Electrolytic hydrogen production cathode catalyst, preparation method thereof, CO2-enhanced seawater electrolysis hydrogen production device and CO2-enhanced seawater electrolysis hydrogen production method
By using self-supporting titanium-containing non-precious metal phosphide catalysts and CO2 enhancement technology in electrolyzing seawater hydrogen production, the problems of high cost of precious metal catalysts and high electrolytic cell voltage are solved, and low-cost and efficient seawater electrolysis and CO2 storage are achieved. Improves the stability and reaction efficiency of the catalyst.
Patent Information
- Application Number
- CN202410929077.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-12
AI Technical Summary
In the existing electrolytic seawater hydrogen production technology, most of the catalysts are precious metals, with high costs and shortage of resources. In the process of seawater electrolysis, the theoretical voltage of the electrolytic cell is relatively large, the complex ion environment leads to poor stability, and the cathode calcium and magnesium ion deposition blocks the active site. Influences the reaction efficiency.
Using foam copper as the substrate, loaded with non-precious metal phosphides and titanium dioxide to form a self-supporting non-precious metal phosphide catalyst containing titanium. Combined with CO2-enhanced electrolytic seawater hydrogen production device, separate the anode through a sodium ion exchange membrane, and use sodium hydroxide. The solution and CO2 dissolve seawater for electrolysis, reducing the voltage and stabilizing the pH difference of the cathode and anode.
It realizes low-cost, efficient and stable direct seawater electrolysis, avoids the use of precious metals, improves the activity and stability of the catalyst, inhibits the increase in the cathode pH value, prevents calcium and magnesium ions from precipitation, and reduces the overall electrolytic water device. Energy consumption and reduce greenhouse effects through CO2 capture.
Smart Images

Figure CN118932391A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field related to hydrogen production by water electrolysis, and more specifically, relates to a cathode catalyst for hydrogen production by electrolysis, a preparation method thereof, and a CO2-enhanced seawater electrolysis hydrogen production device and method. Background Art
[0002] With the current improvement of living standards and the vigorous promotion of scientific and technological development, energy demand has also increased significantly. However, according to statistics, traditional fossil fuels account for more than 80% of the total global supply. As we all know, fossil fuels are non-renewable and will cause serious environmental pollution, such as the release of greenhouse gas CO2, the generation of flue gas, etc. In order to implement net zero carbon dioxide emissions, on the one hand, it is urgent to develop new renewable, green and pollution-free alternative energy sources, and on the other hand, carbon capture, utilization and storage are equally critical. Among many new energy systems, hydrogen energy has attracted widespread attention due to its high specific energy density (142kJ / kg) and pure and pollution-free products. However, the existing water electrolysis hydrogen production technology relies heavily on ultra-high purity fresh water (9kg H2O / kgH2) to ensure the service life of the hydrogen plant infrastructure. Economic and technical problems such as fresh water shortage (less than 1% of the earth's water) and uneven distribution further limit its large-scale application. Based on this, the abundant seawater resources on the earth (accounting for about 96.5% of the earth's water) have gradually attracted the interest of researchers. In addition, building hydrogen production plants directly on the coast will make it more convenient to obtain raw materials and transport products. Therefore, the use of electrocatalysis to drive green hydrogen production from seawater has great potential.
[0003] Natural seawater is a neutral environment (pH = 8.0-8.3), and the bipolar reaction kinetics are slow. Currently, the commonly used catalysts are mostly precious metals, which are expensive and in short supply. In addition, during the process of seawater electrolysis to produce hydrogen, OH is generated at the cathode as the electrolysis proceeds. - The gradual increase will cause the pH value at the cathode to gradually increase, so that the pH gradient formed near the cathode and anode will gradually decrease, which will further increase the theoretical voltage of the electrolyzer. On the other hand, the composition of seawater is relatively complex, and the chlorine oxidation side reaction on the anode side is serious, which will cause serious corrosion to the anode catalyst; the main problem of the cathode comes from calcium and magnesium ions. Seawater electrolysis will cause the local pH value of the cathode to increase. When the local pH is greater than 9.5, calcium and magnesium ions will deposit on the surface of the cathode catalyst to block the active sites, causing the reaction to be unable to continue. Summary of the invention
[0004] In view of the above defects or improvement needs of the prior art, the present invention provides a cathode catalyst for hydrogen production by electrolysis, a preparation method thereof, a CO2-enhanced seawater electrolysis hydrogen production device and method, which solves the problems that the catalysts commonly used for hydrogen production by electrolysis of seawater are mostly precious metals, which are expensive and in short supply. In addition, when seawater is used for hydrogen production by electrolysis, the theoretical voltage of the electrolyzer is large and the complex ion environment leads to poor stability. Low-cost, efficient and stable low-voltage direct seawater electrolysis and CO2 storage can be achieved.
[0005] To achieve the above-mentioned purpose, according to the first aspect of the present invention, there is provided a cathode catalyst for hydrogen production by electrolysis, comprising copper foam, non-precious metal phosphide and titanium dioxide; the non-precious metal phosphide and titanium dioxide are loaded on the copper foam to form a self-supporting titanium-containing non-precious metal phosphide, wherein the titanium dioxide has an amorphous structure and the non-precious metal phosphide has a nanorod morphology.
[0006] According to the cathode catalyst for hydrogen production by electrolysis provided by the present invention, the self-supporting titanium-containing non-precious metal phosphide is a self-supporting titanium-containing cobalt-molybdenum phosphide, a self-supporting titanium-containing nickel-molybdenum phosphide or a self-supporting titanium-containing nickel-iron phosphide.
[0007] According to the cathode for producing hydrogen by electrolysis provided by the present invention, the self-supporting titanium-containing non-precious metal phosphide is a self-supporting titanium-containing cobalt-molybdenum phosphide.
[0008] According to a second aspect of the present invention, a method for preparing a cathode catalyst for hydrogen production by electrolysis is provided, which is used to prepare the cathode catalyst for hydrogen production by electrolysis as described in any one of the above items, and the preparation method comprises:
[0009] S1, taking copper foam as a substrate, placing it in a solution prepared by a precursor for hydrothermal treatment, wherein the precursor comprises a compound containing a first non-precious metal element A and a compound containing a second non-precious metal element B, to obtain a precatalyst ABO / CF supported on the copper foam;
[0010] S2, placing ABO / CF downstream of the tube furnace and red phosphorus upstream of the tube furnace for calcination to obtain a phosphated precatalyst ABP / CF;
[0011] S3, uniformly dripping TiCl3 solution onto ABP / CF, drying and then placing in a tube furnace for hollow calcination, to obtain a final catalyst which is a self-supporting titanium-containing non-precious metal phosphide TiO2-ABP / CF.
