Monolithic low-carbon alkane catalyst with in-situ grown active components as well as preparation method and application of monolithic low-carbon alkane catalyst

The in-situ growth of active components is achieved on the support surface by rotary hydrothermal method, and the mechanical strength of the catalyst is improved through nickel ion doping, solving the problem of covering the active components and insufficient mechanical strength, and achieving efficient low-carbon alkanes Catalyst preparation reduces costs and improves stability.

CN118949998APending Publication Date: 2024-11-15SOUTH CHINA UNIV OF TECH

Patent Information

Application Number
CN202411094007.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

During the preparation of the monolithic catalyst, the active components are easily covered by inorganic binders, resulting in a decrease in catalytic activity and insufficient mechanical strength in the in-situ growth process, which limits the application of the process.

Method used

The rotary hydrothermal method is used to achieve in situ growth of active components on the surface of the carrier, and the mechanical strength and catalytic activity of the catalyst are improved through nickel ion doping, avoiding the problem of binder coverage.

Benefits of technology

It significantly improves the catalytic activity and mechanical strength of low-carbon alkane catalysts, reduces the preparation cost, simplifies the process flow, and improves the stability and application potential of the integrated catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118949998A_ABST
    Figure CN118949998A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a monolithic low-carbon alkane catalyst with in-situ growth of active components. The method comprises the following steps: carrying out acid treatment on a cordierite monolithic catalyst, coating pseudo-boehmite glue, calcining to obtain a catalyst carrier, uniformly mixing metal nitrate, deionized water, disodium ethylene diamine tetraacetate, urea and NH4F to prepare a precursor solution, transferring the catalyst carrier into a reaction kettle of the precursor solution, and carrying out hydrothermal reaction at the temperature of 60-80 DEG C to obtain the catalyst. Carrying out hydrothermal reaction in a drying oven with a rotating function, and then cleaning, drying and calcining the catalyst to obtain the monolithic low-carbon alkane catalyst with in-situ growth of active components. According to the invention, metal ions are directly loaded in the catalyst carrier through an active component in-situ growth method to prepare the monolithic catalyst, full exposure of surface active components is realized, the doping of nickel ions not only improves the catalytic activity, but also significantly improves the mechanical strength of the active components, and high efficiency of low-carbon alkane can be realized. And low-cost catalytic oxidation is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalytic oxidation of low-carbon alkanes in air pollution prevention and control, and specifically relates to a preparation method and application of an integral low-carbon alkane catalyst with in-situ growth of active components. Background Art

[0002] Methane is a potent greenhouse gas with a much higher greenhouse effect potential (GWP) than carbon dioxide. Although the concentration of methane in the atmosphere is much lower than that of carbon dioxide, its contribution to global warming cannot be ignored. Methane emissions mainly come from the extraction and use of fossil fuels, agricultural activities (such as rice cultivation, animal husbandry), landfills, etc.

[0003] Catalytic oxidation technology has the advantages of high efficiency, high adaptability, high selectivity, and easy operation. The core lies in the development of highly active catalysts. The high activity of cobalt-based spinel catalysts has attracted widespread attention, and related research is also in full swing. However, in scientific research, the development of catalyst powder is the primary task. In practical applications, monolithic catalysts are the most commonly used catalyst form in air pollution control.

[0004] However, in the process of producing monolithic catalysts, inorganic and organic binders are usually added to the active metal oxide to prepare slurry, and the obtained slurry is used to load the active components on the carrier surface by coating (CN 111167436B). After high-temperature sintering, some active components may be covered by the binder, thereby reducing the catalytic activity and making it difficult to achieve the expected catalytic activity. This has become a problem that needs to be solved urgently at this stage.

[0005] The in-situ growth process can avoid the problem of active components being covered, but when the active components are grown in-situ on the surface of the carrier by wet chemical methods, sol-gel methods, etc., the interaction between these newly generated active phases and the carrier may not reach the optimal state, especially without proper post-treatment. Subsequently, if calcination is directly performed to remove impurities and promote crystallization, the mechanical strength may be significantly reduced due to the temperature gradient, stress concentration and the difference in thermal expansion coefficient between the active components and the carrier during the heat treatment process, thus greatly limiting the application of the in-situ growth process.

[0006] Chinese patent CN102151564A, Preparation method of denitration monolithic catalyst and slurry thereof, introduces the preparation of a denitration monolithic catalyst and its slurry formula, the slurry is mixed with catalyst, silica gel and water, and the catalyst is prepared by impregnation. However, the prepared monolithic catalyst has the problem that the active components are easy to fall off, and the performance requirements are not met.

