Preparation and application of controllable nitrogen-doped catalytic material for synthesizing H2O2 through electro-catalytic oxygen reduction

By combining freeze-drying and vacuum drying with ultrasonic treatment, cobalt precursors are added dropwise, and nitrogen doping is controlled to ensure uniform distribution of cobalt. This solves the problems of low current density, high overpotential, and poor stability of existing catalytic materials in electrocatalytic oxygen reduction synthesis reactions, and achieves highly efficient electrocatalytic oxygen reduction reactions.

CN118932399APending Publication Date: 2024-11-12EAST CHINA UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411034829.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing catalytic materials exhibit low current density, high overpotential, and poor stability in electrocatalytic oxygen reduction synthesis reactions, and the nitrogen doping is uneven, which affects catalytic efficiency and selectivity.

Method used

By combining freeze-drying and vacuum drying with ultrasonic treatment, cobalt precursors are added dropwise, nitrogen doping is controlled, and cobalt is uniformly distributed to optimize the material structure. Through surface cleaning and dispersibility treatment, a stable catalytic structure is formed.

Benefits of technology

It improves the electrochemical performance of catalytic materials, enhances conductivity and catalytic activity, reduces overpotential, increases current density and material stability, and improves the selectivity and yield of target products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932399A_ABST
    Figure CN118932399A_ABST
Patent Text Reader

Abstract

The invention discloses preparation and application of a controllable nitrogen-doped catalytic material for synthesizing H2O2 through electro-catalytic oxygen reduction, and relates to the technical field of material synthesis and application.The preparation method comprises the steps that S100, materials are prepared, specifically, a proper amount of oxidized carbon nanotubes and ammonium salt are selected, and a cobalt precursor is prepared. According to the present invention, the reaction path is optimized, such that the electro-catalytic oxygen reduction reaction can be performed at the low overpotential while the high current density is generated, the uniform distribution of the cobalt element on the surface and the surrounding of the nanotube is ensured through the ultrasonic treatment and the cobalt precursor dropwise adding method, and the uniform distribution is beneficial to the formation of the stable catalytic structure so as to provide the good catalytic effect on the surface and the surrounding of the nanotube; the catalytic performance reduction caused by overhigh local concentration is prevented, the oxidized carbon nanotubes are subjected to surface cleaning and dispersion treatment, the surface roughness and dispersion of the oxidized carbon nanotubes are improved, and the agglomeration phenomenon is effectively prevented.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of material synthesis and application, and in particular to the preparation and application of a catalytic material for synthesizing H2O2 by electrocatalytic oxygen reduction with controllable nitrogen doping. Background Art

[0002] In the field of electrocatalysis, especially in the research of catalytic materials for oxygen reduction synthesis reactions, although some progress has been made, there are still many challenges and shortcomings. At present, many traditional catalytic materials have poor electrochemical performance, mainly reflected in low current density, high overpotential and poor stability. These problems limit the widespread application of catalytic materials in energy conversion and storage devices (such as fuel cells, metal-air batteries, etc.).

[0003] In addition, traditional preparation methods have limitations in controlling the uniformity and structural characteristics of materials, resulting in uneven distribution of catalytic active sites, which affects catalytic efficiency and selectivity. In particular, for nitrogen-doped catalytic materials, how to effectively achieve uniform doping of nitrogen atoms during the preparation process while retaining the porous structure and large specific surface area of ​​the material is a major challenge in current research.

[0004] On the other hand, the selectivity and yield of catalytic materials are also important indicators for evaluating their performance. Catalytic materials prepared by traditional methods often perform poorly in these aspects and are difficult to meet the high requirements of industrial applications. Especially in the electrocatalytic oxygen reduction synthesis reaction, how to improve the selectivity of catalytic materials for the target product and at the same time improve the yield and Faraday efficiency is a problem that needs to be solved urgently.

