Preparation method of sulfur-doped dual-MOF heterostructure catalyst S-ZIF-67 (at) MIL-53-NF
By preparing the sulfur-doped double MOF heterostructure catalyst S-ZIF-67@MIL-53-NF, the problem of poor OER performance of non-precious metal catalysts in electrolytic water is solved, and efficient OER catalysis and stability improvement is achieved, revealing that Structural effect relationship between double MOF heterostructure and OER.
Patent Information
- Application Number
- CN202411158187.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-12
AI Technical Summary
The existing non-precious metal catalysts have poor catalytic performance in electrolyzed water, and the conductivity of MOF-based catalysts is low, which limits its efficiency of oxygen evolution reaction under high current density. The regulation and strong interaction mechanism of heterostructure catalyst interface are unclear. , restricts the optimal design of the catalyst.
The preparation method of S-ZIF-67@MIL-53-NF, a sulfur-doped double MOF heterostructure catalyst, is used to form a heterostructure of ZIF-67 and MIL-53, optimize the OER mechanism, improve the electron transmission rate, and pass Room temperature sulfur doping treatment reduces OER activation energy and realizes the synergistic effect of the catalyst interface.
It significantly improves the catalytic performance of OER, reduces the overpotential, improves the stability and activity of the catalyst, realizes the transformation from the adsorbent evolution mechanism to the lattice oxygen-mediated mechanism, and breaks through the limits of traditional AEM theory.
Smart Images

Figure CN118932404A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of new energy materials, and specifically relates to a method for preparing a sulfur-doped dual MOF heterostructure catalyst S-ZIF-67@MIL-53-NF. Background Art
[0002] In recent years, the growing energy demand and corresponding environmental issues have accelerated the development of renewable energy and clean energy. Water electrolysis (EWS) is an environmentally friendly, simple, and efficient high-purity hydrogen production technology that can not only avoid the uneven geographical distribution and intermittent supply of other renewable energy sources, but also reduce the waste of excess electricity. Water electrolysis includes the anodic oxygen evolution reaction (OER) and the cathodic hydrogen evolution reaction (HER). The anodic OER requires a multi-electron transfer process and produces a large overpotential; overcoming the slow kinetic process requires a lot of energy, making it a rate-limiting step, which seriously hinders the practical application of water electrolysis. Traditional noble metal catalysts, such as iridium and ruthenium, have been shown to have high catalytic activity for OER. However, their extremely high cost and instability limit their large-scale application. Therefore, the design and development of economical, efficient, abundant, and durable OER electrocatalysts is one of the main goals of contemporary research. In the past few years, catalytic materials based on transition metals iron, cobalt, and nickel have become the most promising OER catalysts. Metal-organic frameworks (MOFs) have attracted extensive attention in many fields due to their advantages such as large specific surface area, potential for changing metal cations, and feasible post-synthesis modification. Among various MOF structures, zeolitic imidazolate frameworks (ZIFs) formed with imidazolyl ligands (Im) and transition metals as cations (C) have been widely studied in various applications. Among various ZIFs, ZIF-67 is Co 2+ Self-assembled structures of metal ions interconnected with 2-methylimidazole (Hmim) organic compounds with cubic crystal symmetry Due to the special flexibility of ZIF-67 in structural / morphological engineering and composition control, ZIF-67 and its derivatives have been explored for various applications, including secondary batteries, supercapacitors, fuel cells, gas adsorption / separation, and electrochemical / photoelectrochemical water splitting applications. The morphology of ZIF-67 can be effectively controlled by changing the solvent type, ratio, or the ratio of organic ligands and cobalt sources, including 3D dodecahedrons, flower-like shapes, and 2D spindle-shaped flakes. The poor conductivity of ZIF-67 limits its direct use as a catalyst for water electrolysis. Studies have shown that 2D catalysts have lower conductivity and more exposed active sites, which makes 2D catalysts perform better than 3D catalysts in water electrolysis applications. In some ZIF-67 derivatives, the formation of heterostructures with modified electronic structures at the interface is an excellent strategy to improve the electrocatalytic activity. However, few groups have provided sufficient experimental evidence to explain the role of heterostructure formation in obtaining high catalytic activity. In addition, new strategies are needed to precisely manipulate the interface between the two phases of the heterostructure to stimulate strong interactions and close contacts. At the same time, during the synthesis process, the