[0012] According to the preparation method of the cathode catalyst for electrolytic hydrogen production provided by the present invention, S1 specifically comprises: dissolving the precursor in a urea aqueous solution, placing it in a copper foam for hydrothermal treatment, wherein the hydrothermal condition is heating at 100-200° C. for 5-10 hours, and the contents of A and B in the obtained ABO / CF are 20%-70% respectively;
[0013] And / or, S2 specifically includes: placing ABO / CF downstream of a tubular furnace, placing red phosphorus upstream of the tubular furnace, and calcining at 400-600° C. for 1-3 hours in a N2 atmosphere, and obtaining an ABP / CF with a P content of 10-20%.
[0014] According to the preparation method of the cathode catalyst for electrolytic hydrogen production provided by the present invention, S3 specifically comprises: uniformly dropping a TiCl3 solution with a mass fraction of 0.1%-1% on the ABP / CF, drying it, placing it in a tubular furnace and burning it at 200-250°C for 30min-2h;
[0015] And / or, the Ti content in the TiO2-ABP / CF obtained in S3 is 1 to 10%.
[0016] According to a third aspect of the present invention, there is provided a CO2-enhanced seawater electrolysis hydrogen production device, comprising an anode chamber and a cathode chamber, wherein an anode electrode sheet is disposed in the anode chamber, and a cathode electrode sheet is disposed in the cathode chamber, wherein the anode chamber and the cathode chamber are separated by a sodium ion exchange membrane, wherein the anode electrode sheet is a self-supporting nickel-iron layered hydroxide, and the cathode electrode sheet is a cathode catalyst for hydrogen production by electrolysis as described in any one of the above items;
[0017] The anode chamber is fed with an anolyte, which is a sodium hydroxide solution, and the cathode chamber is fed with a catholyte, which is seawater dissolved with CO2.
[0018] According to a fourth aspect of the present invention, a CO2-enhanced method for producing hydrogen by electrolysis of seawater is provided, which is implemented based on the above-mentioned CO2-enhanced hydrogen production device by electrolysis of seawater, and comprises:
[0019] Placing an anode electrode sheet in the anode chamber and introducing a sodium hydroxide solution as an anode electrolyte;
[0020] Placing a cathode electrode sheet in the cathode chamber and introducing seawater as a cathode electrolyte;
[0021] Voltage is applied to the anode electrode sheet and the cathode electrode sheet to perform an electrolytic hydrogen production reaction, and CO2 is continuously introduced into the cathode chamber during the reaction.
[0022] The CO2-enhanced seawater electrolysis method for producing hydrogen provided by the present invention also includes: adjusting the amount of CO2 introduced according to a preset electrolysis current, and the larger the preset electrolysis current, the larger the amount of CO2 introduced into the cathode chamber.
[0023] The CO2-enhanced seawater electrolysis method for producing hydrogen provided by the present invention also includes: heating the cathode electrolyte after the reaction to decompose the bicarbonate in the solution into carbonates and collecting metal resources.
[0024] In general, compared with the prior art, the above technical solutions conceived by the present invention provide cathode catalysts for hydrogen production by electrolysis, preparation methods thereof, and CO2-enhanced hydrogen production devices and methods by electrolysis of seawater:
[0025] 1. The provided cathode catalyst for hydrogen production by electrolysis shows good performance and stability in hydrogen production by electrolysis, does not require the use of precious metals, has abundant reserves of electrode materials and reduces costs; the cathode material has excellent performance in hydrogen production by electrolysis and can be applied to hydrogen production by seawater electrolysis;
[0026] 2. When the provided cathode catalyst for hydrogen production by electrolysis is used in the hydrogen production device for electrolysis of seawater provided by the present invention, it exhibits higher catalytic activity in seawater dissolved with CO2. Specifically, the cathode catalyst can enhance the migration ability of the proton source in seawater to the catalyst surface by interacting with CO2, for example, by adsorption, and promote the formation of a highly active interface on the catalyst surface, thereby promoting the hydrogen evolution reaction;
[0027] 3. The cathode electrolyte of the provided seawater electrolysis hydrogen production device uses seawater dissolved with CO2. By dissolving CO2 in seawater, the increase in the pH value of the cathode electrolyte as the electrolysis reaction proceeds can be suppressed, thereby stabilizing the pH difference between the anode and cathode. The anode electrolyte uses a sodium hydroxide solution, and the large pH difference on both sides is used to provide energy to reduce the theoretical potential of water decomposition, thereby reducing the energy consumption of the overall water electrolysis device, and has a lower theoretical water decomposition voltage compared with the traditional direct seawater electrolysis device;
[0028] 4. The electrolysis of seawater to produce hydrogen can generate OH - Capturing CO2 to form HCO3 - , increasing the solubility of carbon dioxide to alleviate the greenhouse effect. At the same time, CO2 dissolves in seawater to form carbonic acid, which can be used as a proton source for hydrogen evolution reaction, thereby solving the problem of slow reaction kinetics in neutral seawater. The anode electrolyte uses sodium hydroxide solution, thereby avoiding the chlorine oxidation side reaction on the anode side, which is beneficial to maintain the activity and performance of the anode catalyst.
