinese patent 201410311844.8 discloses an aluminum alloy sacrificial anode with high current efficiency suitable for deep-sea environment. It takes aluminum as the matrix and adds zinc, indium, tin, magnesium and titanium alloy elements. The specific composition ratio (wt%) is: zinc 4.0-6.0%, indium 0.020-0.030%, tin 0.05-0.10%, magnesium 0.5-1.0%, titanium 0.05-0.10%, wherein the impurities iron <0.050%, copper <0.010%, and the balance is aluminum; its current efficiency in a simulated deep-sea environment (temperature of 4°C, hydrostatic pressure of 8MPa) is greater than 92%, and the open circuit potential is -1.05 to -1.20. Chinese patent 201110142890.6 discloses an aluminum alloy sacrificial anode for deep sea environment, which is composed of aluminum, zinc, indium and cadmium, and is calculated by weight as 94-98 parts of aluminum, 3-5 parts of zinc, 0.04-0.06 parts of indium, and 0.01-0.03 parts of cadmium; its working potential in a simulated deep sea environment (temperature of 4°C, hydrostatic pressure of 8MPa) is -1.07 to -1.10V, current efficiency is 86 to 90%, and capacitance is 2500 to 2700Ah / kg. The sacrificial anode in the above patent has good activation performance in deep sea environment, dissolves evenly, and corrosion products are easy to fall off.
[0004] Although the current efficiency of deep-sea anodes in the prior art is higher than 90%, the hydrostatic pressure of the test is less than 30 MPa, which is only suitable for cathodic protection of metal structural materials in a deep-sea environment of 0 to 3000 meters. When the hydrostatic pressure in a deep-sea environment of 10,000 meters exceeds 100 MPa, the sacrificial anode will be damaged by Cl - The accelerated ion diffusion rate faces the aggravation of self-corrosion, which seriously affects the anode current efficiency. Therefore, it cannot be used for a long time in the deep sea environment of 3000 to 10000 meters. At present, there is no sacrificial anode material suitable for cathodic protection of metal structural materials in the deep sea environment of 3000 to 10000 meters and related research reports. Therefore, an aluminum alloy anode with high activity and high current efficiency suitable for the deep sea of 10,000 meters and its preparation method are developed and designed. Summary of the invention:
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art, develop and design an aluminum alloy sacrificial anode with high activity, synergistic effect of multiple alloying elements, uniform microstructure and high current efficiency, so as to provide cathodic protection for metal structural materials in a deep sea environment of 0 to 10,000 meters.
[0006] In order to achieve the above-mentioned purpose, the present invention relates to a full deep-sea octal aluminum alloy sacrificial anode, which uses Al as the main raw material, and adds alloying elements: Zn, In, Ga, Mg, Ti, Ca and Mn, and the weight percentage of each component is as follows: Zn is 2.5-3.5wt%, In is 0.01-0.03wt%, Ga is 0.01-0.03wt%, Mg is 0.5-2.0wt%, Ti is 0.005-0.02wt%, Ca is 0.02-0.1wt%, Mn is 0.05-0.2wt%, impurity Fe content is <0.1%, impurity Cu content is <0.01%, impurity Si content is <0.01%, and the balance is Al, wherein the total amount of alloying elements does not exceed 6%.
[0007] The Zn, In, Ga and Mg in the alloying elements of the present invention are activation elements dissolved in the Al matrix. Low-content In and Ga activate the Al matrix surface by dissolution and re-deposition. The oxides formed by Zn and Mg destroy the continuity and density of the Al matrix surface oxide layer through the volume effect, thereby inhibiting the Al matrix surface from forming a crust.
[0008] Ti and Ca exist in the Al matrix as uniformly distributed micron-sized precipitated phases (AlTi3, Al4Ca), forming uniformly distributed micron-sized corrosion galvanic pairs with the Al matrix, which has the effect of activating the surface of the Al matrix;
[0009] Mn can balance the impurity Fe, stabilize the activity of the sacrificial anode of the deep-sea octal aluminum alloy, and reduce the self-corrosion rate.