[0005] In summary, the development of a new type of controllable nitrogen-doped catalytic material for electrocatalytic oxygen reduction synthesis and its preparation method aims to solve the problems of existing catalytic materials in electrochemical performance, uniformity, stability, selectivity and yield, which is of great significance for promoting the advancement and application of electrocatalytic technology. Summary of the invention

[0006] The purpose of the present invention is to make up for the deficiencies of the prior art and provide a controllable nitrogen-doped electrocatalytic oxygen reduction synthesis H2O2 catalytic material preparation and application, which can be freeze-dried and vacuum-dried, the method effectively retains the porous structure and large specific surface area of ​​the material, this structural feature provides more active sites for the catalytic reaction, so that the reactants can be more fully in contact with the catalyst, thereby improving the catalytic efficiency, the doping of nitrogen elements not only improves the conductivity of the material, but also significantly enhances its catalytic activity, the introduction of nitrogen atoms changes the electronic structure of the material, optimizes the reaction path, so that the electrocatalytic oxygen reduction reaction can be carried out at a lower overpotential, while generating a higher current density, through ultrasonic treatment and dropwise addition of cobalt precursor methods, ensure the uniform distribution of cobalt elements on the surface of the nanotubes and around, this uniform distribution helps to form a stable catalytic structure, prevents the catalytic performance from being reduced due to excessive local concentration, and performs surface cleaning and dispersibility treatment on the oxidized carbon nanotubes, improves its surface roughness and dispersibility, and effectively prevents the occurrence of agglomeration, these measures not only optimize the uniformity of the material, but also improve its surface activity, so that the catalytic material exhibits more stable performance in subsequent electrochemical tests.

[0007] In order to solve the above technical problems, the present invention provides the following technical solutions: On the one hand, a method for preparing a catalytic material for synthesizing H2O2 by electrocatalytic oxygen reduction with controllable nitrogen doping, the preparation method comprising:

[0008] S100, material preparation: selecting an appropriate amount of oxidized carbon nanotubes and ammonium salt to prepare a cobalt precursor, which will be used to introduce cobalt elements in subsequent steps;

[0009] S200, aqueous solution dispersion: a certain volume of deionized water is taken and placed in a suitable container, and the weighed oxidized carbon nanotubes and ammonium salt are added to the aqueous solution in sequence, and an ultrasonic processor is used to fully ultrasonically disperse them to ensure that the two are evenly dispersed in the water to form a stable suspension. This step helps to increase the uniformity and activity of the material in the subsequent reaction;

[0010] S300, adding dropwise: under the conditions of continuous stirring and ultrasonic dispersion, the cobalt precursor solution is added dropwise to the mixed suspension of the oxidized carbon nanotubes and the ammonium salt, and the dropping speed is controlled to avoid excessive local concentration, and the ultrasonic dispersion is continued for a period of time until the cobalt precursor is completely dissolved and evenly dispersed in the mixed solution. This step ensures that the cobalt element can be evenly distributed on the surface of the nanotubes and around them, providing favorable conditions for subsequent reactions;

[0011] S400, freezing treatment: transferring the mixed solution to a freeze-drying device for freezing treatment, wherein the water in the solution is rapidly frozen by lowering the temperature to form solid ice crystals;

[0012] S500, vacuum drying: under vacuum conditions, the temperature is gradually raised to sublime the ice crystals, thereby removing the moisture in the sample and obtaining a dry powdery substance. This step retains the porous structure and large specific surface area of ​​the material, which is beneficial to the subsequent heat treatment process;

[0013] S600, heat treatment device setting: placing the freeze-dried powder in the downstream position of the heat treatment furnace, and placing nitrogen-containing compounds (such as urea, ammonia, etc., as an additional nitrogen source) in the upstream position, ensuring that the furnace is filled with argon atmosphere to exclude oxygen and other gases that may interfere with the reaction;

[0014] S700, heating treatment: starting the heat treatment furnace and heating according to a predetermined temperature rise program. During the heating process, the cobalt precursor in the powder will undergo decomposition and reduction reactions, and the nitrogen atoms generated by the decomposition of the ammonium salt and the nitrogen-containing compound will be doped into the nanotubes and the cobalt-based compound to form a nitrogen-doped catalytic material;

[0015] S800, cooling and pickling: After heating is completed, the sample is allowed to cool naturally to room temperature in an argon atmosphere, the sample is taken out and placed in an appropriate acid solution (such as dilute hydrochloric acid, dilute sulfuric acid, etc.) for pickling treatment to remove unreacted impurities and surface residues, and after pickling, it is washed with deionized water several times until neutral, and dried to obtain the final controllable nitrogen-doped electrocatalytic oxygen reduction synthesis H2O2 catalytic material.