[0029] 5. Compared with the traditional asymmetric device, the carbon dioxide introduced into the cathode side increases the bicarbonate concentration in the seawater and acts as a buffer to stabilize the cathode pH, solving the problem of calcium and magnesium ion precipitation caused by large pH changes on the cathode side, thereby preventing the formation of calcium hydroxide and magnesium hydroxide from blocking the active sites of the catalyst, so as to achieve long-term and stable direct seawater electrolysis. In addition, the OH - During the long electrolysis process, the concentration difference will drive the alkali through the membrane to the cathode side, and the carbonate buffer solution will neutralize this part of the alkali, thereby maintaining the pH difference on both sides and achieving long-term stable low-voltage direct seawater electrolysis;
[0030] 6. OH generated at the cathode in the method of electrolyzing seawater to produce hydrogen - Capturing CO2 to generate HCO3 - , the temperature of the electrolyte after the reaction is raised to achieve the enrichment of resources such as magnesium and calcium;
[0031] 7. The electrode catalyst used in the electrolytic hydrogen production device is a non-precious metal with abundant reserves and low price. After regulation, it has activity and stability comparable to that of precious metals in neutral seawater, greatly reducing the cost of the catalyst. The catalyst synthesis method provided is simple and efficient, suitable for mass production applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 is the XRD pattern of the self-supporting titanium-containing cobalt-molybdenum phosphide in Example 1 of the present invention;
[0033] Figure 2 This is a scanning electron microscope image of the self-supporting titanium-containing cobalt-molybdenum phosphide in Example 1 of the present invention;
[0034] Figure 3 Polarization curves of the hydrogen evolution process of the self-supporting titanium-containing cobalt-molybdenum phosphide in the CO2 solution of seawater in Examples 1 and 2 of the present invention;
[0035] Figure 4 This is a schematic diagram of the assembly of the electrolytic hydrogen production device in Example 1 of the present invention;
[0036] Figure 5 This is a schematic diagram of the assembly of the electrolytic hydrogen production device in Example 2 of the present invention;
[0037] Figure 6 The potential-time diagram of the electrolytic cell of Example 1 of the present invention, wherein the test current density is 100 mA cm -2 , test temperature 25℃;
[0038] Figure 7 The potential-time diagram of the electrolytic cell of Example 1 of the present invention, wherein the test current density is 200 mA·cm -2 , test temperature 60℃;
[0039] Figure 8 The potential-time diagram of the electrolytic cell of Example 2 of the present invention, wherein the test current density is 100 mA·cm -2 , test temperature 25℃;
[0040] Fig. 9 The potential-time diagram of the electrolytic cell of Example 3 of the present invention, wherein the test current density is 100 mA·cm -2 , test temperature 25℃;
[0041] Fig.10This is the potential-time diagram of the electrolytic cell of Comparative Example 1 of the present invention, wherein the test current is 100 mA·cm -2 , test temperature 25℃;
[0042] Fig.11 This is the potential-time diagram of the electrolytic cell of comparative example 2-1 of the present invention, wherein the test current is 100 mA·cm -2 , test temperature 25℃;
[0043] Fig.12 This is the potential-time diagram of the electrolytic cell of comparative example 2-2 of the present invention, wherein the test current is 100 mA·cm -2 , test temperature 25℃;
[0044] Fig.13 This is the electrolytic cell potential-time diagram of comparative example 3 of the present invention, wherein the test current is 100 mA·cm -2 , test temperature 25℃;
[0045] Fig.14 This is the potential-time diagram of the electrolytic cell of Comparative Example 4 of the present invention, wherein the test current is 100 mA·cm -2 , test temperature 25℃;
[0046] Fig.15 It is the white precipitate collected after the cathode electrolyte is heated in Example 1 of the present invention, and the heating condition is 100°C. DETAILED DESCRIPTION
[0047] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0048] The present invention provides a cathode catalyst for hydrogen production by electrolysis, which comprises copper foam, non-precious metal phosphide and titanium dioxide; the non-precious metal phosphide and titanium dioxide are loaded on the copper foam to form a self-supporting titanium-containing non-precious metal phosphide, wherein the titanium dioxide is an amorphous structure and the non-precious metal phosphide presents a nanorod morphology.
[0049] Specifically, non-precious metal phosphides are evenly distributed on the copper foam, and titanium dioxide is distributed on the non-precious metal phosphides in the form of small clusters. Self-supporting means that the catalyst material does not need to be loaded on carbon paper or other external support materials to be used as an electrode sheet, but the non-precious metal phosphides and titanium dioxide grow directly on the copper foam, and the catalyst material formed by the three can be directly used as an electrode sheet, so that the non-precious metal phosphides and titanium dioxide can present a three-dimensional distribution effect through the self-supporting structure, which is conducive to increasing the reaction area and improving the catalyst performance; and the conventional electrode sheets loaded on carbon paper or other external support materials need to add ionomers (adhesives), and ionomers may also affect the properties of the material. The catalyst of this embodiment can avoid the use of ionomers, which is conducive to ensuring the catalyst performance.
[0050] The cathode catalyst used in the present invention shows good performance and stability in hydrogen production by electrolysis, mainly for the following reasons: the base copper foam is a porous 3D structure, which provides a large reaction area, which is conducive to increasing the reaction speed and thus improving the performance; the non-precious metal-based phosphide adjusts the adsorption free energy of H, so that H2 can leave the catalyst surface faster, and avoids the use of precious metals, thereby reducing costs; TiO2 adsorbs water molecules to form a TiO(OH)2 layer, which reduces the activation energy required for water dissociation, so as to promote water dissociation in a neutral environment; thus, the cathode material has excellent performance in hydrogen production by electrolysis, and can be applied to hydrogen production by seawater electrolysis.
[0051] Furthermore, the diameter of the nanorods is about 80-200 nm.
[0052] Furthermore, the self-supporting titanium-containing non-precious metal phosphide is a self-supporting titanium-containing cobalt-molybdenum phosphide, a self-supporting titanium-containing nickel-molybdenum phosphide or a self-supporting titanium-containing nickel-iron phosphide.
[0053] In some specific embodiments, the self-supporting titanium-containing non-noble metal phosphide is a self-supporting titanium-containing cobalt-molybdenum phosphide.
[0054] Taking the self-supporting titanium-containing non-precious metal phosphide as a self-supporting titanium-containing cobalt-molybdenum phosphide as an example: X-ray diffraction analysis of the self-supporting catalyst of titanium-containing cobalt-molybdenum phosphide supported on copper foam was performed. Figure 1 As shown, there are diffraction peaks corresponding to CoMoP and Cu substrate in TiO2-CoMoP / Cu, but there is no diffraction peak corresponding to TiO2, which indicates that the loaded titanium dioxide is an amorphous structure without a crystalline phase, and CoMoP has a little crystalline phase, but the degree of crystallinity is very low.
[0055] Scanning electron microscopy analysis of the self-supporting catalyst of cobalt molybdenum phosphide containing titanium supported on copper foam. The catalyst was ultrasonically dispersed from the substrate in ethanol to obtain a characterization sample. Figure 2It can be seen that the catalyst is in the shape of nanorods with a diameter of about 100 nm.
[0056] Furthermore, the present invention also provides a method for preparing a cathode catalyst for hydrogen production by electrolysis, which is used to prepare the cathode catalyst for hydrogen production by electrolysis as described in any one of the above items, and the preparation method comprises:
[0057] S1, taking copper foam as a substrate, placing it in a solution prepared by a precursor for hydrothermal treatment, wherein the precursor comprises a compound containing a first non-precious metal element A and a compound containing a second non-precious metal element B, to obtain a precatalyst ABO / CF supported on the copper foam;
[0058] S2, placing ABO / CF downstream of the tube furnace and red phosphorus upstream of the tube furnace for calcination to obtain a phosphated precatalyst ABP / CF;
[0059] S3, uniformly dripping TiCl3 solution onto ABP / CF, drying and then placing in a tube furnace for hollow calcination, to obtain a final catalyst which is a self-supporting titanium-containing non-precious metal phosphide TiO2-ABP / CF.