[0007] Chinese patent CN102151564A discloses a method for preparing a monolithic catalyst, and proposes a process for preparing a monolithic catalyst, including preparing a hydrotalcite-like slurry, mixing it with water and a binder to form a coating slurry, and then evenly coating the slurry on a carrier, and drying and calcining the slurry to obtain the catalyst. However, the catalyst has poor effect and a high catalyst shedding rate. Summary of the invention

[0008] In order to overcome the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a preparation method and application of an integral low-carbon alkane catalyst with in-situ growth of active components.

[0009] The purpose of the present invention is achieved by at least one of the following technical solutions.

[0010] The preparation method provided by the present invention not only realizes the direct growth of active components on the surface of the catalyst carrier by the rotary hydrothermal method, but also overcomes the problem of active components being covered due to the addition of inorganic adhesives during the preparation process, thereby increasing the specific surface area of ​​the catalyst.

[0011] The rotational hydrothermal process and the presence of additives can achieve uniform embedding of nickel ions in the cobalt-based spinel lattice, further improving the catalytic activity of low-carbon alkanes.

[0012] Nickel ions not only act as dopants to improve the activity of the catalyst, but also doping with nickel ions increases the mechanical strength of the active components on the carrier surface, significantly improving the stability of the catalyst.

[0013] The present invention provides a method for preparing and using a monolithic low-carbon alkane catalyst with in-situ growth of active components, comprising the following steps (refer to Figure 1 ):

[0014] (1) dissolving a metal nitrate and urea in deionized water respectively to obtain a metal nitrate solution and a urea solution, and adding the urea solution dropwise to the metal nitrate solution under stirring to obtain a clear mixed solution;

[0015] (2) adding NH4F and disodium ethylenediaminetetraacetate to the clarified mixed solution to obtain a clarified precursor solution;

[0016] (3) treating the cordierite carrier with acid, coating it with aluminum gel and calcining it, then placing the cordierite carrier in a reaction kettle and adding the precursor solution obtained in step (2);

[0017] (4) transferring the reactor containing the cordierite carrier in step (3) to an oven with a rotating function for hydrothermal reaction to obtain a monolithic catalyst loaded with active components;

[0018] (5) The integral catalyst obtained in step (4) is cleaned, dried, and calcined under air conditions to obtain an integral low-carbon alkane catalyst with in-situ growth of the active components.

[0019] Further, in step (1), the molar ratio of the metal nitrate to urea is 1:2-1:5, the concentration of the metal nitrate solution is 0.4-0.6 mol / L, the metal nitrate needs to contain cobalt nitrate and nickel nitrate at the same time, wherein the molar ratio of cobalt nitrate to nickel nitrate is 2:1-14:1, and the concentration of the urea solution is 0.8-1.2 mol / L. The stirring rate of the stirring reaction is 1000-2000 rpm.

[0020] Preferably, in step (1), the molar ratio of the metal nitrate to urea is 1:2, the concentration of the metal nitrate solution is 0.5 mol / L, the molar ratio of the cobalt nitrate to the nickel nitrate is 5:1, the concentration of the urea solution is 1.0 mol / L. The stirring rate of the stirring reaction is 2000 rpm.

[0021] Furthermore, in step (2), the molar ratio of NH4F to metal nitrate is 1:10-1:15, and the molar ratio of disodium ethylenediaminetetraacetate to metal nitrate is 1:15-1:20.

[0022] Preferably, in step (2), the molar ratio of NH4F to metal nitrate is 1:10, and the molar ratio of disodium ethylenediaminetetraacetate to metal nitrate is 1:15.

[0023] Furthermore, in step (3), the cordierite carrier is subjected to acid treatment and then aluminum gel coating and calcination are specifically performed by: using 4-6 mol / L nitric acid for acid treatment, controlling the acid treatment temperature to 80-90°C, and the acid treatment time to 1-2 hours; after the acid treatment is completed, ultrasonic cleaning is performed in deionized water, and the water is changed 3-4 times, and then the aluminum gel coating and calcination steps are performed after drying.

[0024] Preferably, in step (3), the cordierite carrier is treated with 5 mol / L nitric acid, the acid treatment temperature is controlled to be 80° C., and the acid treatment time is 1 hour. After the acid treatment, ultrasonic cleaning is performed in deionized water, and the water is changed 3 times.

[0025] Furthermore, the synthesis method of the aluminum gel described in step (3) is as follows: add 13-15 g of pseudo-boehmite to every 100 ml of deionized water, fully dissolve it and heat it to 80-85° C., add 2-3 ml of 5 mol / L nitric acid solution, stir until the solution is a milky white clear colloid and then use it.

[0026] Preferably, the synthesis method of the aluminum gel described in step (3) is as follows: 13 g of pseudo-boehmite is added to 100 ml of deionized water, fully dissolved and heated to 80° C., and 3 ml of 5 mol / L nitric acid solution is added.