[0010] The process of the method for preparing a full deep-sea octal aluminum alloy sacrificial anode according to the present invention is as follows:
[0011] First, Al and Zn are heated to 750-1000°C according to a set ratio to make them melt;
[0012] Then, In, Ga, Mg, Ti, Ca and Mn are added in the set ratio, mixed thoroughly, kept warm and allowed to stand for 2 to 5 minutes;
[0013] Finally, by casting at a temperature of 700-750°C and quenching in water at room temperature, a full deep-sea octal aluminum alloy sacrificial anode with an average grain size of less than 500μm is obtained. The micron-sized precipitates formed by the alloying elements are uniformly distributed in the grain, and the precipitate size is less than 10μm.
[0014] The invention relates to a method for preparing a full deep-sea octa-element aluminum alloy sacrificial anode. The prepared full deep-sea octa-element aluminum alloy sacrificial anode is suitable for cathode protection of high-strength steel structures in a deep-sea environment of 0 to 10,000 meters. The working potential in deep-sea water of 0 to 10,000 meters is -1.053V to -1.140V, the current efficiency is 90 to 95%, the surface dissolution is uniform, the corrosion products are easy to fall off, and the activation performance is good.
[0015] The full deep-sea octal aluminum alloy sacrificial anode of the present invention can also be prepared by other metallurgical means such as powder metallurgy.
[0016] Compared with the prior art, the present invention forms a full-deep sea octal aluminum alloy sacrificial anode by adding Ca, improves the activation ability by virtue of the effect of In and Ga dissolving and re-depositing, the effect of Zn and Mg destroying the continuity and compactness of the oxide layer, and the effect of surface micron-level dot pairs activating the surface of the Al matrix, and at the same time, the effect of Ti refining the grain size makes the distribution of the alloying elements uniform and without segregation, avoids internal self-corrosion, improves the current efficiency, can be applied to the full-sea deep sea water environment of 0 to 10,000 meters, and the current efficiency reaches 90 to 95%, which is significantly higher than the applicable range of 0 to 3,000 meters water depth, and has obvious practicality. Description of the drawings:
[0017] Figure 1 This is a metallographic photograph of the grain structure of the full deep-sea octal aluminum alloy sacrificial anode prepared in Example 1 of the present invention.
[0018] Figure 2 This is a scanning electron microscope photograph of the micron-scale precipitation phase of the full deep-sea octal aluminum alloy sacrificial anode prepared in Example 1 of the present invention.
[0019] Figure 3This is a corrosion surface photograph of the full deep-sea octal aluminum alloy sacrificial anode prepared in Example 4 of the present invention after the electrochemical performance test. Specific implementation method:
[0020] The present invention will be further described below with reference to the accompanying drawings and in conjunction with embodiments.
[0021] Embodiment 1:
[0022] The present embodiment involves a full deep-sea octal aluminum alloy sacrificial anode with Al as the main raw material, and alloying elements: Zn, In, Ga, Mg, Ti, Ca and Mn are added, and the weight percentage of each component is as follows: Zn is 3.5wt%, In is 0.03wt%, Ga is 0.01wt%, Mg is 2.0wt%, Ti is 0.02wt%, Ca is 0.1wt%, Mn is 0.2wt%, impurity Fe content is <0.1%, impurity Cu content is <0.01%, impurity Si content is <0.01%, and the balance is Al;
[0023] The specific process of its preparation method is:
[0024] First, Al and Zn are heated to 750-1000°C to be in a molten state;
[0025] Then, add In, Ga, Mg, Ti, Ca and Mn, stir and mix thoroughly, keep warm and let stand for 2 to 5 minutes;
[0026] Finally, it is cast at a temperature of 700-750°C and quenched in water at room temperature;
[0027] The obtained metallographic microstructure of the deep-sea octal aluminum alloy sacrificial anode is shown in the following figure: Figure 1 As shown, the average grain size of the alloy is 480 μm;
[0028] The obtained full deep-sea octal aluminum alloy sacrificial anode obtained the precipitated phase scanning electron microscope photo as shown in Figure 2 As shown, the micron-sized precipitates rich in alloying elements are mainly precipitated within the grains, and the size is less than 10 μm.