[0060] The preparation method of the cathode catalyst for hydrogen production by electrolysis provided in this embodiment is to first load non-precious metal elements on copper foam by hydrothermal treatment to obtain a pre-catalyst, then phosphate the pre-catalyst by calcination treatment in an inert atmosphere in a sequential manner with red phosphorus, and then obtain the final catalyst by dripping a titanium salt solution and drying and empty burning. The preparation method can obtain a self-supporting titanium-containing non-precious metal phosphide catalyst with an amorphous structure and nanorod morphology loaded on copper foam, and the catalyst has better performance in hydrogen production by electrolysis.
[0061] In some specific embodiments, the first non-precious metal element A is cobalt, and the second non-precious metal element B is molybdenum; or the first non-precious metal element A is nickel, and the second non-precious metal element B is molybdenum; or the first non-precious metal element A is nickel, and the second non-precious metal element B is iron.
[0062] Taking the first non-precious metal element A as cobalt Co and the second non-precious metal element B as molybdenum Mo as an example: the precursor in S1 includes at least one of cobalt salts such as cobalt nitrate, cobalt chloride, cobalt sulfate, and at least one of molybdenum-containing compounds such as sodium molybdate, molybdenum acetylacetonate, and molybdenum chloride; the precatalyst supported on the copper foam obtained by S1 is CoMoO / CF. The precatalyst obtained by S2 after phosphation is CoMoP / CF. The final catalyst obtained by S3 is a self-supporting titanium-containing cobalt molybdenum phosphide, recorded as TiO2-CoMoP / CF.
[0063] In some specific embodiments, S1 specifically includes: dissolving the precursor in a urea aqueous solution, placing it in a copper foam for hydrothermal treatment, wherein the hydrothermal condition is heating at 100-200°C for 5-10h, and the contents of A and B in the obtained ABO / CF are 20%-70% respectively; specifically, the concentration of the urea aqueous solution is 0.1-1mol / L. Taking the first non-precious metal element A as cobalt Co and the second non-precious metal element B as molybdenum Mo as an example: dissolving the precursor in a urea aqueous solution with a concentration of 0.1-1mol / L to prepare a solution containing a cobalt concentration of 0.1-1mol / L and a Mo concentration of 0.1-1mol / L, and then placing it in a copper foam for hydrothermal treatment, the obtained CoMoO / CF has a Co content of 20%-70% and a Mo content of 20%-70%, and the content is mass fraction.
[0064] And / or, S2 specifically includes: placing ABO / CF downstream of a tubular furnace, placing red phosphorus upstream of a tubular furnace, calcining at 400-600°C in a N2 atmosphere for 1-3h, and obtaining an ABP / CF with a P content of 10-20%, which is a mass fraction.
[0065] In some specific embodiments, S3 specifically includes: uniformly dropping a TiCl3 solution with a mass fraction of 0.1%-1% on the ABP / CF, drying it, placing it in a tube furnace and burning it at 200-250°C for 30min-2h;
[0066] And / or, the TiO2-ABP / CF obtained in S3 has a Ti content of 1-10%, which is a mass fraction.
[0067] Furthermore, before S1, it also includes: pre-treating the copper foam; the specific pre-treatment method of the copper foam is to first ultrasonically treat the copper foam in ethanol for a preset time, such as 30 minutes, to remove surface organic matter, then ultrasonically treat the copper foam in 1 mol / L HCl for a preset time, such as 30 minutes, to remove surface oxides, and finally treat the copper foam in ultrapure water for 10-20 minutes to remove residual ethanol and hydrochloric acid.
[0068] The present invention also provides a CO2-enhanced electrolysis of seawater for hydrogen production, comprising an anode chamber and a cathode chamber, wherein an anode electrode sheet is provided in the anode chamber, and a cathode electrode sheet is provided in the cathode chamber, wherein the anode chamber and the cathode chamber are separated by a sodium ion exchange membrane, wherein the anode electrode sheet is a self-supporting nickel-iron layered hydroxide, and the cathode electrode sheet is a cathode catalyst for hydrogen production by electrolysis as described in any one of the above items; an anolyte is introduced into the anode chamber, wherein the anolyte is a sodium hydroxide solution, and a cathode electrolyte is introduced into the cathode chamber, wherein the cathode electrolyte is seawater dissolved with CO2. The sodium ion exchange membrane separates the cathode and the anode, and also separates the cathode electrolyte and the anolyte. The sodium ion exchange membrane conducts sodium ions from the anode to the cathode to maintain the charge balance of the electrolytes on both sides.
[0069] Furthermore, the anode electrode sheet is a self-supporting nickel-iron layered hydroxide. The cathode electrode sheet is a self-supporting titanium-containing cobalt molybdenum phosphide. The cathode electrolyte is a seawater CO2 solution with a pH of 4-9, and the anode electrolyte is a 1-4 mol / L sodium hydroxide solution.
[0070] The device can reach 100 mA·cm at room temperature -2 The current density only needs to be lower than 1.5V voltage to reach 200mA·cm at 60℃ -2 The current density only needs to be lower than 1.71V.
[0071] The present invention is a direct seawater electrolysis hydrogen production device enhanced by CO2. By dissolving CO2 in seawater, on the one hand, a seawater buffer solution is formed to inhibit the increase of the pH value of the cathode electrolyte as the electrolysis reaction proceeds, stabilize the pH difference between the anode and cathode, reduce the theoretical water decomposition voltage, and solve the problem of calcium and magnesium ion precipitation; on the other hand, carbon dioxide is captured and stored to alleviate the trend of global warming; carbon dioxide reacts with calcium and magnesium in seawater to generate bicarbonate and then converts into carbonate to achieve the enrichment of metal resources and the fixation of carbon dioxide. The strategy of directly passing NaOH on the anode side is adopted to avoid Cl - The occurrence of oxidation side reactions. The catalysts used are all non-precious metals, and the prepared catalysts show good catalytic performance in a neutral environment. Based on this, the present invention can achieve low-cost, efficient and stable low-voltage direct seawater electrolysis and CO2 storage.