[0016] Furthermore, the surface of the oxidized carbon nanotubes selected in S100 is pre-cleaned, and the specific content of the surface treatment is: using mechanical and chemical methods to remove oil stains on the surface of CNTs, including but not limited to using steam degreasing, organic solvent degreasing and electrochemical degreasing to remove grease and oil stains on the surface of CNTs, further removing oil stains, rust products and oxide films on the surface of CNTs through an etching process, deeply cleaning the surface of CNTs, improving the surface roughness, which is beneficial to subsequent processing and coating adhesion, using deionized water or pure water to wash CNTs to remove residual chemicals and impurities, and then drying to ensure that there is no residue on the surface of CNTs, in preparation for subsequent dispersion processing.

[0017] Furthermore, the oxidized carbon nanotubes selected in S100 are subjected to a dispersion treatment, and the specific content of the dispersion treatment is: adding CNTs to a mixed strong acid, and breaking the CNTs into ultra-short segments through cyclic alternating treatment of ultrasound and mechanical stirring, and generating a large number of carboxylic acid groups on the side walls and both ends, thereby improving the surface activity and dispersibility of the CNTs and preventing the occurrence of agglomeration; mixing the CNTs with an appropriate amount of solvent or matrix material, and performing a dispersion treatment through a ball mill or an ultrasonic disperser to ensure that the CNTs are evenly distributed in the solvent or matrix material, thereby improving the performance of the composite material; for the chemically modified CNTs, further performing a stabilization treatment to prevent them from agglomerating during subsequent processing; and improving the stability of the CNTs in the solution or matrix by adding a stabilizer or surfactant.

[0018] Furthermore, the ammonium salt described in S100 includes but is not limited to ammonium carbonate, ammonium bicarbonate, ammonium chloride, ammonium fluoride and ammonium iodide, and the mass ratio of the oxidized carbon nanotubes to the ammonium salt is 1:(0.1-1000).

[0019] Furthermore, the cobalt precursor described in S100 includes but is not limited to cobalt chloride, cobalt nitrate, cobalt sulfate and cobalt acetylacetonate, and the molar amount of the cobalt precursor is 1 to 10000 μmol.

[0020] Furthermore, the nitrogen-containing compound in S600 is one of melamine, urea, dicyandiamide and cyanuric acid, wherein the mass ratio of the powder obtained by freeze-drying to the nitrogen-containing compound is 1:(0.1-10000).

[0021] Furthermore, the heating temperature in S700 is 100-1000° C., and the heating time is 0.5-12 hours.

[0022] Furthermore, it is prepared by the method according to any one of claims 1 to 7.

[0023] On the other hand, an application of a catalytic material for electrocatalytic oxygen reduction synthesis of H2O2 by controllable nitrogen doping, characterized in that the catalytic material is used for the electrocatalytic oxygen reduction synthesis of H2O2 reaction, comprising:

[0024] Step 1: Prepare a suspension of catalytic material to ensure a concentration of 20 to 200 ug cm -2 The catalytic material is uniformly loaded on a 0.196 cm 2 On the rotating ring disk electrode, wait until the solvent evaporates completely to ensure that the catalytic material is firmly attached to the electrode surface;

[0025] Step 2: Install the rotating ring disk electrode loaded with the catalytic material on the electrochemical workstation, set a suitable potential range in a 0.1M HClO4 solution to perform cyclic voltammetry (CV) or linear sweep voltammetry (LSV) test to evaluate the electrochemical performance of the catalytic material, control the working electrode rotation speed to 1600rpm to eliminate the influence of the diffusion layer thickness on the current, measure the disk current and ring current, and calculate the selectivity of the electrocatalytic synthesis of H2O2 using the relevant equation, i.e., the collection efficiency method;

[0026] Step 3: Select or prepare carbon paper with good conductivity as the substrate, and use the same method to add the catalytic material at a concentration of 100 to 500 ug·cm -2 The loading capacity is loaded on 1cm 2 On the carbon paper, ensure that the catalytic material is evenly distributed on the carbon paper without falling off;

[0027] Step 4: Place the carbon paper loaded with catalytic material in the flow cell to ensure full contact with the electrolyte. Inject 75 mL of 0.1 M HClO4 solution into the flow cell as the electrolyte and set the electrolyte flow rate to 15 mL min. -1 , to ensure that the electrolyte is evenly distributed in the flow cell and carries away the reaction products;

[0028] Step 5: pure oxygen is introduced into the flow cell, and the oxygen flow rate is controlled to be 30 sccm (standard cubic centimeters per minute) to provide sufficient reactants;

[0029] Step 6: Within the given current density range of 20-50 mA cm -2 A constant current electrolysis test was carried out. Samples were taken regularly from the flow cell using the cerium sulfate titration method to determine the concentration of H2O2, and its yield and Faraday efficiency were calculated. The voltage change and current stability during the experiment were recorded to evaluate the stability and durability of the catalytic material.

