Preparation method and application of NiFe LDH oxygen evolution catalyst with bimetal cation vacancy introduced
By introducing Ni2+ and Fe3+ bimetallic cation vacancies into the NiFe LDH basal surface and adjusting the electronic structure, the problem of insufficient catalytic activity and stability of NiFe LDH in alkaline seawater electrolysis was solved, achieving efficient seawater decomposition and improved stability.
Patent Information
- Application Number
- CN202411147188.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-12
AI Technical Summary
The existing pure-phase NiFe LDH exhibits low catalytic activity and insufficient stability in alkaline seawater electrolysis, making it difficult to effectively decompose Cl- and OER in seawater, thus affecting the water decomposition efficiency.
By introducing Ni2+ and Fe3+ bimetallic cation vacancies into the NiFe LDH basal plane, and adjusting the electronic structure through electrochemical deposition and alkaline etching, the binding energy between the metal and oxygen is enhanced, thus promoting the evolution of the NiFeOOH active phase.
It improves the catalytic activity and stability of NiFe LDH, making it suitable for large-scale production. It is also suitable for the efficient decomposition of seawater in alkaline environments, reducing overpotential and extending service life.
Smart Images

Figure CN118932379A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the fields of electrocatalysis and energy, specifically to a method for preparing and applying a NiFe LDH oxygen evolution catalyst with introduced bimetallic cation vacancies. Background Technology
[0002] Hydrogen energy, as a clean and renewable energy source that can replace traditional fossil fuels and alleviate the energy crisis, has received increasing attention. Seawater electrolysis for hydrogen production is considered a promising energy conversion strategy. However, the application of seawater electrolysis is hindered by its complex composition, such as the presence of Cl- as a major component. - (~0.55 M), Na + (~0.48 M), Mg 2+ (~0.05 M), etc. On the anode side, especially Cl... - The chlorine evolution reaction (ClER) has a similar thermodynamic equilibrium potential to the oxygen evolution reaction (OER), but its kinetic reaction rate is faster, allowing it to compete with OER and severely impacting water decomposition efficiency. An alkaline environment can inhibit ClER and simultaneously increase the alkaline environment. 2+ and Mg 2+ It is converted into a precipitate, thereby removing Ca. 2+ Mg 2+ However, hypochlorite formation in alkaline environments can still compete with OER, but the onset potential is 490 mV higher than that of OER, indicating that achieving 100% seawater oxidation without being affected by ClO is more difficult. - The overpotential of the OER should not exceed 490 mV.
[0003] NiFe layered double hydroxides (NiFe LDHs) show great promise for application in alkaline environments due to their abundant reserves, inherent high activity, and tunable chemical composition. However, the low basal activity and insufficient long-term stability of pure-phase NiFe LDHs limit their application in alkaline seawater electrocatalysis. Summary of the Invention
[0004] This invention overcomes the shortcomings of existing technologies and provides a method for preparing a NiFe LDH oxygen evolution catalyst by introducing bimetallic cation vacancies. The method of this invention introduces Ni into the NiFe LDH basal surface... 2+ and Fe 3+ The bimetallic cation vacancies modulate the basal electronic structure of NiFe LDH, enhance the binding energy between metal and oxygen in LDH, and accelerate the evolution of the NiFeOOH active phase, thereby improving the catalytic activity and stability of NiFe LDH. This method is easy to operate, has high preparation efficiency, low cost, and is suitable for large-scale production.
[0005] To solve the above-mentioned technical problems, the technical solution adopted in this invention is as follows: a method for preparing a NiFe LDH oxygen evolution catalyst with introduced bimetallic cation vacancies, firstly, NiZnFeAl LDH is prepared by electrochemical deposition, and then Ni is introduced onto the NiFe LDH substrate by alkaline etching. 2+ and Fe 3+ The oxygen evolution catalyst is obtained by filling the bimetallic cation vacancy.