[0072] The present invention also provides a CO2-enhanced seawater electrolysis hydrogen production method, based on the above-mentioned CO2-enhanced seawater electrolysis hydrogen production device, the seawater electrolysis hydrogen production method comprises:
[0073] Placing an anode electrode sheet in the anode chamber and introducing a sodium hydroxide solution as an anode electrolyte;
[0074] Placing a cathode electrode sheet in the cathode chamber and introducing seawater as a cathode electrolyte;
[0075] Voltage is applied to the anode electrode sheet and the cathode electrode sheet to perform an electrolytic hydrogen production reaction, and CO2 is continuously introduced into the cathode chamber during the reaction.
[0076] Specifically, the CO2 in the cathode chamber can be directly and continuously introduced into the seawater, or a gas path can be set to connect the cathode chamber so that the CO2 first passes through the gas path to the cathode catalyst surface and then into the seawater. The specific CO2 introduction method and position are not limited, with the purpose of being soluble in seawater.
[0077] The specific principle of hydrogen production by electrolysis is as follows:
[0078] Cathode: 2H2O+2e- →H2+2OH - ; Anode: 2H2O-2e - →O2+2H + .
[0079] Furthermore, the method for producing hydrogen by electrolyzing seawater also includes: adjusting the amount of CO2 introduced according to a preset electrolysis current, and the greater the preset electrolysis current, the greater the amount of CO2 introduced into the cathode chamber.
[0080] Specifically, the amount of CO2 introduced into the cathode chamber is obtained by the following formula:
[0081] V CO2 =V m n CO2 / t=V m I / F; where V CO2 is the inflow rate of CO2; V m is the molar volume of the gas; n CO2 is the number of moles of CO2 consumed; t is time; I is current; and F is the Faraday constant. The specific derivation principle is as follows:
[0082] In the electrolysis reaction, I = Q / t; n e- =Q / F; n H2 =n e- / 2 = It / 2F;
[0083] According to the chemical formula of CO2 dissolution reaction in the cathode chamber: 2CO2+2OH - →2HCO3 - +2H + ; 2H + +2e - →H2; we can get: n CO2 =2n H2 ; Where Q is the total input power; n e- is the number of moles of transferred electrons; n H2 is the number of moles of H2 generated; and the calculation formula for the above-mentioned CO2 inflow rate can be derived.
[0084] That is, applying current to the hydrogen production device can obtain the theoretical hydrogen production without any loss. Every 1M H2 produced will be accompanied by 2M OH - , that is, 2M CO2 is needed for neutralization, from which the theoretical CO2 demand under the corresponding current can be obtained, and the CO2 flow rate can be set accordingly.
[0085] For example, assuming the applied current is 50 mA and the electrode reaction area is 0.5 cm 2 , assuming that the Faraday efficiency of hydrogen production is 100%, the theoretical CO2 consumption is calculated as follows:
[0086] 50mA=0.05C / s, 50mA=100mA·cm -2 ,
[0087] V CO2 =V m I / F=22.4×50 / 96500=0.0116mL / s=0.696mL / min.
[0088] Furthermore, the method for producing hydrogen by electrolyzing seawater further comprises: heating the cathode electrolyte after the reaction to decompose the bicarbonate in the solution into carbonates, and collecting metal resources. Heating the cathode electrolyte after the reaction to 100° C. to decompose the calcium bicarbonate and magnesium bicarbonate in the solution into calcium carbonate and magnesium carbonate, and collecting the enriched metal resources such as magnesium and calcium.
[0089] The purpose of the present invention is to solve the problems of slow cathode reaction kinetics, cathode calcium and magnesium ion precipitation, interference from anode chlorine oxidation side reaction and high device voltage in direct seawater electrolysis; at the same time, CO2 is mineralized to alleviate global warming while enriching metal resources in the ocean. The raw materials of the catalyst used in the present invention are all non-precious metals with abundant content and low price, and the preparation method is simple and environmentally friendly. The device has a simple structure and is easy to assemble, and is energy-saving and environmentally friendly as a whole, and has broad application prospects.
[0090] The following specific examples and comparative examples are provided to better illustrate the scheme and effects of the present invention. Unless otherwise specified, the raw materials used in the examples of the present invention are purchased from commercial sources, directly used in the treatment, and the instrument parameters used are recommended parameters.
[0091] Example 1: This example provides a CO2 enhanced direct seawater electrolysis device.
[0092] (1) Preparation of titanium-containing cobalt-molybdenum phosphide catalyst supported on copper foam as cathode electrode:
[0093] The copper foam was cut into 2×3 cm small pieces for easy placement in a polytetrafluoroethylene liner for reaction. The copper foam was first ultrasonically treated in ethanol for 30 minutes to remove surface organic matter, then ultrasonically treated in 1 mol / L HCl for 30 minutes to remove surface oxides, and finally treated in ultrapure water for 10-20 minutes to remove residual ethanol and hydrochloric acid, and dried to obtain the substrate required for subsequent hydrothermal treatment. 0.291 g Co(NO3)2·6H2O, 0.242 g Na2MoO4·2H2O and 0.18 g urea were weighed on an analytical balance and dissolved in 40 mL ultrapure water, stirred and dissolved, and then transferred to a 100 mL polytetrafluoroethylene liner. The treated copper foam was placed in the prepared solution and then hydrothermally treated in a blast oven. The reaction conditions were heating at 150°C for 6 hours, cooling to room temperature and then taking out, rinsing with ultrapure water, and drying to obtain the CoMoO / CF precatalyst.
[0094] Weigh 0.1g of red phosphorus and place it at the bottom of the test tube, place CoMoO / CF in the middle of the test tube, place the test tube in the center of the quartz tube with the bottom facing the air inlet, place the quartz tube in the middle of the tube furnace, calcine at 450℃ in N2 atmosphere for 1h, and take it out after cooling to room temperature to obtain CoMoP / CF. Dissolve 10mL of TiCl3 in 490mL of ethanol to prepare a solution with a mass fraction of 0.28%, evenly add 9 drops to CoMoP / CF, dry it, place it in a tube furnace and burn it at 200℃ for 30 minutes to obtain the final catalyst, recorded as TiO2-CoMoP / CF.
[0095] (2) According to Figure 4 The device is assembled in the manner of Example 1 in the schematic diagram.
[0096] The titanium-containing cobalt molybdenum phosphide self-supporting catalyst TiO2-CoMoP / CF is loaded on the foam copper as the cathode electrode, and the self-supporting nickel-iron layered hydroxide NiFe LDH / NF is used as the anode electrode; the cathode and anode electrodes are separated by a sodium ion exchange membrane; the cathode electrolyte is a CO2 solution of seawater, which can be a saturated CO2 solution of seawater, and the anode electrolyte is 4 mol / L NaOH. Both the cathode and anode electrolytes are injected into the seawater electrolysis device through a peristaltic pump and flow to the cathode chamber and anode chamber of the electrolytic cell respectively. The cathode electrolyte after the reaction is heated to 100°C to collect the enriched magnesium, calcium and sodium resources.