[0027] Furthermore, the aluminum gel coating and calcining step is: the cordierite carrier is coated with aluminum gel 3-4 times by an immersion pulling method, and then calcined in a muffle furnace at 1000-1200° C. after drying; the calcination is: heating to the target temperature at a heating rate of 2° C. / min and then keeping the temperature for 1-2 hours;

[0028] Preferably, in step (3), the cordierite carrier is coated with aluminum gel three times by an immersion pulling method, and then calcined in a muffle furnace at 1000° C. after drying, and the temperature is raised to the target temperature at a heating rate of 2° C. / min and then kept at this temperature for 2 hours;

[0029] Preferably, the pore direction of the cordierite carrier described in step (3) should be perpendicular to the cross section (horizontal cross section) of the reactor, and the maximum size of the square or circular cross section of the cordierite carrier should be slightly smaller than the diameter of the reactor, so that it is restricted to vertical movement during rotation.

[0030] Furthermore, in step (4), the rotation rate of the reactor in the oven is 2-8 r / min. The temperature is raised to 120-150°C at a heating rate of 2-10°C / min, kept at that temperature for 9-24 hours, and then naturally cooled to room temperature.

[0031] Preferably, in step (4), in the rotary hydrothermal process, the rotation speed is controlled to 5 r / min, the temperature is increased to 120° C. at a heating rate of 5° C. / min, kept for 12 hours, and then naturally cooled to room temperature.

[0032] Furthermore, in step (5), the cleaning step is performed by rinsing the catalyst surface with deionized water, the drying step is performed in an oven at 80-120° C., and the calcination step is performed in a muffle furnace at 500-600° C. for 2-5 hours.

[0033] Preferably, the drying step in step (5) is performed in an oven at 80°C, and the calcining step is performed in a muffle furnace at 550°C for 3 hours.

[0034] The invention provides an integral low-carbon alkane catalyst prepared by a preparation method and having an active component grown in situ for catalytic combustion reaction of low-carbon alkane.

[0035] The integral light alkane catalyst with in-situ growth of active components provided by the invention can be applied in light alkane catalysis.

[0036] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0037] (1) The preparation method provided by the present invention is simple, green and environmentally friendly, and has high controllability. The obtained active component in-situ grown monolithic low-carbon alkane catalyst uses methane as a probe molecule. When the conversion rate is 10%, its conversion temperature is 281°C, and when the conversion rate is 90%, its conversion temperature is 320°C. It has high catalytic activity; no precious metals are required, which significantly reduces the preparation cost;

[0038] (2) The traditional method for preparing integral catalysts is a slurry coating method. The problem of active components being covered by inorganic adhesives in the slurry is difficult to solve. However, the present invention uses a process of in-situ growth of active components on the surface of the carrier to load the active components, which eliminates the problem of adhesive covering the active sites and improves the catalytic activity of low-carbon alkanes.

[0039] (3) The reason why the traditional in-situ growth process cannot be widely used is that the mechanical strength of the active components grown in situ decreases after calcination and they are easy to fall off. By doping with nickel ions, we found that the mechanical strength of the active components is significantly improved. This makes the in-situ growth process of active components applicable in industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.

[0041] Figure 1 A flow chart of a method for preparing a monolithic low-carbon alkane catalyst with in-situ growth of active components provided by the present invention;

[0042] Figure 2 The methane catalytic activity diagram of Examples 1-3 and Comparative Examples 1-2 of the present invention;

[0043] Figure 3 This is a physical picture of Example 2 of the present invention after the active component is grown in situ;

[0044] Figure 4 XRD comparison diagram between Examples 1-3 of the present invention and Co3O4 standard product;

[0045] Figure 5 is a SEM image of the cordierite carrier in Example 2 of the present invention;

[0046] Figure 6 This is a SEM image of the monolithic low-carbon alkane catalyst prepared in Example 2 of the present invention;

[0047] Figure 7 This is a SEM image of the monolithic low-carbon alkane catalyst prepared in Comparative Example 1 of the present invention;

[0048] Figure 8 This is a cyclic stability test diagram of Example 2 of the present invention. DETAILED DESCRIPTION

[0049] The following will be combined with the accompanying drawings and specific examples to further explain the detailed embodiments of the present invention, but it should be clear that the practical application and protection scope of the present invention are not limited thereto. It is worth noting that the technical processes not particularly described in detail in the following content are deemed to be self-implemented or fully understood by those skilled in the art based on the prior art knowledge. In addition, reagents or instruments that are not clearly marked as manufacturers are deemed to be standard products that can be widely purchased on the market.

[0050] The following examples are methods for preparing monolithic low-carbon alkane catalysts with in-situ growth of active components. Figure 1 shown.