[0006] As a further limitation of the technical solution of the present invention, the preparation method specifically includes the following steps: (1) Dissolve nickel nitrate, ferric nitrate, aluminum chloride and zinc chloride in ultrapure water and stir until dissolved to obtain a homogeneous mixed solution for later use; (2) The mixed solution obtained in step (1) is transferred into a three-electrode electrolytic cell and a voltage is applied to carry out the reaction. The working electrode is nickel foam NF, the auxiliary electrode is a platinum mesh electrode, and the reference electrode is an Ag / AgCl electrode. (3) The working electrode obtained in step (2) is washed with ultrapure water and dried naturally to obtain NiZnFeAl LDH nanosheet oxygen evolution catalyst; (4) The NiZnFeAl LDH nanosheet oxygen evolution catalyst obtained in step (3) is transferred to NaOH and soaked for a period of time for alkaline etching; (5) The NiZnFeAl LDH catalyst after alkaline etching in step (4) is washed with ultrapure water and dried naturally to finally obtain the NiFe LDH oxygen evolution catalyst with bimetallic cation vacancies.
[0007] As a further limitation of the technical solution of the present invention, in step (1), the concentration of nickel nitrate and ferric nitrate in the mixed solution is 0.12 M; the concentration of aluminum chloride and zinc chloride is 0.5 ~ 2 mM, and the concentration ratio of aluminum chloride and zinc chloride is maintained at 1:1.
[0008] As a further limitation of the technical solution of the present invention, the size of the platinum mesh electrode in step (2) is 1×1 cm; in step (2), the reaction temperature is 25℃, the applied voltage is -1.0 V, and the reaction time is 10~500 s.
[0009] As a further limitation of the technical solution of the present invention, in step (4), the alkaline etching reaction temperature is 25°C, the NaOH concentration is 5 M, and the alkaline etching time is 3~12 h.
[0010] The present invention also provides a NiFe LDH oxygen evolution catalyst with introduced bimetallic cation vacancies obtained by the above preparation method.
[0011] The present invention also provides the application of the NiFe LDH oxygen evolution catalyst with introduced bimetallic cation vacancies obtained by the above preparation method in electrocatalysis.
[0012] In addition, the present invention also provides a method for preparing NiZnFeAl LDH nanosheet oxygen evolution catalyst, comprising the following steps: (1) Dissolve nickel nitrate, ferric nitrate, aluminum chloride and zinc chloride in ultrapure water and stir until dissolved to obtain a homogeneous mixed solution for later use; the concentration of nickel nitrate and ferric nitrate in the mixed solution is 0.12 M; the concentration of aluminum chloride and zinc chloride is 0.5 ~ 2 mM, and the concentration ratio of aluminum chloride and zinc chloride is maintained at 1:1. (2) The mixed solution obtained in step (1) is transferred into a three-electrode electrolytic cell and a voltage is applied to carry out the reaction. The working electrode is nickel foam NF, the auxiliary electrode is a platinum mesh electrode, and the reference electrode is an Ag / AgCl electrode. (3) The working electrode obtained in step (2) is washed with ultrapure water and dried naturally to obtain NiZnFeAl LDH nanosheet oxygen evolution catalyst.
[0013] The present invention also provides a NiZnFeAl LDH nanosheet oxygen evolution catalyst obtained by the above preparation method.
[0014] The present invention also provides the application of the NiZnFeAl LDH nanosheet oxygen evolution catalyst obtained by the above preparation method in electrocatalysis.
[0015] Compared with the prior art, the present invention has the following beneficial effects: 1. The method of this invention introduces Ni into the NiFe LDH basal plane. 2+ and Fe 3+ The bimetallic cation vacancies regulate the basal electronic structure of NiFeLDH, enhance the binding energy between metal and oxygen in LDH, and accelerate the evolution of the NiFeOOH active phase, thereby improving the catalytic activity and stability of NiFe LDH for seawater decomposition.
[0016] 2. The NiFe LDH oxygen evolution catalyst with bimetallic cation vacancies disclosed in this invention has a nanosheet structure and contains vacancies of two metal cations, exhibiting high activity and stability and a long service life.
[0017] 3. This invention employs electrochemical deposition and alkaline etching methods, which provide mild preparation conditions, are easy to operate, have high preparation efficiency, low cost, and are suitable for large-scale production. Attached Figure Description
[0018] Figure 1 The image shows the elemental mapping of the NiZnFeAl LDH oxygen evolution catalyst obtained in Example 1.