[0097] Example 2
[0098] This embodiment provides a CO2-enhanced direct seawater electrolysis device. The catalyst material provided in this embodiment is obtained in the same manner as in Example 1, but this embodiment differs from Example 1 in that the CO2 is introduced into the electrolysis device in a different manner:
[0099] (1) Preparation of titanium-containing cobalt-molybdenum phosphide catalyst supported on copper foam as cathode electrode:
[0100] The copper foam was cut into 2×3cm small pieces for easy placement in a polytetrafluoroethylene liner for reaction. The copper foam was first ultrasonically treated in ethanol for 30 minutes to remove surface organic matter, then ultrasonically treated in 1mol / L HCl for 30 minutes to remove surface oxides, and finally treated in ultrapure water for 10-20 minutes to remove residual ethanol and hydrochloric acid, and dried to obtain the substrate required for subsequent hydrothermal treatment. 0.291g Co(NO3)2·6H2O, 0.242g Na2MoO4·2H2O and 0.18g urea were weighed on an analytical balance and dissolved in 40mL ultrapure water, stirred and dissolved, and then transferred to a 100mL polytetrafluoroethylene liner. The treated copper foam was placed in the prepared solution and then hydrothermally treated in a blast oven. The reaction conditions were heating at 150°C for 6h, cooling to room temperature and then taking it out, rinsing with ultrapure water, and drying to obtain the CoMoO / CF precatalyst.
[0101] Weigh 0.1g of red phosphorus and place it at the bottom of the test tube, place CoMoO / CF in the middle of the test tube, place the test tube in the center of the quartz tube with the bottom facing the air inlet, place the quartz tube in the middle of the tube furnace, calcine at 450℃ in N2 atmosphere for 1h, and take it out after cooling to room temperature to obtain CoMoP / CF. Dissolve 10mL of TiCl3 in 490mL of ethanol to prepare a solution with a mass fraction of 0.28%, evenly add 9 drops to CoMoP / CF, dry it, place it in a tube furnace and burn it at 200℃ for 30 minutes to obtain the final catalyst, recorded as TiO2-CoMoP / CF.
[0102] (2) According to Figure 5 The device is assembled in the manner of Example 2 in the schematic diagram.
[0103] The titanium-containing cobalt-molybdenum phosphide self-supporting catalyst TiO2-CoMoP / CF is loaded on the foam copper as the cathode electrode, and the self-supporting nickel-iron layered hydroxide is used as the anode electrode NiFe LDH / NF; the cathode and anode electrodes are separated by a sodium ion exchange membrane; the cathode electrolyte is first introduced into the cathode chamber into real seawater, and the anode electrolyte is 4 mol / L NaOH, and then CO2 flows to the cathode catalyst through the upper gas path of the electrolyzer and then into the real seawater. Both the cathode and anode electrolytes are injected into the seawater electrolysis device through a peristaltic pump and flow to the cathode chamber and anode chamber of the electrolyzer, respectively. The cathode electrolyte after the reaction is heated to 100°C to collect the enriched magnesium, calcium and sodium resources.
[0104] Example 3
[0105] This embodiment provides a CO2-enhanced direct seawater electrolysis device. The catalyst material provided in this embodiment is obtained in the same manner as in Example 1, but the difference between this embodiment and Example 1 is that the cathode catalyst material used is different:
[0106] Self-supporting catalysts such as titanium-containing nickel-molybdenum phosphide or nickel-iron phosphide are loaded on the foam copper as the cathode electrode, and self-supporting nickel-iron layered hydroxide is used as the anode electrode; the cathode and anode electrodes are separated by a sodium ion exchange membrane; the cathode electrolyte is a CO2 solution of seawater, and the anode electrolyte is 4mol / LNaOH. Both the cathode and anode electrolytes are injected into the seawater electrolysis device through a peristaltic pump and flow to the cathode chamber and anode chamber of the electrolytic cell respectively. The cathode electrolyte after the reaction is heated to 100°C to collect the enriched magnesium, calcium and sodium resources.
[0107] Comparative Example 1
[0108] This comparative example provides an asymmetric direct seawater electrolysis device. The catalyst material provided in this comparative example is obtained in the same manner as in Example 1, except that the cathode electrolyte is seawater and no CO2 enhancement is used.
[0109] (1) Preparation of a titanium-containing cobalt-molybdenum phosphide catalyst supported on copper foam as a cathode electrode. The specific preparation process is shown in Examples 1 and 2 above and will not be described in detail.
[0110] (2)Reference Figure 4 Schematic diagram of the device for assembly.
[0111] The self-supporting catalyst of cobalt molybdenum phosphide containing titanium is loaded on the copper foam as the cathode electrode, and the self-supporting nickel-iron layered hydroxide is used as the anode electrode; the cathode and anode electrodes are separated by a sodium ion exchange membrane; the cathode electrolyte is real seawater, and the anode electrolyte is 4mol / L NaOH. Both the cathode and anode electrolytes are injected into the seawater electrolysis device through a peristaltic pump and flow to the cathode chamber and anode chamber of the electrolyzer respectively.
[0112] Comparative Example 2-1
[0113] This comparative example provides a CO2-enhanced direct seawater electrolysis device. The difference from Example 1 is that this comparative example uses commercial Pt / C as the cathode electrode.
[0114] refer to Figure 4The device is assembled as shown in the schematic diagram. Commercial Pt / C is used as the cathode electrode, and the self-supporting nickel-iron layered hydroxide NiFeLDH / NF is used as the anode electrode; the cathode and anode electrodes are separated by a sodium ion exchange membrane; the cathode electrolyte is a CO2 solution in seawater, and the anode electrolyte is 4 mol / L NaOH. Both the cathode and anode electrolytes are injected into the seawater electrolysis device through a peristaltic pump and flow to the cathode chamber and anode chamber of the electrolytic cell, respectively. The cathode electrolyte after the reaction is heated to 100°C to collect the enriched magnesium, calcium and sodium resources.
[0115] Comparative Example 2-2
[0116] This comparative example provides a CO2-enhanced direct seawater electrolysis device. The difference from Example 1 is that this comparative example uses commercial Pt / C as the cathode electrode and commercial IrO2 / C as the anode electrode.