[0030] Compared with the prior art, the preparation and application of the controllable nitrogen-doped electrocatalytic oxygen reduction catalytic material for synthesizing H2O2 has the following beneficial effects:

[0031] 1. The preparation method of the present invention retains the porous structure and large specific surface area of ​​the material by finely controlling each step, especially through freeze drying and vacuum drying processes, which significantly increases the number of active sites of the catalytic material, thereby improving its electrochemical performance. The doping of nitrogen further enhances the conductivity and catalytic activity of the material, so that it exhibits higher current density and lower overpotential in the electrocatalytic oxygen reduction reaction.

[0032] 2. In the preparation process of the present invention, the uniform distribution of cobalt elements on the surface of the nanotubes and its surroundings is ensured by ultrasonic treatment and dropwise addition of cobalt precursor. In addition, the surface of the oxidized carbon nanotubes is cleaned and dispersed to improve its surface roughness and dispersion, effectively preventing the occurrence of agglomeration. These measures jointly optimize the uniformity of the material, so that the catalytic material exhibits more stable performance in subsequent electrochemical tests and extends the service life of the material.

[0033] 3. The preparation method of the present invention can accurately control the doping amount and distribution position of nitrogen element, so as to adjust the electronic structure and catalytic performance of the catalytic material. In the electrocatalytic oxygen reduction synthesis reaction, this helps to improve the selectivity of the catalytic material for the target product and reduce the generation of by-products. At the same time, by optimizing the experimental conditions (such as electrolyte flow rate, oxygen flow rate, etc.), the yield and Faraday efficiency of the product are further improved. The characteristics of high selectivity and high yield make the catalytic material have broad application prospects in the field of energy conversion and storage. The characteristics of high selectivity and high yield make the catalytic material have broad application prospects in the field of energy conversion and storage.

[0034] Other advantages, objectives and features of the present invention will be set forth in part in the following description and, in part, will be apparent to those skilled in the art based on an examination of the following or may be taught from the practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0036] Figure 1 This is a scanning electron microscope image of the catalytic material for synthesizing H2O2 by electrocatalytic oxygen reduction with controllable nitrogen doping of the present invention;

[0037] Figure 2 A transmission electron microscope image of the catalytic material for synthesizing H2O2 by electrocatalytic oxygen reduction with controllable nitrogen doping of the present invention;

[0038] Figure 3 The X-ray diffraction pattern of the catalytic material for synthesizing H2O2 by electrocatalytic oxygen reduction with controllable nitrogen doping of the present invention;

[0039] Figure 4 A linear voltammetric curve diagram of the catalytic material for synthesizing H2O2 by electrocatalytic oxygen reduction with controllable nitrogen doping according to the present invention;

[0040] Figure 5 It is a H2O2 selectivity curve diagram of the catalytic material for synthesizing H2O2 by electrocatalytic oxygen reduction with controllable nitrogen doping of the present invention;

[0041] Figure 6 The actual production yield and Faraday efficiency of the catalytic material for synthesizing H2O2 by controllable nitrogen-doped electrocatalytic oxygen reduction of the present invention. DETAILED DESCRIPTION

[0042] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0043] Embodiment 1:

[0044] 30 mg OCNT and 200 mg ammonium chloride were dissolved in 30 mL H2O and ultrasonicated to homogeneity. Subsequently, 100 μL cobalt chloride solution (0.5 M) was added dropwise thereto and ultrasonication was continued for 1 hour. Then, the liquid was quickly frozen in liquid nitrogen and then transferred to a freeze dryer for drying for 48 hours to obtain a fluffy gray-white product. After taking it out, it was ground in a mortar, and then it and 2 g urea were placed in two porcelain boats (the porcelain boat carrying urea was placed upstream of the tube furnace, and the other was placed downstream) under argon and reacted at 400 ° C for 2 hours. The obtained product was treated with 1 M HNO3 at 60 ° C for 10 hours, centrifuged and filtered to neutrality, and dried to obtain the Co-OCNT catalyst.