[0019] Figure 2 Product V obtained in Example 2 NiFe - Scanning electron microscope (SEM) image of NiFe LDH oxygen evolution catalyst.
[0020] Figure 3 Product V obtained in Example 2 NiFe - Electron paramagnetic resonance (ERP) spectrum of NiFe LDH oxygen evolution catalyst.
[0021] Figure 4 Product V obtained in Example 2 NiFe - X-ray photoelectron spectroscopy (XPS) of NiFe LDH oxygen evolution catalyst.
[0022] Figure 5 Product V obtained in Example 2 NiFe Raman spectra of NiFe LDH oxygen evolution catalysts after oxygen evolution for 30 min at voltages of 1.4 V and 1.6 V, respectively.
[0023] Figure 6 Product V obtained in Example 2 NiFe -NiFe LDH oxygen evolution catalyst oxygen evolution polarization curves in simulated seawater (with iR compensation) (a) and at 50 mA cm⁻¹ -2 The timing potential curve (b) is shown below. Detailed Implementation
[0024] The present invention will be further described below with reference to specific embodiments.
[0025] Example 1 (Preparation of NiZnFeAl LDH nanosheet oxygen evolution catalyst) A method for preparing a NiZnFeAl LDH oxygen evolution catalyst includes the following steps: (1) Dissolve nickel nitrate (0.12 M), ferric nitrate (0.12 M), aluminum chloride (0.001 M) and zinc chloride (0.001 M) in ultrapure water and stir until dissolved to obtain a homogeneous mixed solution for later use; (2) The solution obtained in step (1) was transferred into a three-electrode electrolytic cell and electrochemical deposition reaction was carried out at room temperature (25°C) with a voltage of -1.0 V and a reaction time of 50 s. The working electrode used was nickel foam NF, the auxiliary electrode was a platinum mesh electrode (1×1 cm), and the reference electrode was an Ag / AgCl electrode. (3) The working electrode obtained in step (2) is washed with ultrapure water and dried naturally at room temperature (25°C) to finally obtain NiZnFeAl LDH nanosheet oxygen evolution catalyst.
[0026] The elemental mapping diagram of the NiZnFeAl LDH oxygen evolution catalyst obtained in this example (as shown in the figure) Figure 1 The results show that Zn and Al atoms are uniformly distributed in NiFe LDH, indicating the successful preparation of the NiZnFeAl LDH oxygen evolution catalyst.
[0027] Example 2 (V) NiFe (Preparation of NiFe LDH oxygen evolution catalyst) A V NiFe The preparation method of NiFe LDH (i.e., NiFe LDH with introduced bimetallic cation vacancies) oxygen evolution catalyst includes the following steps: (1) Dissolve nickel nitrate (0.12 M), ferric nitrate (0.12 M), aluminum chloride (0.001 M) and zinc chloride (0.001 M) in ultrapure water and stir until dissolved to obtain a homogeneous mixed solution for later use; (2) The solution obtained in step (1) was transferred into a three-electrode electrolytic cell and electrochemical deposition reaction was carried out at room temperature (25°C) with a voltage of -1.0 V and a reaction time of 100 s. The working electrode used was nickel foam NF, the auxiliary electrode was a platinum mesh electrode (1×1 cm), and the reference electrode was an Ag / AgCl electrode. (3) The working electrode obtained in step (2) is washed with ultrapure water and dried naturally at room temperature (25°C) to finally obtain NiZnFeAl LDH nanosheet oxygen evolution catalyst.
[0028] (4) The NiZnFeAl LDH catalyst obtained in step (3) was transferred to 5 M NaOH and soaked at room temperature (25°C) for 9 hours.
[0029] (5) The NiZnFeAl LDH catalyst etched by alkali in step (4) was washed with ultrapure water and dried naturally at room temperature (25°C) to finally obtain V. NiFe -NiFe LDH oxygen evolution catalyst.