ZIF-67 structure is combined with other structures with multiple active sites such as layered double hydroxides (LDHs) or other MOFs to form a heterojunction, which can exert the synergistic effect of the two high-quality structures to achieve a catalytic performance of 1+1>2. In order to further improve the OER performance, sulfur (S) doping can weaken the strong binding of intermediates (O* / OH* / OOH*) on the catalyst surface during the OER process, effectively reduce the activation energy of OER kinetics, and may realize the transformation of the OER mechanism from the adsorbate evolution mechanism (AEM) to the lattice oxygen mediated mechanism (LOM). The intermediates OH* and OOH* are no longer in a linear adsorption relationship, thus breaking through the AEM theoretical limit potential of 370mV and reaching a lower overpotential. Therefore, the use of ZIF-67 self-supporting composite materials for oxygen evolution reaction still faces the following problems: how to accurately design and synthesize heterostructure catalysts that work together with ZIF-67 and other MOFs to have ideal morphology and atomic coordination environment; the precise regulation of the interface of heterostructure catalysts and the unclear mechanism of strong interaction between the two phases of heterostructures restrict the optimization design of catalysts. Summary of the invention
[0003] Technical issues solved:
[0004] This application aims at the technical problems that the non-precious metals in the prior art have poor catalytic performance in oxygen evolution reaction (OER) at high current density compared with precious metal catalysts, and the MOF-based catalysts have low conductivity and poor catalytic performance. It provides a method for preparing a sulfur-doped dual MOF heterostructure catalyst S-ZIF-67@MIL-53-NF, which allows two two-dimensional MOF materials to form a heterostructure in structure, generating strong interactions to accelerate the electron transfer rate between the catalyst interface, and optimizes the adsorption of OER mechanism intermediates through simple room temperature sulfur doping, which may realize the transformation of OER mechanism from adsorbate evolution mechanism (AEM) to lattice oxygen mediated mechanism (LOM), greatly improving the OER catalytic performance of dual MOF materials. At the same time, based on the changes in the catalytic environment space, it is beneficial to affect the selectivity and kinetics of the electrochemical reaction, reveal the structure-activity relationship between dual MOF heterostructure materials and OER, and further guide the synthesis of new and efficient dual MOF heterostructure material catalysts.
[0005] Technical solution:
[0006] To achieve the above objectives, this application is implemented through the following technical solutions:
[0007] A method for preparing a sulfur-doped dual MOF heterostructure catalyst S-ZIF-67@MIL-53-NF specifically comprises the following steps:
[0008] The first step: the nickel foam NF is subjected to ultrasonic treatment for 15 minutes in sequence with acetone, dilute hydrochloric acid, ethanol and deionized water to remove impurities and nickel oxide on the surface of the nickel foam; deionized water, anhydrous ethanol and N, N-dimethylformamide are mixed in a volume ratio of deionized water: anhydrous ethanol: DMF = 1:1:14 to obtain 40 mL of solvent A, and the precursor iron salt and the organic ligand terephthalic acid are dissolved in the solvent A in a molar ratio of precursor iron salt: terephthalic acid = 1:3 to obtain solution B and stir, the speed is controlled to be 500r / min, and the stirring time is 0.1-2 hours;
[0009] Step 2: Evenly distribute solvent A into three 50 mL polytetrafluoroethylene liners, put the nickel foam NF that has been ultrasonically treated in the first step into each liner, and install the liner into a stainless steel reactor;
[0010] Step 3: Place the reactor in a forced air drying oven and perform a hydrothermal reaction at 110-130°C for 10-18 hours. After the reaction is completed, wait for the reactor to cool naturally, take out the sample, and rinse it with N,N-dimethylformamide, anhydrous ethanol and deionized water in sequence to obtain MIL-53 / NF;
[0011] Step 4: Dissolve 0.4-0.6 mg of the precursor cobalt salt in 30 mL of deionized water according to a mass volume ratio to obtain solution C, take the organic ligand 2-methylimidazole at a molar ratio of precursor cobalt salt: 2-methylimidazole = 1:8, take the sulfur source at a mass ratio of precursor cobalt salt: sulfur source = 1:0.5-2, dissolve the organic ligand 2-methylimidazole and the sulfur source in 30 mL of deionized water to obtain solution D, stir solutions C and D for 5 minutes respectively, and quickly pour solution C into solution D to obtain solution E;
[0012] Step 5: Place MIL-53 / NF into solution E and stir it, control the speed to 300 r / min, and stir for 1-2 hours; let the sample stand for aging. After the reaction is completed, clean the sample and place it in a vacuum drying oven. Dry it in a vacuum at 60°C for 8 hours to finally generate the S-doped dual MOF heterostructure catalyst S-ZIF-67@MIL-53 / NF.