[0117] refer to Figure 4 The device is assembled as shown in the schematic diagram. Commercial Pt / C is used as the cathode electrode, and commercial IrO2 / C is used as the anode electrode; a sodium ion exchange membrane is used to separate the cathode and anode electrodes; the cathode electrolyte is a CO2 solution in seawater, and the anode electrolyte is 4 mol / L NaOH. Both the cathode and anode electrolytes are injected into the seawater electrolysis device through a peristaltic pump and flow to the cathode chamber and anode chamber of the electrolyzer, respectively. The cathode electrolyte after the reaction is heated to 100°C to collect the enriched magnesium, calcium and sodium resources.
[0118] Comparative Example 3
[0119] This comparative example provides a conventional alkaline seawater electrolysis device. The catalyst material provided in this comparative example is obtained in the same manner as in Example 1, except that both the cathode and anode electrolytes are alkaline seawater.
[0120] refer to Figure 4 The device is assembled as shown in the schematic diagram. The self-supporting catalyst of cobalt molybdenum phosphide containing titanium is loaded on the copper foam as the cathode electrode, and the self-supporting nickel-iron layered hydroxide NiFe LDH / NF is used as the anode electrode; the cathode and anode electrodes are separated by a sodium ion exchange membrane; the cathode and anode electrolytes are both alkaline seawater. The cathode and anode electrolytes are injected into the seawater electrolysis device through a peristaltic pump and flow to the cathode chamber and anode chamber of the electrolyzer, respectively.
[0121] Comparative Example 4
[0122] This comparative example provides an asymmetric direct seawater electrolysis device. The difference between this comparative example and Example 3 is that the cathode electrolyte is seawater and no CO2 enhancement is used.
[0123] Self-supporting catalysts such as titanium-containing nickel-molybdenum phosphide or nickel-iron phosphide are loaded on the copper foam as the cathode electrode, and self-supporting nickel-iron layered hydroxide is used as the anode electrode; the cathode and anode electrodes are separated by a sodium ion exchange membrane; the cathode electrolyte is real seawater, and the anode electrolyte is 4 mol / L NaOH. Both the cathode and anode electrolytes are injected into the seawater electrolysis device through a peristaltic pump and flow to the cathode chamber and anode chamber of the electrolyzer, respectively.
[0124] Results and analysis:
[0125] The structure and morphology of the titanium-containing cobalt-molybdenum phosphide self-supporting catalyst supported on the copper foam in Example 1 were characterized as follows: Figure 1 and Figure 2 shown.
[0126] The electrochemical performance of the titanium-containing cobalt-molybdenum phosphide catalyst supported on copper foam was tested in a CO2 solution in seawater. Figure 3 As shown, its hydrogen evolution reaction (HER) exhibits better performance than that of commercial Pt / C, which is due to the fact that TiO2 promotes the dissociation of water in a neutral environment.
[0127] The stability test of the CO2-enhanced direct seawater electrolysis device in Example 1 was carried out under the following test conditions: the current density was 100 mA·cm -2 , the test temperature is 25℃. Figure 6 As shown, to achieve this current density, the electrolysis device of the present invention only requires a voltage of 1.49V.
[0128] The stability test of the CO2-enhanced direct seawater electrolysis device in Example 1 was carried out under the following test conditions: the current density was 200 mA·cm -2 , the test temperature is 60℃. Figure 7 As shown, to achieve this current density, the electrolysis device of the present invention only requires a voltage of 1.71V.
[0129] The hydrogen production device provided by electrolyzing seawater in this embodiment 1 can reach 100 mA·cm at room temperature. -2 The current density only needs 1.5V voltage to reach 200mA·cm at 60℃ -2 The current density only requires a voltage of 1.71V, which is much lower than other direct seawater electrolysis devices.
[0130] The stability test of the CO2-enhanced direct seawater electrolysis device in Example 2 was carried out under the following test conditions: the current density was 100 mA·cm -2 , the test temperature is 25℃. Figure 8 As shown, to achieve this current density, the electrolysis device of the present invention only needs a voltage of 1.51 V, which means that the CO2 introduction method does not affect the performance and stability of the device.
[0131] The stability test of the CO2-enhanced direct seawater electrolysis device in Example 3 was carried out under the following test conditions: the current density was 100 mA·cm -2 , the test temperature is 25℃. Fig. 9 As shown, to achieve this current density, when TiO2-NiMoP / CF is used as the cathode catalyst, the electrolysis device of the present invention requires a voltage of 1.53V, and when TiO2-NiFeP / CF is used as the cathode catalyst, the electrolysis device of the present invention requires a voltage of 1.57V.
[0132] The stability test of the asymmetric direct seawater electrolysis device in Comparative Example 1 was carried out under the following test conditions: the current density was 100 mA cm -2 , the test temperature is 25℃. Fig.10 As shown, to achieve this current density, the electrolysis device of the present invention requires a voltage of 1.62 V. Compared with Example 1, the performance of the device without CO2 is poor, which proves that CO2 dissolved in the cathode electrolyte reduces the cathode pH and thus increases the pH difference between the two electrodes, reducing the voltage, that is, the energy consumption required for electrolyzing water.
[0133] The stability test of the CO2-enhanced direct seawater electrolysis device in Comparative Example 2-1 was carried out under the following test conditions: the current density was 100 mA·cm -2 , the test temperature is 25℃. Fig.11 As shown, to achieve this current density, the electrolysis device of the present invention requires a voltage of 1.6 V. Compared with Example 1, the electrolysis device assembled using the cathode catalyst for hydrogen electrolysis provided by the present invention requires a smaller voltage to achieve the same current density than the electrolysis device assembled using the commercial catalyst, which proves that the cathode catalyst exhibits better catalytic activity than the commercial catalyst.
[0134] The stability test of the CO2-enhanced direct seawater electrolysis device in Comparative Example 2-2 was carried out under the following test conditions: the current density was 100 mA·cm -2 , the test temperature is 25℃. Fig.12 As shown, to achieve this current density, the electrolysis device of the present invention requires a voltage of 1.63 V. Compared with Example 1, the electrolysis device assembled using the catalyst of the present invention requires a smaller voltage to achieve the same current density than the electrolysis device assembled using the commercial catalyst, proving that the catalyst exhibits better catalytic activity than the commercial catalyst.
[0135] The stability test of the conventional alkaline seawater electrolysis device in Comparative Example 3 was carried out under the following test conditions: the current density was 100 mA·cm -2 , the test temperature is 25℃. Fig.13As shown, to achieve this current density, the electrolysis device of the present invention requires a voltage of 1.74 V. Compared with Example 1 and Comparative Example 1, it can be seen that the performance of the CO2-enhanced direct seawater electrolysis device provided by the present invention, the asymmetric electrolysis device, and the symmetric electrolysis device gradually deteriorate, further indicating that CO2 can increase the pH difference between the two electrodes and reduce the voltage for electrolyzing seawater.