[0045] Embodiment 2:

[0046] 30 mg OCNT and 400 mg ammonium chloride were dissolved in 30 mL H2O and ultrasonicated to uniformity. Subsequently, 100 μL cobalt chloride solution (0.5 M) was added dropwise thereto and ultrasonication was continued for 1 hour. Next, the liquid was quickly frozen in liquid nitrogen and then transferred to a freeze dryer for 48 hours to obtain a fluffy gray-white product. After taking it out, it was ground in a mortar, and then it and 4 g urea were placed in two porcelain boats (the porcelain boat carrying melamine was placed upstream of the tube furnace, and the other was placed downstream) under argon and reacted at 300 ° C for 2 hours. The obtained product was treated with 1MHNO3 at 60 ° C for 10 hours, centrifuged and filtered to neutrality, and dried to obtain the Co-OCNT catalyst.

[0047] Embodiment three:

[0048] 40 mg OCNT and 300 mg ammonium carbonate were dissolved in 30 mL H2O and ultrasonicated until uniform. Subsequently, 200 μL cobalt sulfate solution (0.5 M) was added dropwise and ultrasonicated for 1 hour. Next, the liquid was quickly frozen in liquid nitrogen and then transferred to a freeze dryer for drying for 48 hours to obtain a fluffy gray-white product. After taking it out, it was ground in a mortar. Then, it and 6 g dicyandiamide were placed in two porcelain boats (the porcelain boat carrying urea was placed upstream of the tube furnace, and the other was placed downstream) under argon and reacted at 500°C for 2 hours. The product was treated with 1 M HNO3 at 60°C for 10 hours, centrifuged and filtered to neutrality, and dried to obtain the Co-OCNT catalyst.

[0049] Embodiment 4:

[0050] 40 mg OCNT and 500 mg ammonium bicarbonate were dissolved in 30 mL H2O and ultrasonicated until uniform. Subsequently, 200 μL of cobalt acetylacetonate solution (0.5 M) was added dropwise thereto and ultrasonicated for 1 hour. Next, the liquid was quickly frozen in liquid nitrogen and then transferred to a freeze dryer for drying for 48 hours to obtain a fluffy gray-white product. After taking it out, it was ground in a mortar and then placed in two porcelain boats (the porcelain boat carrying urea was placed upstream of the tubular furnace, and the other was placed downstream) with 8 g cyanuric acid under argon and reacted at 400°C for 1 hour. The product was treated with 1 M HNO3 at 60°C for 10 hours, centrifuged and filtered to neutrality, and dried to obtain the Co-OCNT catalyst.

[0051] Embodiment five:

[0052] 60 mg OCNT and 700 mg ammonium fluoride were dissolved in 30 mL H2O and ultrasonicated until uniform. Subsequently, 400 μL cobalt nitrate solution (0.5 M) was added dropwise thereto and ultrasonicated for 1 hour. Next, the liquid was quickly frozen in liquid nitrogen and then transferred to a freeze dryer for drying for 48 hours to obtain a fluffy gray-white product. After taking it out, it was ground in a mortar and then placed in two porcelain boats (the porcelain boat carrying urea was placed upstream of the tubular furnace, and the other was placed downstream) with 10 g cyanuric acid under argon and reacted at 400 °C for 6 hours. The product was treated with 1 M HNO3 at 60 °C for 10 hours, centrifuged and filtered to neutrality, and dried to obtain the Co-OCNT catalyst.

[0053] Embodiment six:

[0054] 100 mg OCNT and 800 mg ammonium iodide were dissolved in 30 mL H2O and ultrasonicated until uniform. Subsequently, 500 μL of cobalt acetylacetonate solution (0.5 M) was added dropwise and ultrasonicated for 1 hour. Next, the liquid was quickly frozen in liquid nitrogen and then transferred to a freeze dryer for drying for 48 hours to obtain a fluffy gray-white product. After taking it out, it was ground in a mortar and then placed in two porcelain boats (the porcelain boat carrying urea was placed upstream of the tubular furnace, and the other was placed downstream) with argon and reacted at 700°C for 8 hours. The product was treated with 1 M HNO3 at 60°C for 10 hours, centrifuged and filtered to neutrality, and dried to obtain the Co-OCNT catalyst.