[0013] Furthermore, the size of the nickel foam is 2 cm*3 cm, and the raw materials in solvent A are 2.5 mL of deionized water, 2.5 mL of anhydrous ethanol and 35 mL of N,N-dimethylformamide.
[0014] Furthermore, in the reaction solution B, the concentration of iron ions is 25 mmol / L, and the molar ratio of the precursor iron salt to the organic ligand terephthalic acid is 1:3; the concentration of cobalt ions in solution E is 25 mmol / L, and the molar ratio of the precursor cobalt salt to 2-methylimidazole in solution E is 1:8.
[0015] Furthermore, the precursor iron salt is ferric nitrate nonahydrate; and the precursor cobalt salt is cobalt nitrate hexahydrate.
[0016] Furthermore, the sulfur source is sodium thiosulfate pentahydrate and / or thiourea.
[0017] Furthermore, in the fifth step, the reaction temperature is room temperature and the reaction time is 1-3 hours.
[0018] Furthermore, the solvents for cleaning the sample in the third step are N,N-dimethylformamide, anhydrous ethanol and deionized water in sequence, and the amount of each cleaning agent is 15-30 mL.
[0019] Furthermore, the solvent for cleaning the sample in the fifth step is ethanol.
[0020] Principle explanation: Based on the synergistic effect of heterogeneous structure catalysts, the bonding between the heterogeneous interfaces formed by ZIF-67 and MIL-53 improves the electron transfer rate and solves the problem of poor conductivity of MOF materials themselves; and based on the strain effect of the structure, the change of the crystal structure affects the adsorption energy of the intermediates, improving the catalytic performance of the material; and based on the electronic interaction of the structure, the different arrangements of different energy bands will lead to charge transfer at the interface, which is beneficial to surface electronic modulation. Finally, the incorporation of sulfur can weaken the strong binding of intermediates (O* / OH* / OOH*) on the catalyst surface during the OER process, further improving the oxygen evolution reaction (OER) activity of the catalyst.
[0021] Beneficial effects:
[0022] The present application provides a method for preparing a sulfur-doped dual MOF heterostructure catalyst S-ZIF-67@MIL-53-NF, which has the following beneficial effects compared with the prior art:
[0023] 1. The catalyst prepared by this method is a dual MOF heterostructure, which exhibits a uniformly distributed, closely connected two-dimensional sheet morphology on nickel foam;
[0024] 2. The catalyst S-ZIF-67@MIL-53-NF prepared by this method is based on the ZIF-67 structure combined with other MIL-53 with multiple active sites to form a heterojunction, which can exert the synergistic effect of the two high-quality structures to achieve a catalytic performance of 1+1>2;
[0025] 3. In order to further improve the OER performance, sulfur (S) doping can weaken the strong binding of intermediates (O* / OH* / OOH*) in the OER process on the catalyst surface, effectively reduce the activation energy of OER kinetics, and possibly realize the transformation of the OER mechanism from the adsorbate evolution mechanism (AEM) to the lattice oxygen mediated mechanism (LOM). The intermediates OH* and OOH* are no longer in a linear adsorption relationship, thus breaking through the AEM theoretical limit potential of 370 mV and reaching a lower overpotential;
[0026] 4. During the experimental test, we measured the S-ZIF-67@MIL-53-NF in 1 M KOH electrolyte solution by linear sweep voltammetry at a high current density of 500 mA cm -2 , 1A cm -2 and 1.5A cm -2 The overpotentials (relative to standard hydrogen electrode, RHE) of S-ZIF-67@MIL-53 / NF were 292 mV, 320 mV, and 323 mV, respectively, which were much lower than those of MIL-53 / NF catalyst and NF at a large current density of 500 mA cm -2 , 1A cm -2and 1.5A cm -2 The overpotentials (relative to standard hydrogen electrode, RHE) under the conditions of 5 mV s -1 The OER polarization curves were obtained at a scan rate of 400–600 mA cm -2 The stability test results under a constant current density showed that there was no obvious decrease in activity for 70 consecutive hours. The S-doped dual MOF heterostructure catalyst S-ZIF-67@MIL-53-NF has high activity and stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 1 is a scanning electron microscope image of the S-ZIF-67@MIL-53 / NF catalyst obtained in Example 1 of the present application, wherein a is the structural morphology of the S-ZIF-67@MIL-53 / NF catalyst at a low magnification, and b is the two-dimensional sheet structure of the S-ZIF-67@MIL-53 / NF catalyst at a high magnification;