[0029] Embodiment 2:
[0030] The weight percentages of the components of a full deep-sea octal aluminum alloy sacrificial anode involved in this embodiment are as follows: Zn is 3.0wt%, In is 0.02wt%, Ga is 0.02wt%, Mg is 1.5wt%, Ti is 0.01wt%, Ca is 0.1wt%, Mn is 0.1wt%, impurity Fe content is <0.1%, impurity Cu content is <0.01%, impurity Si content is <0.01%, and the balance is Al;
[0031] The specific process of its preparation method is the same as that of Example 1.
[0032] Embodiment 3:
[0033] The present embodiment involves a full deep-sea octal aluminum alloy sacrificial anode with the following weight percentages of the Al components: Zn is 2.5wt%, In is 0.01wt%, Ga is 0.03wt%, Mg is 1.0wt%, Ti is 0.005wt%, Ca is 0.05wt%, Mn is 0.05wt%, impurity Fe content is <0.1%, impurity Cu content is <0.01%, impurity Si content is <0.01%, and the balance is Al;
[0034] The specific process of its preparation method is the same as that of Example 1.
[0035] Embodiment 4:
[0036] The weight percentages of the components of a full deep-sea octal aluminum alloy sacrificial anode involved in this embodiment are as follows: Zn is 3.0wt%, In is 0.02wt%, Ga is 0.02wt%, Mg is 0.5wt%, Ti is 0.005wt%, Ca is 0.05wt%, Mn is 0.05wt%, impurity Fe content is <0.1%, impurity Cu content is <0.01%, impurity Si content is <0.01%, and the balance is Al;
[0037] The specific process of its preparation method is the same as that of Example 1.
[0038] Embodiment 5:
[0039] This example involves accelerated testing of the electrochemical properties of the full deep-sea octal aluminum alloy sacrificial anodes prepared in Examples 1-4;
[0040] According to the national standard GB / T17848-1999, the electrochemical performance accelerated test was performed on the full deep-sea octal aluminum alloy sacrificial anodes prepared in Examples 1-4;
[0041] The test results of the deep-sea octal aluminum alloy sacrificial anode prepared in Example 1 in shallow sea water at room temperature show that the working potential is -1.053 to -1.124 V, the current efficiency is 95%, the dissolution is uniform without obvious local corrosion, the corrosion products have no obvious adhesion, and the activation is good;
[0042] The test results of the full deep-sea octal aluminum alloy sacrificial anode prepared in Example 2 in a simulated 2000-meter deep-sea environment (hydrostatic pressure of 20 MPa, dissolved oxygen content of 0.5 mg / L, temperature of 5°C) showed that: the working potential was -1.059 to -1.128 V, the current efficiency was 94.3%, the dissolution was uniform without obvious local corrosion, the corrosion products had no obvious adhesion, and the activation was good;
[0043] The test results of the full deep-sea octal aluminum alloy sacrificial anode prepared in Example 3 in a simulated 5000-meter deep-sea environment (hydrostatic pressure of 50 MPa, dissolved oxygen content of 3 mg / L, temperature of 2°C) showed that: the working potential was -1.062 to -1.137 V, the current efficiency was 92.7%, the dissolution was uniform without obvious local corrosion, the corrosion products had no obvious adhesion, and the activation was good;
[0044] The test results of the deep-sea octal aluminum alloy sacrificial anode prepared in Example 4 in a simulated 10,000-meter deep-sea environment (hydrostatic pressure of 100 MPa, dissolved oxygen content of 2 mg / L, temperature of 2°C) showed that the working potential was -1.056 to -1.117 V, the current efficiency was 90.7%, and the corrosion surface was as follows: Figure 3 As shown, the dissolution is uniform without obvious local corrosion, the corrosion products have no obvious adhesion, and the activation is good.