[0055] Embodiment seven:

[0056] 80 mg OCNT and 900 mg ammonium chloride were dissolved in 30 mL H2O and ultrasonicated until uniform. Subsequently, 700 μL cobalt sulfate solution (0.5 M) was added dropwise thereto and ultrasonicated for 1 hour. Next, the liquid was quickly frozen in liquid nitrogen and then transferred to a freeze dryer for drying for 48 hours to obtain a fluffy gray-white product. After taking it out, it was ground in a mortar and then placed in two porcelain boats (the porcelain boat carrying urea was placed upstream of the tubular furnace, and the other was placed downstream) with 5 g cyanuric acid under argon and reacted at 500°C for 3 hours. The product was treated with 1 M HNO3 at 60°C for 10 hours, centrifuged and filtered to neutrality, and dried to obtain the Co-OCNT catalyst.

[0057] Embodiment eight:

[0058] 70 mg OCNT and 1000 mg ammonium bicarbonate were dissolved in 30 mL H2O and ultrasonicated until uniform. Subsequently, 800 μL cobalt nitrate solution (0.5 M) was added dropwise thereto and ultrasonicated for 1 hour. Next, the liquid was quickly frozen in liquid nitrogen and then transferred to a freeze dryer for drying for 48 hours to obtain a fluffy gray-white product. After taking it out, it was ground in a mortar. Then, it and 3 g dicyandiamide were placed in two porcelain boats (the porcelain boat carrying urea was placed upstream of the tubular furnace, and the other was placed downstream) under argon and reacted at 500°C for 4 hours. The product was treated with 1 M HNO3 at 60°C for 10 hours, centrifuged and filtered to neutrality, and dried to obtain the Co-OCNT catalyst.

[0059] Embodiment nine:

[0060] The Co-OCNT catalytic material prepared in Example 1 was characterized in terms of its material structure and electrocatalytic performance in producing H2O2:

[0061] (1) Figure 1This is a scanning electron microscope image of the Co-OCNT catalytic material prepared in Example 1. It can be seen that the Co-OCNT prepared in this example maintains the tubular structure of OCNT, with a length of micrometers and a diameter of about 18 nanometers. Figure 2 This is a transmission electron microscope image of the Co-OCNT catalytic material prepared in Example 1. It can be seen that there are no large metal particles on the surface of the catalytic material prepared in this example, indicating that the prepared cobalt is highly dispersed. Figure 3 This is an X-ray diffraction diagram of the Co-OCNT catalytic material prepared in Example 1. It can be seen that there is no characteristic peak of metallic cobalt, indicating that the content of cobalt is low or highly dispersed;

[0062] (2) Co-OCNT was heated to 100 μg cm -2 The loading amount was loaded on the rotating ring disk electrode, and the disk current and ring current were tested in 0.1M HClO4 solution at a rotation speed of 1600rpm. Figure 4 As shown, it can be seen that the catalytic material prepared by Example 1 has a larger ring current, and the results of H2O2 selectivity are as follows Figure 5 As shown, it can be seen that the selectivity of the catalytic material prepared by Example 1 is greater than 80% in the wide voltage window range of 0.2-0.7V for H2O2;

[0063] (3) The catalytic material was heated to 200 ug cm -2 The loading capacity is loaded on the reaction area of ​​1cm 2 The hydrophobic carbon paper loaded with the catalytic material was placed in a flow cell for reaction. The reaction system was 75 mL of 0.1 M HClO4 solution. The electrolyte flow rate was controlled at 15 mL min -1 , oxygen flow rate is 30sccm, test current is 20~50mA·cm -2 , the results are as follows Figure 6 As shown in the figure, it can be seen that the Co-OCNT prepared by Example 1 exhibits high H2O2 yield and Faraday efficiency in the range of 20 to 50 mA·cm-2, especially at 50 mA·cm -2 The highest H2O2 yield was 3320mmol·g -1 ·h -1 , and the Faraday efficiency is above 70%.