[0051] Example 1

[0052] A method for preparing a monolithic low-carbon alkane catalyst with in-situ growth of active components comprises the following steps:

[0053] (1) Dissolve 14 mmol of cobalt nitrate hexahydrate and 1 mmol of nickel nitrate hexahydrate in 30 mL of deionized water, and dissolve 2 g of urea in 30 mL of deionized water. Combine the urea solution with the nitrate solution under vigorous stirring to obtain 60 mL of a mixed solution. Weigh 1.5 mmol of NH4F and 1 mmol of disodium ethylenediaminetetraacetate and add them to the mixed solution, and continue stirring for 2 hours.

[0054] (2) The cordierite carrier was treated with 5 mol / L nitric acid at 80°C, and then ultrasonically cleaned with deionized water for 3 times for use. 13 g of pseudo-boehmite was added to 100 ml of deionized water, fully dissolved in a water bath at 80°C, and 3 ml of 5 mol / L nitric acid solution was added dropwise. When the aluminum gel turned into a milky white liquid, it indicated that the aluminum gel was successfully prepared. The aluminum gel was coated by the immersion pulling method for 3 times, and after drying, it was calcined in a muffle furnace at 1000°C for 1 hour.

[0055] (3) The cordierite carrier coated with aluminum gel is placed in a reactor, and 60 ml of the precursor solution is added thereto. The reactor is transferred to an oven with a rotating function for hydrothermal reaction, the rotation rate is set to 5 r / min, the temperature is increased to 120°C at a heating rate of 2°C / min, and then kept warm for 12 hours, and naturally cooled to room temperature to obtain a monolithic catalyst loaded with the precursor.

[0056] (4) The hydrothermally completed monolithic catalyst is dried and transferred to a muffle furnace for calcination, and the temperature is raised to 500° C. at a heating rate of 2° C. / min and kept at this temperature for 3 hours, thereby obtaining a monolithic low-carbon alkane catalyst with in-situ growth of active components.

[0057] Example 2

[0058] A method for preparing a monolithic low-carbon alkane catalyst with in-situ growth of active components comprises the following steps:

[0059] (1) Dissolve 12.5 mmol of cobalt nitrate hexahydrate and 2.5 mmol of nickel nitrate hexahydrate in 30 mL of deionized water, and dissolve 2 g of urea in 30 mL of deionized water. Combine the urea solution with the nitrate solution under vigorous stirring to obtain 60 mL of a mixed solution. Weigh 1.5 mmol of NH4F and 1 mmol of disodium ethylenediaminetetraacetate and add them to the mixed solution, and continue stirring for 2 hours.

[0060] (2) The cordierite carrier was treated with 5 mol / L nitric acid at 80°C, and then ultrasonically cleaned with deionized water for 3 times for use. 13 g of pseudo-boehmite was added to 100 ml of deionized water, fully dissolved in a water bath at 80°C, and 3 ml of 5 mol / L nitric acid solution was added dropwise. When the aluminum gel turned into a milky white liquid, it indicated that the aluminum gel was successfully prepared. The aluminum gel was coated by the immersion pulling method for 3 times, and after drying, it was calcined in a muffle furnace at 1000°C for 1 hour.

[0061] (3) The cordierite carrier coated with aluminum gel is placed in a reactor, and 60 ml of the precursor solution is added thereto. The reactor is transferred to an oven with a rotating function for hydrothermal reaction, the rotation rate is set to 5 r / min, the temperature is increased to 120°C at a heating rate of 2°C / min, and then kept warm for 12 hours, and naturally cooled to room temperature to obtain a monolithic catalyst loaded with the precursor.

[0062] (4) The hydrothermally completed monolithic catalyst is dried and transferred to a muffle furnace for calcination, and the temperature is raised to 500° C. at a heating rate of 2° C. / min and kept at this temperature for 3 hours, thereby obtaining a monolithic low-carbon alkane catalyst with in-situ growth of active components.

[0063] Example 3

[0064] An integral light alkane catalyst with in-situ growth of active components comprises the following steps:

[0065] (1) Dissolve 10 mmol of cobalt nitrate hexahydrate and 5 mmol of nickel nitrate hexahydrate in 30 mL of deionized water, and dissolve 2 g of urea in 30 mL of deionized water. Combine the urea solution with the nitrate solution under vigorous stirring to obtain 60 mL of a mixed solution. Weigh 1.5 mmol of NH4F and 1 mmol of disodium ethylenediaminetetraacetate and add them to the mixed solution, and continue stirring for 2 hours.

[0066] (2) The cordierite carrier was treated with 5 mol / L nitric acid at 80°C, and then ultrasonically cleaned with deionized water for 3 times for use. 13 g of pseudo-boehmite was added to 100 ml of deionized water, fully dissolved in a water bath at 80°C, and 3 ml of 5 mol / L nitric acid solution was added dropwise. When the aluminum gel turned into a milky white liquid, it indicated that the aluminum gel was successfully prepared. The aluminum gel was coated by the immersion pulling method for 3 times, and after drying, it was calcined in a muffle furnace at 1000°C for 1 hour.