[0028] Figure 2 : is a scanning electron microscope energy spectrum of the S-ZIF-67@MIL-53 / NF catalyst obtained in Example 1 of the present application; wherein a is an EDS layered image, and b is a surface total spectrum;
[0029] Figure 3 1 is a transmission electron microscope image of the S-ZIF-67@MIL-53 / NF catalyst obtained in Example 1 of the present application; wherein a is the structural morphology of the S-ZIF-67@MIL-53 / NF catalyst at a low magnification, and b is the S-ZIF-67@MIL-53 / NF catalyst at a high magnification;
[0030] Figure 4 It is the LSV (linear voltammetric sweep) curve of the catalytic activity of oxygen evolution reaction of S-ZIF-67@MIL-53 / NF, MIL-53 / NF catalyst and NF obtained in Example 1 of the present application in alkaline 1M KOH solution. In the figure, the blue line represents the LSV curve of the catalytic activity of oxygen evolution reaction of S-ZIF-67@MIL-53 / NF catalyst, the red line represents the LSV curve of the catalytic activity of oxygen evolution reaction of MIL-53 / NF catalyst, and the black line represents the LSV curve of the catalytic activity of oxygen evolution reaction of NF;
[0031] Figure 5 This is the constant potential polarization (It) curve of the stability test of S-ZIF-67@MIL-53 / NF obtained in Example 1 of the present application in alkaline 1M KOH. DETAILED DESCRIPTION
[0032] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Embodiment 1:
[0034] A method for preparing a sulfur-doped dual MOF heterostructure catalyst S-ZIF-67@MIL-53-NF specifically comprises the following steps:
[0035] The first step: 2cm*3cm nickel foam NF is subjected to ultrasonic treatment for 15 minutes with acetone, dilute hydrochloric acid, ethanol and deionized water in sequence to remove impurities and nickel oxide on the surface of the nickel foam; 2.5mL deionized water, 2.5mL anhydrous ethanol and 35mL N,N-dimethylformamide are mixed to obtain 40mL solvent A in a volume ratio of deionized water: anhydrous ethanol: DMF=1:1:14, the molar ratio of the precursor iron salt to the organic ligand terephthalic acid is 1:3, the precursor iron salt nonahydrate ferric nitrate and the organic ligand terephthalic acid are dissolved in the solvent A to obtain a solution B and stir, the speed is controlled to be 500r / min, the stirring time is 0.1-2 hours, and the concentration of iron ions in the reaction solution B is 25mmol / L;
[0036] Step 2: Evenly distribute solvent A into three 50 mL polytetrafluoroethylene liners, put the nickel foam NF that has been ultrasonically treated in the first step into each liner, and install the liner into a stainless steel reactor;
[0037] Step 3: Place the reactor in a forced air drying oven and perform a hydrothermal reaction at 110-130°C for 10-18 hours. After the reaction is completed, wait for the reactor to cool naturally, take out the sample, and rinse it with N,N-dimethylformamide, anhydrous ethanol and deionized water in sequence. The amount of each cleaning agent is 15-30 mL to obtain MIL-53 / NF;
[0038] Step 4: Dissolve 0.44 mg of the precursor cobalt salt cobalt nitrate hexahydrate in 30 mL of deionized water according to the mass volume ratio to obtain solution C, the molar ratio of the precursor cobalt salt cobalt nitrate hexahydrate and 2-methylimidazole is 1:8, the mass ratio of the precursor cobalt salt: sulfur source = 1:0.5, dissolve the precursor cobalt salt, the organic ligand 2-methylimidazole and the sulfur source sodium thiosulfate pentahydrate in 30 mL of deionized water to obtain solution D, stir solutions C and D for 5 minutes respectively, quickly pour solution C into solution D to obtain solution E, the concentration of cobalt ions in solution E is 25 mmol / L;
[0039] Step 5: Place MIL-53 / NF into solution E and stir it, control the speed to 300 r / min, and stir for 1-2 hours; place the sample for aging, the reaction temperature is room temperature, and the reaction time is 1-3 hours. After the reaction, wash the sample with ethanol, and place the sample in a vacuum drying oven, vacuum dry it at 60°C for 8 hours, and finally generate the S-doped dual MOF heterostructure catalyst S-ZIF-67@MIL-53 / NF.