[0064] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A method for preparing a catalytic material for synthesizing H2O2 by electrocatalytic oxygen reduction with controllable nitrogen doping, characterized in that: The preparation method comprises: S100, material preparation: selecting an appropriate amount of oxidized carbon nanotubes and ammonium salt to prepare a cobalt precursor, which will be used to introduce the cobalt element in a subsequent step; S200, aqueous solution dispersion: a certain volume of deionized water is taken and placed in a suitable container, and the weighed oxidized carbon nanotubes and ammonium salt are added to the aqueous solution in sequence, and an ultrasonic processor is used to fully ultrasonically disperse the carbon nanotubes to form a stable suspension. This step helps to increase the uniformity and activity of the material in the subsequent reaction; S300, adding dropwise: under the conditions of continuous stirring and ultrasonic dispersion, the cobalt precursor solution is added dropwise to the mixed suspension of the oxidized carbon nanotubes and the ammonium salt, and the dropping speed is controlled to avoid excessive local concentration, and the ultrasonic dispersion is continued for a period of time until the cobalt precursor is completely dissolved and evenly dispersed in the mixed solution. This step ensures that the cobalt element can be evenly distributed on the surface of the nanotubes and around them, providing favorable conditions for subsequent reactions; S400, freezing treatment: transferring the mixed solution to a freeze-drying device for freezing treatment, and rapidly freezing the water in the solution to form solid ice crystals by lowering the temperature; S500, vacuum drying: under vacuum conditions, the temperature is gradually raised to sublime the ice crystals, thereby removing the moisture in the sample and obtaining a dry powdery substance. This step retains the porous structure and large specific surface area of ​​the material, which is beneficial to the subsequent heat treatment process; S600, heat treatment device setting: placing the powder obtained by freeze drying in the downstream position of the heat treatment furnace, and placing the nitrogen-containing compound in the upstream position, ensuring that the furnace is filled with argon atmosphere to exclude oxygen and other gases that may interfere with the reaction; S700, heating treatment: starting the heat treatment furnace and heating according to a predetermined temperature rise program. During the heating process, the cobalt precursor in the powder will undergo decomposition and reduction reactions, and the nitrogen atoms generated by the decomposition of the ammonium salt and the nitrogen-containing compound will be doped into the nanotubes and the cobalt-based compound to form a nitrogen-doped catalytic material; S800, cooling and pickling: After heating is completed, the sample is allowed to cool naturally to room temperature in an argon atmosphere. The sample is taken out and placed in an appropriate acid solution for pickling to remove unreacted impurities and surface residues. After pickling, it is washed with deionized water several times until neutral, and dried to obtain the final controllable nitrogen-doped electrocatalytic oxygen reduction synthesis H2O2 catalytic material.

2. The method for preparing a catalytic material for synthesizing H2O2 by electrocatalytic oxygen reduction with controllable nitrogen doping according to claim 1, characterized in that: The surface of the oxidized carbon nanotubes selected in S100 is pre-cleaned, and the specific content of the surface treatment is: using mechanical and chemical methods to remove oil stains on the surface of CNTs, including but not limited to using steam degreasing, organic solvent degreasing and electrochemical degreasing to remove grease and oil stains on the surface of CNTs, further removing oil stains, rust products and oxide films on the surface of CNTs through an etching process, deeply cleaning the surface of CNTs, improving the surface roughness, which is beneficial to subsequent processing and coating adhesion, using deionized water or pure water to wash CNTs to remove residual chemicals and impurities, and then drying to ensure that there is no residue on the surface of CNTs, in preparation for subsequent dispersion processing.

3. The method for preparing a catalytic material for synthesizing H2O2 by electrocatalytic oxygen reduction with controllable nitrogen doping according to claim 2, characterized in that: The oxidized carbon nanotubes selected in S100 are subjected to a dispersion treatment, and the specific content of the dispersion treatment is: adding CNTs to a mixed strong acid, and cyclically alternatingly treating the CNTs with ultrasound and mechanical stirring to break the CNTs into ultra-short segments, and generating a large number of carboxylic acid groups on the side walls and both ends, thereby improving the surface activity and dispersibility of the CNTs and preventing the occurrence of agglomeration; mixing the CNTs with an appropriate amount of solvent or matrix material, and performing a dispersion treatment by ball milling or ultrasonic disperser to ensure that the CNTs are evenly distributed in the solvent or matrix material, thereby improving the performance of the composite material; for the chemically modified CNTs, further performing a stabilization treatment to prevent them from agglomerating during subsequent processing; and improving the stability of the CNTs in the solution or matrix by adding a stabilizer or surfactant.