[0067] (3) The cordierite carrier coated with aluminum gel is placed in a reactor, and 60 ml of the precursor solution is added thereto. The reactor is transferred to an oven with a rotating function for hydrothermal reaction, the rotation rate is set to 5 r / min, the temperature is increased to 120°C at a heating rate of 2°C / min, and then kept warm for 12 hours, and naturally cooled to room temperature to obtain a monolithic catalyst loaded with the precursor.

[0068] (4) The hydrothermally completed monolithic catalyst is dried and transferred to a muffle furnace for calcination, and the temperature is raised to 500° C. at a heating rate of 2° C. / min and kept at this temperature for 3 hours, thereby obtaining a monolithic low-carbon alkane catalyst with in-situ growth of active components.

[0069] Example 4

[0070] A method for preparing a monolithic low-carbon alkane catalyst with in-situ growth of active components comprises the following steps:

[0071] (1) Dissolve 12.5 mmol of cobalt nitrate hexahydrate and 2.5 mmol of nickel nitrate hexahydrate in 30 mL of deionized water, and dissolve 2 g of urea in 30 mL of deionized water. Combine the urea solution with the nitrate solution under vigorous stirring to obtain 60 mL of a mixed solution. Weigh 1.5 mmol of NH4F and 1 mmol of disodium ethylenediaminetetraacetate and add them to the mixed solution, and continue stirring for 2 hours.

[0072] (2) The cordierite carrier was treated with 5 mol / L nitric acid at 80°C, and then ultrasonically cleaned with deionized water for 3 times for use. 13 g of pseudo-boehmite was added to 100 ml of deionized water, fully dissolved in a water bath at 80°C, and 3 ml of 5 mol / L nitric acid solution was added dropwise. When the aluminum gel turned into a milky white liquid, it indicated that the aluminum gel was successfully prepared. The aluminum gel was coated by the immersion pulling method for 3 times, and after drying, it was calcined in a muffle furnace at 1000°C for 1 hour.

[0073] (3) The cordierite carrier coated with aluminum gel was placed in a reactor, and 60 ml of the precursor solution was added thereto. The reactor was transferred to an oven with a rotating function for hydrothermal reaction, the rotation rate was set to 2 r / min, the temperature was raised to 120°C at a heating rate of 2°C / min, and then kept warm for 9 hours, and naturally cooled to room temperature to obtain a monolithic catalyst loaded with the precursor.

[0074] (4) The hydrothermally completed monolithic catalyst is dried and transferred to a muffle furnace for calcination, and the temperature is raised to 500° C. at a heating rate of 2° C. / min and kept at this temperature for 2 hours, thereby obtaining a monolithic low-carbon alkane catalyst with in-situ growth of active components.

[0075] Example 5

[0076] A method for preparing a monolithic low-carbon alkane catalyst with in-situ growth of active components comprises the following steps:

[0077] (1) Dissolve 12.5 mmol of cobalt nitrate hexahydrate and 2.5 mmol of nickel nitrate hexahydrate in 30 mL of deionized water, and dissolve 2 g of urea in 30 mL of deionized water. Combine the urea solution with the nitrate solution under vigorous stirring to obtain 60 mL of a mixed solution. Weigh 1.0 mmol of NH4F and 0.75 mmol of disodium ethylenediaminetetraacetate and add them to the mixed solution, and continue stirring for 2 hours.

[0078] (2) The cordierite carrier was treated with 5 mol / L nitric acid at 80°C, and then ultrasonically cleaned with deionized water for 3 times for use. 15 g of pseudo-boehmite was added to 100 ml of deionized water, fully dissolved in a water bath at 80°C, and 3 ml of 5 mol / L nitric acid solution was added dropwise. When the aluminum gel turned into a milky white liquid, it indicated that the aluminum gel was successfully prepared. The aluminum gel was coated by the immersion pulling method for 3 times, and after drying, it was calcined in a muffle furnace at 1200°C for 2 hours.

[0079] (3) The cordierite carrier coated with aluminum gel is placed in a reactor, and 60 ml of the precursor solution is added thereto. The reactor is transferred to an oven with a rotating function for hydrothermal reaction, the rotation rate is set to 8 r / min, the temperature is increased to 150°C at a heating rate of 10°C / min, and then kept warm for 24 hours, and naturally cooled to room temperature to obtain a monolithic catalyst loaded with the precursor.

[0080] (4) The hydrothermally completed monolithic catalyst is dried and transferred to a muffle furnace for calcination, and the temperature is raised to 600° C. at a heating rate of 5° C. / min and kept at this temperature for 5 hours, thereby obtaining a monolithic low-carbon alkane catalyst with in-situ growth of active components.