[0040] The S-ZIF-67@MIL-53 / NF catalyst obtained above was observed by scanning electron microscopy (SEM). Figure 1 As shown in Figure 2, the morphology of the obtained S-ZIF-67@MIL-53 / NF catalyst is a two-dimensional sheet, and its sheet structure is uniform in size and evenly distributed on the nickel foam. Figure 2 The scanning electron microscope shown in the figure shows the distribution of S, Fe and Co elements in the S-ZIF-67@MIL-53 / NF catalyst and the content of the corresponding elements.
[0041] Electrochemical testing:
[0042] (1) Preparation of catalytic electrode
[0043] The S-ZIF-67@MIL-53 / NF catalyst prepared above was cut into 1*1 cm -2 The electrochemical tests were performed on a Coster electrochemical workstation at room temperature. For the oxygen evolution reaction (OER) test, we used a standard three-electrode system with the prepared sample as the working electrode, a graphite rod as the counter electrode, and a standard Hg / HgO electrode as the reference. The electrolyte used was 1 M KOH with a pH set at 14.
[0044] (2) Oxygen evolution reaction (OER) activity test
[0045] At 5mV s -1 The OER polarization curves were obtained at a scan rate of 400–600 mA cm -2 The stability test was carried out under constant current density.
[0046] The OER performance of S-ZIF-67@MIL-53 / NF obtained in Example 1 was tested in a three-electrode battery system using a Coster workstation. In the three-electrode system, a mercury oxide electrode and a graphite rod were used as a reference electrode and a counter electrode, respectively.
[0047] Figure 4The linear sweep voltammetric curves of S-ZIF-67@MIL-53 / NF, MIL-53 / NF catalyst and NF obtained in Example 1 of the present invention in an alkaline 1M KOH solution, with a potential range of -1V to 4V (relative to mercury oxide electrode, GOE), a sweep rate of 5mV / s, and an IR compensation of 80%, in which the blue line represents the LSV curve of the catalytic activity of the oxygen evolution reaction of the S-ZIF-67@MIL-53 / NF catalyst, the red line represents the LSV curve of the catalytic activity of the oxygen evolution reaction of the MIL-53 / NF catalyst, and the black line represents the LSV curve of the catalytic activity of the oxygen evolution reaction of the NF; Figure 4 It can be seen that the overpotential (relative to the standard hydrogen electrode, RHE) of the S-ZIF-67@MIL-53 / NF catalyst is significantly lower than that of the MIL-53 / NF catalyst and NF, indicating that S-ZIF-67 has a significant promoting effect on improving the catalytic activity of the oxygen evolution reaction.
[0048] Table 1 shows the S-ZIF-67@MIL-53 / NF, MIL-53 / NF catalyst and NF obtained in Example 1 of the present invention. Figure 3 The obtained current density is 500mA cm -2 , 1A cm -2 and 1.5A cm -2 The corresponding oxygen evolution reaction overpotential is 500 mA cm -2 , 1A cm -2 and 1.5A cm -2 The overpotentials (relative to standard hydrogen electrode, RHE) of S-ZIF-67@MIL-53 / NF were 292 mV, 320 mV, and 323 mV, respectively. In contrast, the MIL-53 / NF catalyst and NF exhibited a high current density of 500 mA cm -2 , 1A cm -2 and 1.5A cm -2 The overpotentials (relative to standard hydrogen electrode, RHE) under the reaction conditions are 377 / 722 mV, 474 / 869 mV and 529 / 929 mV, which are far inferior to the catalytic performance of S-ZIF-67@MIL-53 / NF.