[0030] V obtained in this example NiFe Taking NiFe LDH oxygen evolution catalyst as an example, SEM analysis was performed (e.g. Figure 2 It can be seen that it is in the form of nanosheets. EPR spectrum (such as...) Figure 3 Ni 2+ Fe 3+ V enriched by bimetallic cation vacancies NiFe The EPR signal intensity of -NiFe LDH is significantly higher than that of Ni prepared under the same conditions. 2+ or Fe 3+ V enriched by single-metal cation vacancies Ni -NiFe LDH or V Fe-NiFe LDH indicates that Ni 2+ Fe 3+ The successful introduction of bimetallic cation vacancies. For V NiFe -NiFe LDH was analyzed by XPS (e.g. Figure 4 It can be seen that the introduction of Ni and Fe vacancies alters the electronic structure of the NiFe LDH surface, making Ni 3+ The increased content enhanced the interaction between metallic Ni and O. Raman spectroscopy was performed on the electrodes after electrolysis at 1.4 V and 1.6 V for 30 min, respectively (e.g., ...). Figure 5 ), it can be seen that V NiFe -NiFe LDH is more easily converted into the oxygen evolution active component Ni 2+δ -O-Fe 3+ζ O x H y This improves catalytic activity.
[0031] The V prepared in this example NiFe The electrochemical oxygen evolution performance of NiFe LDH was tested in simulated seawater (1 M KOH + 0.5 M NaCl) under the following conditions: ambient temperature (25 °C), ambient pressure (1 atm), and a three-electrode system (working electrode: V). NiFe -NiFeLDH / NF electrode (1 cm × 1 cm), auxiliary electrode: Pt electrode (0.5 mm × 1 cm), reference electrode: Hg / HgO). Linear voltammetry curves were obtained using a stepwise linear scan voltammetry method (scan rate 2 mV / s). -1 Electrode stability was tested using the chronopotential method.
[0032] like Figure 6 As shown, in this example, V NiFe -NiFe LDH exhibited excellent OER catalytic activity and stability in simulated seawater electrolysis, with a stability at 10 mA cm⁻¹. -2 The oxygen evolution overpotential at 215 mV is at 50 mA cm⁻¹. -2 The overpotential increased by only 10 mV after 8 days (192 h) of testing, which is a significant improvement in oxygen evolution activity and stability compared to NiFe LDH.
[0033] Example 3 (V) NiFe (Preparation of NiFe LDH oxygen evolution catalyst) A V NiFe The preparation method of NiFe LDH (i.e., NiFe LDH with introduced bimetallic cation vacancies) oxygen evolution catalyst includes the following steps: (1) Dissolve nickel nitrate (0.12 M), ferric nitrate (0.12 M), aluminum chloride (0.001 M) and zinc chloride (0.001 M) in ultrapure water and stir until dissolved to obtain a homogeneous mixed solution for later use; (2) The solution obtained in step (1) was transferred into a three-electrode electrolytic cell and electrochemical deposition reaction was carried out at room temperature (25°C) with a voltage of -1.0 V and a reaction time of 100 s. The working electrode used was nickel foam NF, the auxiliary electrode was a platinum mesh electrode (1×1 cm), and the reference electrode was an Ag / AgCl electrode. (3) The working electrode obtained in step (2) is washed with ultrapure water and dried naturally at room temperature to finally obtain NiZnFeAl LDH nanosheet oxygen evolution catalyst.
[0034] (4) The NiZnFeAl LDH catalyst obtained in step (3) is transferred to 5 M NaOH and soaked at room temperature (25°C) for 3 hours.
[0035] (5) The NiZnFeAl LDH catalyst etched by alkali in step (4) was washed with ultrapure water and dried naturally at room temperature to finally obtain V. NiFe -NiFe LDH oxygen evolution catalyst.
[0036] The V obtained in this example NiFe -NiFe LDH oxygen evolution catalyst in simulated seawater electrolysis at 10 mA cm⁻¹ -2 The oxygen evolution overpotential at the point is 230 mV.
[0037] The above description is merely a preferred embodiment of this application and should not be construed as limiting the scope of the invention. Any technical solutions obtained by those skilled in the art based on this invention through logical analysis and reasoning on the existing technology should be within the scope of protection of these claims.
Claims
1. A method for preparing a NiFe LDH oxygen evolution catalyst with bimetallic cation vacancies, It is characterized in that First, NiZnFeAl LDH was prepared by electrochemical deposition, and then Ni was introduced into the basal surface of NiFe LDH by alkaline etching. 2+ and Fe 3+ The double metal cation vacancies provide the oxygen evolution catalyst.