4. The method for preparing a catalytic material for synthesizing H2O2 by electrocatalytic oxygen reduction with controllable nitrogen doping according to claim 1, characterized in that: The ammonium salt in S100 includes but is not limited to ammonium carbonate, ammonium bicarbonate, ammonium chloride, ammonium fluoride and ammonium iodide, and the mass ratio of the oxidized carbon nanotubes to the ammonium salt is 1:(0.1-1000).

5. The method for preparing a catalytic material for synthesizing H2O2 by electrocatalytic oxygen reduction with controllable nitrogen doping according to claim 1, characterized in that: The cobalt precursor described in S100 includes but is not limited to cobalt chloride, cobalt nitrate, cobalt sulfate and cobalt acetylacetonate, and the molar amount of the cobalt precursor is 1 to 10000 μmol.

6. The method for preparing a catalytic material for synthesizing H2O2 by electrocatalytic oxygen reduction with controllable nitrogen doping according to claim 1, characterized in that: The nitrogen-containing compound in S600 is one of melamine, urea, dicyandiamide and cyanuric acid, wherein the mass ratio of the powder obtained by freeze drying to the nitrogen-containing compound is 1:(0.1-10000).

7. The method for preparing a catalytic material for synthesizing H2O2 by electrocatalytic oxygen reduction with controllable nitrogen doping according to claim 1, characterized in that: The heating temperature in S700 is 100 to 1000° C., and the heating time is 0.5 to 12 hours.

8. The method for preparing a catalytic material for synthesizing H2O2 by electrocatalytic oxygen reduction with controllable nitrogen doping according to claim 1, characterized in that: The method is prepared by any one of claims 1 to 7.

9. Application of a catalytic material for synthesizing H2O2 by electrocatalytic oxygen reduction with controllable nitrogen doping, characterized in that: The catalytic material is used for electrocatalytic oxygen reduction to synthesize H2O2 reaction, including: Step 1: Prepare a suspension of catalytic material to ensure a concentration of 20 to 200 ug cm -2 The catalytic material is uniformly loaded on a 0.196 cm 2 On the rotating ring disk electrode, wait until the solvent evaporates completely to ensure that the catalytic material is firmly attached to the electrode surface; Step 2: Install the rotating ring disk electrode loaded with the catalytic material on the electrochemical workstation, set a suitable potential range in a 0.1M HClO4 solution to perform cyclic voltammetry (CV) or linear sweep voltammetry (LSV) test to evaluate the electrochemical performance of the catalytic material, control the working electrode rotation speed to 1600rpm to eliminate the influence of the diffusion layer thickness on the current, measure the disk current and ring current, and calculate the selectivity of the electrocatalytic synthesis of H2O2 using the relevant equation, i.e., the collection efficiency method; Step 3: Select or prepare carbon paper with good conductivity as the substrate, and use the same method to add the catalytic material at a concentration of 100 to 500 ug·cm -2 The loading capacity is loaded on 1cm 2 On the carbon paper, ensure that the catalytic material is evenly distributed on the carbon paper without falling off; Step 4: Place the carbon paper loaded with catalytic material in the flow cell to ensure full contact with the electrolyte. Inject 75 mL of 0.1 M HClO4 solution into the flow cell as the electrolyte and set the electrolyte flow rate to 15 mL min. -1 , to ensure that the electrolyte is evenly distributed in the flow cell and carries away the reaction products; Step 5: pure oxygen is introduced into the flow cell, and the oxygen flow rate is controlled to be 30 sccm (standard cubic centimeters per minute) to provide sufficient reactants; Step 6: Within the given current density range of 20-50 mA cm -2 A constant current electrolysis test was carried out. Samples were taken regularly from the flow cell using the cerium sulfate titration method to determine the concentration of H2O2, and its yield and Faraday efficiency were calculated. The voltage change and current stability during the experiment were recorded to evaluate the stability and durability of the catalytic material.

Citation Information

Cited By

  • Bioelectricity-Fenton system based on modified carbon nanotube cathode catalyst and method for degrading organic pollutants by bioelectricity-Fenton system

    CN119750766A