[0081] Comparative Example 1

[0082] A method for preparing a monolithic low-carbon alkane catalyst with in-situ growth of active components comprises the following steps:

[0083] (1) Dissolve 15 mmol of cobalt nitrate hexahydrate in 30 mL of deionized water and 2 g of urea in 30 mL of deionized water. Combine the urea solution with the nitrate solution under vigorous stirring to obtain 60 mL of a mixed solution. Weigh 1.5 mmol of NH4F and 1 mmol of disodium ethylenediaminetetraacetate and add them to the mixed solution. Stir for 2 hours.

[0084] (2) The cordierite carrier was treated with 5 mol / L nitric acid at 80°C, and then ultrasonically cleaned with deionized water for 3 times for use. 13 g of pseudo-boehmite was added to 100 ml of deionized water, fully dissolved in a water bath at 80°C, and 3 ml of 5 mol / L nitric acid solution was added dropwise. When the aluminum gel turned into a milky white liquid, it indicated that the aluminum gel was successfully prepared. The aluminum gel was coated by the immersion pulling method for 3 times, and after drying, it was calcined in a muffle furnace at 1000°C for 1 hour.

[0085] (3) The cordierite carrier coated with aluminum gel is placed in a reactor, and 60 ml of the precursor solution is added thereto. After aging at room temperature for 2 hours, the reactor is transferred to an oven with a rotating function for hydrothermal reaction. The rotation rate is set to 5 r / min, and the temperature is increased to 120°C at a heating rate of 2°C / min. The temperature is then kept at this temperature for 12 hours, and the temperature is naturally cooled to room temperature to obtain a monolithic catalyst loaded with the precursor.

[0086] (4) The hydrothermally completed monolithic catalyst is dried and transferred to a muffle furnace for calcination, and the temperature is raised to 500°C at a heating rate of 2°C / min and kept at this temperature for 3 hours. Thus, a monolithic low-carbon alkane catalyst with in-situ growth of active components is obtained.

[0087] Comparative Example 2

[0088] The cordierite carrier was treated with 5mol / L nitric acid at 80°C, and then ultrasonically cleaned with deionized water for 3 times for use. 13g of pseudo-boehmite was added to 100ml of deionized water, fully dissolved in a water bath at 80°C, and 3ml of 5mol / L nitric acid solution was added dropwise. When the aluminum gel turned into a milky white liquid, the aluminum gel was successfully prepared. The aluminum gel was coated by the immersion pulling method for 3 times, and after drying, it was calcined at 1000°C in a muffle furnace for 1 hour. The cordierite carrier treated with acid and coated with aluminum gel was obtained. Since there are metal ions such as Al, Mg, and Ga in cordierite, they may have a catalytic effect on low-carbon alkanes, so a comparative example was made to exclude this effect.

[0089] The effect of the present invention is verified:

[0090] The monolithic low-carbon alkane catalysts with in-situ growth of active components prepared in Examples 1-5 were respectively tested for catalytic combustion of methane.

[0091] 1. Test of catalyst activity

[0092] The test method of catalyst activity comprises the following steps:

[0093] The monolithic low-carbon alkane catalyst with in-situ growth of active components obtained in Examples 1-5 and Comparative Examples 1 and 2 was cored by a quartz sand opener to obtain a cylindrical monolithic catalyst with a diameter of 18 mm and a length of 50 mm. The obtained catalyst was loaded into a quartz tube reactor with an inner diameter of 18 mm and a length of 400 mm; quartz wool was filled at both ends of the catalyst bed, and the reaction atmosphere introduced into the quartz tube reactor was composed of 1% CH4 and 20% O2 balanced in N2, and the total flow rate was controlled to be 100 mL / min. A gas chromatograph (Shimadzu 2014C) equipped with a double flame ionization detector (FID) was used to monitor the concentration of the reactants and the generation of catalytic oxidation products in real time, wherein the CH4 concentration was detected by an FID detector, and the catalytic activity data at each temperature point was obtained after 60 minutes of stable reaction at each temperature point until the temperature was raised to 600°C.

[0094] The results are as follows Figure 2 As shown in Table 1 below, Figure 2 The methane catalytic combustion activity diagram of the catalysts prepared in Examples 1-3 is shown in FIG. Figure 2 As shown in Table 1, the catalysts prepared in Examples 1-3 of the present invention all have excellent catalytic activity, among which the catalyst prepared in Example 2 has the best effect. When the conversion temperature is 300°C, the methane conversion rate is 98%. It is much higher than the pure cobalt monolithic catalyst prepared in Comparative Example 1. Compared with the traditional precious metal catalyst, the present invention has high catalytic activity, no need to add precious metals, and low preparation cost; secondly, the doping amount of nickel ions in Examples 1 and 3 is adjusted during the preparation process, and the monolithic catalyst activity is lower than that of the monolithic catalyst prepared in Example 2, indicating that when Ni / Co=1:5, the monolithic catalyst has the best methane catalytic efficiency. The catalytic activity of Examples 1-5 has obvious advantages over Comparative Example 1, which also illustrates the positive effect of nickel doping on improving activity. Examples 4 and 5 compare the effects of operating parameters on nickel-doped catalysts. The results show that high temperature and long-term calcination may cause sintering of the catalyst, resulting in a slight decrease in activity. The catalytic activity of Comparative Example 2 is 0% at all temperature points, indicating that the metal elements in the carrier have no contribution to the catalytic oxidation of low-carbon alkanes.