2. A method for preparing a NiFe LDH oxygen evolution catalyst introducing bimetallic cation vacancies according to claim 1, It is characterized in that The preparation method specifically comprises the following steps: (1) Dissolve nickel nitrate, iron nitrate, aluminum chloride and zinc chloride in ultrapure water, stir until dissolved, and obtain a uniform mixed solution for later use; (2) transferring the mixed solution obtained in step (1) into a three-electrode electrolytic cell and applying voltage to react, wherein the working electrode used is nickel foam NF, the auxiliary electrode is a platinum mesh electrode, and the reference electrode is an Ag / AgCl electrode; (3) washing the working electrode obtained in step (2) with ultrapure water and drying naturally to obtain a NiZnFeAl LDH nanosheet oxygen evolution catalyst; (4) transferring the NiZnFeAl LDH nanosheet oxygen evolution catalyst obtained in step (3) into NaOH and soaking it for a period of time for alkaline etching; (5) The NiZnFeAl LDH catalyst after alkaline etching in step (4) is washed with ultrapure water and dried naturally to finally obtain a NiFe LDH oxygen evolution catalyst with bimetallic cation vacancies introduced therein.
3. The method for preparing a NiFe LDH oxygen evolution catalyst introducing bimetallic cation vacancies according to claim 2, It is characterized in that In step (1), the concentration of nickel nitrate and ferric nitrate in the mixed solution is 0.12 M; the concentration of aluminum chloride and zinc chloride is 0.5 ~ 2 mM, and the ratio of the concentration of aluminum chloride to zinc chloride is maintained at 1:
1.
4. The method for preparing a NiFe LDH oxygen evolution catalyst introducing bimetallic cation vacancies according to claim 2, It is characterized in that In step (2), the size of the platinum mesh electrode is 1×1 cm; in step (2), the reaction temperature is 25°C, the applied voltage is -1.0 V, and the reaction time is 10 to 500 s.
5. The method for preparing a NiFe LDH oxygen evolution catalyst introducing bimetallic cation vacancies according to claim 2, It is characterized in that In step (4), the alkaline etching reaction temperature is 25°C, the NaOH concentration is 5 M, and the alkaline etching time is 3 to 12 hours.
6. A NiFe LDH oxygen evolution catalyst with bimetallic cation vacancies introduced obtained by the preparation method according to any one of claims 1 to 5.
7. Use of the NiFe LDH oxygen evolution catalyst introduced with bimetallic cation vacancies obtained by the preparation method according to any one of claims 1 to 5 in electrocatalysis.
8. A method for preparing a NiZnFeAl LDH nanosheet oxygen evolution catalyst, It is characterized in that The following steps are involved: (1) Dissolve nickel nitrate, ferric nitrate, aluminum chloride and zinc chloride in ultrapure water, stir until dissolved, and obtain a uniform mixed solution for later use; the concentration of nickel nitrate and ferric nitrate in the mixed solution is 0.12 M; the concentration of aluminum chloride and zinc chloride is 0.5 ~ 2mM, and the ratio of aluminum chloride to zinc chloride is maintained at 1:1 (2) transferring the mixed solution obtained in step (1) into a three-electrode electrolytic cell and applying voltage to react, wherein the working electrode used is nickel foam NF, the auxiliary electrode is a platinum mesh electrode, and the reference electrode is an Ag / AgCl electrode; (3) The working electrode obtained in step (2) is washed with ultrapure water and dried naturally to obtain a NiZnFeAl LDH nanosheet oxygen evolution catalyst.
9. A NiZnFeAl LDH nanosheet oxygen evolution catalyst obtained by the preparation method as claimed in claim 8.
10. Use of the NiZnFeAl LDH nanosheet oxygen evolution catalyst obtained by the preparation method as claimed in claim 8 in electrocatalysis.
Citation Information
Cited By
Preparation method and application of PdvFeCoNiZnvLDH high-entropy catalytic material with zinc and palladium double metal vacancies
CN119657173A
With zinc and palladium bimetallic vacancies Pd v FeCoNiZn v Preparation method and application of LDH high entropy catalytic material
CN119657173B
Oxygen evolution reaction catalyst as well as preparation method and application thereof
CN121472927A