[0136] The stability test of the asymmetric direct seawater electrolysis device in Comparative Example 4 was carried out under the following test conditions: the current density was 100 mA cm -2 , the test temperature is 25℃. Fig.14 As shown, to achieve this current density, when TiO2-NiMoP / CF is used as the cathode catalyst, the electrolysis device of the present invention requires a voltage of 1.67 V, and when TiO2-NiFeP / CF is used as the cathode catalyst, the electrolysis device of the present invention requires a voltage of 1.7 V. Compared with Example 3, the performance of the device without CO2 is poor, which further proves that the dissolution of CO2 into the cathode electrolyte reduces the cathode pH, thereby increasing the pH difference between the two electrodes and reducing the voltage.
[0137] The cathode catalyst of the present invention can be replaced by other non-precious metal phosphides containing titanium. The synthesis process is the same as that of the cobalt-molybdenum phosphide catalyst containing titanium supported on copper foam, except that the hydrothermal precursor salt is replaced by the corresponding non-precious metal salt. The prepared phosphide precursors include CoMoP, NiMoP, NiFeP, etc., among which CoMoP has the best performance. The catalyst is assembled on the device, and the performance of all the prepared catalysts is better when the cathode electrolyte uses a CO2 saturated solution of seawater than when the electrolyte uses seawater.
[0138] The cathode electrolyte that has been subjected to the long-term stability test in Example 1 was subjected to a temperature increase of 100° C. to obtain Fig.15 The white powder shown is magnesium carbonate, sodium carbonate and calcium carbonate, which indicates that the device can realize the mineralization of CO2 and the enrichment of metal resources in the ocean, and has great research value.
[0139] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A cathode catalyst for hydrogen production by electrolysis, characterized in that: It includes copper foam, non-precious metal phosphide and titanium dioxide; the non-precious metal phosphide and titanium dioxide are loaded on the copper foam to form a self-supporting titanium-containing non-precious metal phosphide, wherein the titanium dioxide is an amorphous structure and the non-precious metal phosphide presents a nanorod morphology.
2. The cathode catalyst for hydrogen production by electrolysis according to claim 1, characterized in that: The self-supporting titanium-containing non-precious metal phosphide is a self-supporting titanium-containing cobalt-molybdenum phosphide, a self-supporting titanium-containing nickel-molybdenum phosphide or a self-supporting titanium-containing nickel-iron phosphide.
3. The cathode catalyst for hydrogen production by electrolysis according to claim 2, characterized in that: The self-supporting titanium-containing non-noble metal phosphide is a self-supporting titanium-containing cobalt-molybdenum phosphide.
4. A method for preparing a cathode catalyst for hydrogen production by electrolysis, characterized in that: For preparing the cathode catalyst for hydrogen production by electrolysis according to any one of claims 1 to 3, the preparation method comprising: S1, taking copper foam as a substrate, placing it in a solution prepared by a precursor for hydrothermal treatment, wherein the precursor comprises a compound containing a first non-precious metal element A and a compound containing a second non-precious metal element B, to obtain a precatalyst ABO / CF supported on the copper foam; S2, placing ABO / CF downstream of the tube furnace and red phosphorus upstream of the tube furnace for calcination to obtain the phosphated precatalyst ABP / CF; S3, uniformly dripping TiCl3 solution onto ABP / CF, drying and then placing in a tube furnace for hollow calcination, to obtain a final catalyst which is a self-supporting titanium-containing non-precious metal phosphide TiO2-ABP / CF.
5. The method for preparing a cathode catalyst for hydrogen production by electrolysis according to claim 4, characterized in that: S1 specifically comprises: dissolving the precursor in a urea aqueous solution, placing it in a copper foam for hydrothermal treatment, wherein the hydrothermal condition is heating at 100-200° C. for 5-10 hours, and the contents of A and B in the obtained ABO / CF are 20%-70% respectively; And / or, S2 specifically includes: placing ABO / CF downstream of a tubular furnace, placing red phosphorus upstream of the tubular furnace, and calcining at 400-600° C. for 1-3 hours in a N2 atmosphere, and obtaining an ABP / CF with a P content of 10-20%.
6. The method for preparing a cathode catalyst for hydrogen production by electrolysis according to claim 4, characterized in that: S3 specifically comprises: uniformly dropping a TiCl3 solution with a mass fraction of 0.1%-1% on the ABP / CF, drying it, placing it in a tube furnace and burning it at 200-250°C for 30min-2h; And / or, the Ti content in the TiO2-ABP / CF obtained in S3 is 1 to 10%.
7. A CO2-enhanced seawater electrolysis hydrogen production device, characterized in that: It comprises an anode chamber and a cathode chamber, wherein an anode electrode sheet is arranged in the anode chamber, and a cathode electrode sheet is arranged in the cathode chamber, wherein the anode chamber and the cathode chamber are separated by a sodium ion exchange membrane, wherein the anode electrode sheet is a self-supporting nickel-iron layered hydroxide, and the cathode electrode sheet is a cathode catalyst for hydrogen production by electrolysis as described in any one of claims 1 to 3; The anode chamber is fed with an anolyte, which is a sodium hydroxide solution, and the cathode chamber is fed with a catholyte, which is seawater dissolved with CO2.
8. A CO2-enhanced method for producing hydrogen by electrolysis of seawater, characterized in that: The CO2-enhanced seawater electrolysis hydrogen production device according to claim 7 is implemented, comprising: Placing an anode electrode sheet in the anode chamber and introducing a sodium hydroxide solution as an anode electrolyte; Placing a cathode electrode sheet in the cathode chamber and introducing seawater as a cathode electrolyte; Voltage is applied to the anode electrode sheet and the cathode electrode sheet to perform an electrolytic hydrogen production reaction, and CO2 is continuously introduced into the cathode chamber during the reaction.
9. The CO2-enhanced seawater electrolysis method for producing hydrogen as claimed in claim 8, characterized in that: Also includes: The amount of CO2 introduced is adjusted according to the preset electrolysis current. The larger the preset electrolysis current, the larger the amount of CO2 introduced into the cathode chamber.
10. The CO2-enhanced seawater electrolysis method for producing hydrogen as claimed in claim 8, characterized in that: Also includes: The cathode electrolyte after the reaction is subjected to a temperature-raising treatment to decompose the bicarbonate in the solution into carbonate, and the metal resources are collected.