[0049] Table 1 shows the S-ZIF-67@MIL-53 / NF, MIL-53 / NF catalyst and NF obtained in Example 1 of the present invention. Figure 3 The obtained current density is 500mAcm -2 , 1A cm -2 and 1.5A cm -2 The corresponding oxygen evolution reaction overpotential
[0050]
[0051] Figure 5 The S-ZIF-67@MIL-53 / NF obtained in Example 1 of the present invention was subjected to a current density of 400-600 mA cm in alkaline 1 M KOH. -2 The stability test (It) curve under the conditions is given by Figure 5 It can be seen that after 70 hours of continuous testing, the curve did not show an obvious decline, only a slight reduction, indicating that the oxygen evolution reaction stability of S-ZIF-67@MIL-53 / NF under alkaline and high current density conditions is good.
[0052] Example 2
[0053] A method for preparing a sulfur-doped dual MOF heterostructure catalyst S-ZIF-67@MIL-53-NF specifically comprises the following steps:
[0054] The first step: 2cm*3cm nickel foam NF is subjected to ultrasonic treatment for 15 minutes with acetone, dilute hydrochloric acid, ethanol and deionized water in sequence to remove impurities and nickel oxide on the surface of the nickel foam; 2.5mL deionized water, 2.5mL anhydrous ethanol and 35mL N,N-dimethylformamide are mixed to obtain 40mL solvent A in a volume ratio of deionized water: anhydrous ethanol: DMF=1:1:14, the molar ratio of the precursor iron salt to the organic ligand terephthalic acid is 1:3, the precursor iron salt nonahydrate ferric nitrate and the organic ligand terephthalic acid are dissolved in the solvent A to obtain a solution B and stir, the speed is controlled to be 500r / min, the stirring time is 0.1-2 hours, and the concentration of iron ions in the reaction solution B is 25mmol / L;
[0055] Step 2: Evenly distribute solvent A into three 50 mL polytetrafluoroethylene liners, put the nickel foam NF that has been ultrasonically treated in the first step into each liner, and install the liner into a stainless steel reactor;
[0056] Step 3: Place the reactor in a forced air drying oven and perform a hydrothermal reaction at 110-130°C for 10-18 hours. After the reaction is completed, wait for the reactor to cool naturally, take out the sample, and rinse it with N,N-dimethylformamide, anhydrous ethanol and deionized water in sequence. The amount of each cleaning agent is 15-30 mL to obtain MIL-53 / NF;
[0057] Step 4: Dissolve 0.4 mg of the precursor cobalt salt cobalt nitrate hexahydrate in 30 mL of deionized water according to the mass volume ratio to obtain solution C, the molar ratio of the precursor cobalt salt cobalt nitrate hexahydrate and 2-methylimidazole is 1:8, the mass ratio of the precursor cobalt salt: sulfur source = 1:1, dissolve the precursor cobalt salt, the organic ligand 2-methylimidazole and the sulfur source sodium thiosulfate pentahydrate in 30 mL of deionized water to obtain solution D, stir solutions C and D for 5 minutes respectively, and quickly pour solution C into solution D to obtain solution E, the concentration of cobalt ions in solution E is 25 mmol / L;
[0058] Step 5: Place MIL-53 / NF into solution E and stir it, control the speed to 300 r / min, and stir for 1-2 hours; place the sample for aging, the reaction temperature is room temperature, and the reaction time is 1-3 hours. After the reaction, wash the sample with ethanol, and place the sample in a vacuum drying oven, vacuum dry it at 60°C for 8 hours, and finally generate the S-doped dual MOF heterostructure catalyst S-ZIF-67@MIL-53 / NF.
[0059] The S-ZIF-67@MIL-53 / NF catalyst obtained above was observed by scanning electron microscopy (SEM). Figure 1 As shown in Figure 2, the morphology of the obtained S-ZIF-67@MIL-53 / NF catalyst is a two-dimensional sheet, and its sheet structure is uniform in size and evenly distributed on the nickel foam. Figure 2 The scanning electron microscope shown in the figure shows the distribution of S, Fe and Co elements in the S-ZIF-67@MIL-53 / NF catalyst and the content of the corresponding elements.