[0095] Table 1

[0096]

[0097]

[0098] 2. Active components and mechanical strength test

[0099] The biggest problem with the monolith prepared by the in-situ growth process is that the mechanical strength of the active components is low and the active components are easy to fall off. Therefore, it is necessary to test the mechanical strength of the active components of the monolithic catalyst. The test method for the mechanical strength of the active components of the catalyst includes the following steps: weighing the monolithic catalyst sample and recording the mass. Place the catalyst in a beaker and add deionized water to cover the surface of the catalyst. Place the beaker in an ultrasonic cleaning machine, adjust the ultrasonic frequency to 20KHz, the power density to 0.3W / cm2, and the ultrasonic time to 10min. After the ultrasonic sample is completely dried, weigh it again. The mass change results of the catalyst are shown in Table 2.

[0100] Table 2

[0101] Before load(g) After load (g) Load rate (%) After ultrasound (g) Dropout rate (%) Example 1 6.6384 7.1851 8.24 7.1034 14.94 Example 2 6.7946 7.4851 10.16 7.4551 4.34 Example 3 6.931 7.5951 9.58 7.5654 4.47 Comparative Example 1 6.8416 7.1134 3.97 7.0440 25.53

[0102] The results of the mass change of the catalyst are shown in Table 2. From Table 2, it can be seen that the shedding rate of the active components of the catalysts prepared in Examples 2 and 3 of the present invention is significantly lower than that of Comparative Example 1, indicating that the monolithic catalyst preparation methods of Examples 2 and 3 are helpful in improving the mechanical strength of the active components. Figure 6 As shown in FIG. 1 , it can be found that a regular nanoarray grows on the surface of the carrier, which is a key factor for high catalytic activity and high mechanical strength. Figure 7 As shown, there is no obvious regular structure on the carrier surface, and a flower-like cluster structure can be observed.

[0103] 3. Catalyst cyclic stability test

[0104] The monolithic low-carbon alkane catalyst with in-situ growth of active components obtained in Example 2 was cored with a quartz sand hole opener to obtain a cylindrical monolithic catalyst with a diameter of 18 mm and a length of 50 mm. The obtained catalyst was loaded into a quartz tube reactor with an inner diameter of 18 mm and a length of 400 mm; quartz wool was filled at both ends of the catalyst bed, and the reaction atmosphere introduced into the quartz tube reactor was composed of 1% CH4 and 20% O2 in N2 in a balanced manner, and the total flow rate was controlled to be 100 mL / min; a gas chromatograph (Shimadzu 2014C) equipped with a double flame ionization detector (FID) was used to monitor the concentration of reactants and the generation of catalytic oxidation products in real time, wherein the FID detector was used to detect the CH4 concentration, and the catalytic activity data at each temperature point was obtained after 60 minutes of stable reaction at each temperature point until the temperature was raised to 600°C. Repeat the above operation 3 times to determine the cyclic stability of the catalyst obtained in Example 2.

[0105] Figure 8 This is a graph showing the stability of the methane catalytic combustion cycle of a monolithic low-carbon alkane catalyst with in-situ growth of active components prepared in Example 2. Figure 8It can be seen from the above that the catalyst prepared in Example 2 has excellent methane catalytic combustion cycle stability.

[0106] The above embodiments are only preferred implementation modes of the present invention and are only used to explain the present invention rather than to limit the present invention. Any changes, substitutions, modifications, etc. made by those skilled in the art without departing from the spirit of the present invention should fall within the scope of protection of the present invention.

Claims

1. A method for preparing a monolithic low-carbon alkane catalyst with in-situ growth of active components, characterized in that: The steps include: (1) dissolving a metal nitrate and urea in deionized water respectively to obtain a metal nitrate solution and a urea solution, and adding the urea solution dropwise to the metal nitrate solution under stirring to obtain a clear mixed solution; (2) adding NH4F and disodium ethylenediaminetetraacetate to the clarified mixed solution to obtain a clarified precursor solution; (3) treating the cordierite carrier with acid, coating it with aluminum gel and calcining it, then placing the cordierite carrier in a reaction kettle and adding the precursor solution obtained in step (2); (4) transferring the reactor containing the cordierite carrier in step (3) to an oven with a rotating function for hydrothermal reaction to obtain a monolithic catalyst loaded with active components; (5) The integral catalyst obtained in step (4) is cleaned, dried, and calcined under air conditions to obtain an integral low-carbon alkane catalyst with in-situ growth of the active components.