Claims
1. A full deep-sea octal aluminum alloy sacrificial anode, characterized in that: Al is the main raw material, and alloying elements are added: Zn, In, Ga, Mg, Ti, Ca and Mn.
2. The full deep sea octal aluminum alloy sacrificial anode according to claim 1, characterized in that: The weight percentage of each component is as follows: Zn is 2.5-3.5wt%, In is 0.01-0.03wt%, Ga is 0.01-0.03wt%, Mg is 0.5-2.0wt%, Ti is 0.005-0.02wt%, Ca is 0.02-0.1wt%, Mn is 0.05-0.2wt%, impurity Fe content is <0.1%, impurity Cu content is <0.01%, impurity Si content is <0.01%, and the balance is Al.
3. A full deep sea octal aluminum alloy sacrificial anode according to claim 1 or 2, characterized in that: The total amount of alloying elements does not exceed 6%.
4. The full deep sea octal aluminum alloy sacrificial anode according to claim 3, characterized in that: Zn, In, Ga and Mg are activation elements dissolved in the Al matrix. In and Ga activate the Al matrix surface by dissolving and re-depositing. The oxides formed by Zn and Mg destroy the continuity and density of the Al matrix surface oxide layer through the volume effect, thus inhibiting the Al matrix surface crusting. Ti and Ca exist in the Al matrix as micron-sized precipitates, forming micron-sized corrosion galvanic pairs with the Al matrix to activate the Al matrix surface; Mn balances the impurity Fe.
5. A method for preparing a full deep-sea octal aluminum alloy sacrificial anode, characterized in that: The process is: First, Al and Zn are melted; Then, In, Ga, Mg, Ti, Ca and Mn were added, stirred and mixed, kept warm and allowed to stand; Finally, it is cast and quenched in room temperature water.
6. The method for preparing a full deep-sea octal aluminum alloy sacrificial anode according to claim 5, characterized in that: Heat Al and Zn to 750-1000°C to melt them; The standing time is 2 to 5 minutes; The casting temperature is 700-750°C.
7. A method for preparing a full deep-sea octal aluminum alloy sacrificial anode according to claim 5 or 6, characterized in that: The average grain size of the prepared full deep-sea octal aluminum alloy sacrificial anode is less than 500 μm, and the micron-sized precipitated phase formed by the alloying elements is uniformly distributed in the grain, and the precipitated phase size is less than 10 μm.
8. A method for preparing a full deep-sea octal aluminum alloy sacrificial anode according to claim 5 or 6, characterized in that: The prepared full deep-sea octal aluminum alloy sacrificial anode has a working potential of -1.053V to -1.140V in deep-sea water at a depth of 0 to 10,000 meters, and a current efficiency of 90 to 95%. It is suitable for cathodic protection of high-strength steel structures in deep-sea environments at a depth of 0 to 10,000 meters.
9. The method for preparing a full deep-sea octal aluminum alloy sacrificial anode according to claim 5, characterized in that: The product is prepared by metallurgical means including powder metallurgy.
Citation Information
Patent Citations
Aluminum alloy sacrificial anode suitable for abyssal environment
CN101445935A
Mg-Mn-Ca-Zn-Sr sacrificial anode with high current efficiency
CN101665944A
Aluminum alloy sacrificial anode suitable for deep sea environment and high in current efficiency
CN104060280A
Aluminum alloy anode material as well as preparation method and application thereof
CN113667985A
Zn-Li alloy sacrificial anode for deep sea and preparation method of Zn-Li alloy sacrificial anode
CN115198277A