2. The method for preparing the monolithic light alkane catalyst with in-situ growth of active components according to claim 1, characterized in that: In step (1), the molar ratio of the metal nitrate to urea is 1:2-1:5; the concentration of the metal nitrate solution is 0.4-0.6 mol / L; the metal nitrate comprises cobalt nitrate and nickel nitrate, and the molar ratio of the cobalt nitrate to the nickel nitrate is 2:1-14:1; the concentration of the urea solution is 0.8-1.2 mol / L; and the stirring rate is 1000-2000 rpm.

3. The method for preparing the monolithic light alkane catalyst with in-situ growth of active components according to claim 1, characterized in that: In step (2), the molar ratio of NH4F to metal nitrate is 1:10-1:15, and the molar ratio of disodium ethylenediaminetetraacetate to metal nitrate is 1:15-1:

20.

4. The method for preparing the monolithic light alkane catalyst with in-situ growth of active components according to claim 1, characterized in that: In step (3), the cordierite carrier is subjected to acid treatment and then aluminum gel coating and calcination are specifically: 4-6 mol / L nitric acid is used for acid treatment, the acid treatment temperature is controlled to be 80-90° C., and the acid treatment time is 1-2 hours; after the acid treatment is completed, ultrasonic cleaning is performed in deionized water, and the water is changed 3-4 times, and then the aluminum gel coating and calcination step is performed after drying; The aluminum gel coating and calcining steps are: using an immersion and pulling method to coat the cordierite carrier with aluminum gel 3-4 times, and then calcining in a muffle furnace at 1000-1200° C. after drying; the calcining is: heating to the target temperature at a heating rate of 2° C. / min and then keeping the temperature for 1-2 hours; The synthesis method of the aluminum colloid is as follows: 13-15 g of pseudo-boehmite is added to every 100 ml of deionized water, fully dissolved and heated to 80-85° C., 2-3 ml of 5 mol / L nitric acid solution is added, and stirred until the solution is a milky white clear colloid.

5. The method for preparing the monolithic light alkane catalyst with in-situ growth of active components according to claim 1, characterized in that: In step (3), the pore direction of the cordierite carrier is perpendicular to the horizontal cross section of the reactor; the maximum size of the square or circular cross section of the cordierite carrier should be slightly smaller than the diameter of the reactor so that it is restricted to move in a vertical direction during rotation.

6. The method for preparing the monolithic light alkane catalyst with in-situ growth of active components according to claim 1, characterized in that: In step (4), the rotation rate of the reactor in the oven is 2-8 r / min; the hydrothermal reaction is: heating to 120-150°C at a heating rate of 2-10°C / min, keeping warm for 9-24 hours, and then naturally cooling to room temperature.

7. The method for preparing the monolithic light alkane catalyst with in-situ growth of active components according to claim 1, characterized in that: In step (4), the rotation rate of the reactor in the oven is 2-8 r / min; the hydrothermal reaction is: heating to 120-150°C at a heating rate of 2.5-5°C / min, keeping warm for 12-24 hours, and then naturally cooling to room temperature.

8. The method for preparing the monolithic light alkane catalyst with in-situ growth of active components according to claim 1, characterized in that: In step (5), the cleaning is: rinsing the catalyst surface with deionized water; the drying is completed in an oven at 80-120° C.; and the calcination step is performed in a muffle furnace at 500-600° C. for 2-5 hours.

9. An integral light alkane catalyst with in-situ growth of active components prepared by the preparation method according to any one of claims 1 to 7.

10. Use of the monolithic light alkane catalyst with in-situ growth of active components as claimed in claim 9 in light alkane catalysis.

Citation Information

Patent Citations

  • Nitrogen-doped carbon-coated cobaltosic oxide nanowire monolithic catalyst and preparation method thereof

    CN112536055A

  • Efficient soot catalytic oxidation monolithic catalyst and preparation method thereof

    CN115814802A

  • Efficient monolithic catalyst for catalytic oxidation of OVOCs (Organic Volatile Organic Compounds) as well as preparation method and application of efficient monolithic catalyst

    CN116273024A

  • Preparation method and application of multi-stage cobalt-manganese spinel array photo-thermal catalyst

    CN116920868A

  • Monolithic VOCs (Volatile Organic Compounds) catalyst with multiple active component layers as well as preparation method and application of monolithic VOCs catalyst

    CN118217997A

Cited By

  • Quenching silver-loaded cobalt-based monolithic catalyst as well as preparation method and application thereof

    CN119281352A

  • A quenched silver-loaded cobalt-based monolithic catalyst and its preparation method and application