[0060] The S-ZIF-67@MIL-53 / NF catalyst obtained above was observed by transmission electron microscopy. Figure 3 Transmission electron microscopy shows that the catalyst has a thin sheet structure and presents a stacked sheet morphology. At the same time, lattice patterns can be observed, indicating that the catalyst forms crystals. The stacked two-dimensional sheet structure of S-ZIF-67@MIL-53 / NF is conducive to promoting electron transfer and improving the activity of oxygen evolution reaction.
[0061] Embodiment 3:
[0062] A method for preparing a sulfur-doped dual MOF heterostructure catalyst S-ZIF-67@MIL-53-NF specifically comprises the following steps:
[0063] The first step: 2cm*3cm nickel foam NF is subjected to ultrasonic treatment for 15 minutes with acetone, dilute hydrochloric acid, ethanol and deionized water respectively to remove impurities and nickel oxide on the surface of the nickel foam; 2.5mL deionized water, 2.5mL anhydrous ethanol and 35mL N,N-dimethylformamide are mixed to obtain 40mL solvent A according to the volume ratio of deionized water: anhydrous ethanol: DMF=1:1:14, the molar ratio of the precursor iron salt to the organic ligand terephthalic acid is 1:3, the precursor iron salt nonahydrate ferric nitrate and the organic ligand terephthalic acid are dissolved in the solvent A to obtain solution B and stir, the speed is controlled to be 500r / min, the stirring time is 0.1-2 hours, and the concentration of iron ions in the reaction solution B is 25mmol / L;
[0064] Step 2: Evenly distribute solvent A into three 50 mL polytetrafluoroethylene liners, put the nickel foam NF that has been ultrasonically treated in the first step into each liner, and install the liner into a stainless steel reactor;
[0065] Step 3: Place the reactor in a forced air drying oven and perform a hydrothermal reaction at 110-130°C for 10-18 hours. After the reaction is completed, wait for the reactor to cool naturally, take out the sample, and rinse it with N,N-dimethylformamide, anhydrous ethanol and deionized water in sequence. The amount of each cleaning agent is 15-30 mL to obtain MIL-53 / NF;
[0066] Step 4: Dissolve 0.6 mg of the precursor cobalt salt cobalt nitrate hexahydrate in 30 mL of deionized water according to the mass volume ratio to obtain solution C, the molar ratio of the precursor cobalt salt cobalt nitrate hexahydrate and 2-methylimidazole is 1:8, the mass ratio of the precursor cobalt salt: sulfur source = 1:2, dissolve the precursor cobalt salt, the organic ligand 2-methylimidazole and the sulfur source sodium thiosulfate pentahydrate in 30 mL of deionized water to obtain solution D, stir solutions C and D for 5 minutes respectively, quickly pour solution C into solution D to obtain solution E, the concentration of cobalt ions in solution E is 25 mmol / L;
[0067] Step 5: Place MIL-53 / NF into solution E and stir it, control the speed to 300 r / min, and stir for 1-2 hours; place the sample for aging, the reaction temperature is room temperature, and the reaction time is 1-3 hours. After the reaction, wash the sample with ethanol, and place the sample in a vacuum drying oven, vacuum dry it at 60°C for 8 hours, and finally generate the S-doped dual MOF heterostructure catalyst S-ZIF-67@MIL-53 / NF.
[0068] In summary, the S-doped dual MOF heterostructure catalyst S-ZIF-67@MIL-53 / NF prepared by the preparation method of the present invention has good catalytic activity for oxygen evolution reaction, that is, good oxygen evolution reaction activity and excellent stability, and the preparation process is simple, the cost is low, and it is easy to produce on an industrial scale.
[0069] The above description has fully disclosed the specific embodiments of the present invention. It should be pointed out that any changes made by those skilled in the art to the specific embodiments of the present invention do not deviate from the scope of the claims of the present invention. Accordingly, the scope of the claims of the present invention is not limited to the above specific embodiments.
Claims
1. A method for preparing a sulfur-doped dual MOF heterostructure catalyst S-ZIF-67@MIL-53-NF, characterized in that: The specific steps are as follows: The first step: the nickel foam NF is subjected to ultrasonic treatment for 15 minutes in sequence with acetone, dilute hydrochloric acid, ethanol and deionized water to remove impurities and nickel oxide on the surface of the nickel foam; deionized water, anhydrous ethanol and N, N-dimethylformamide are mixed in a volume ratio of deionized water: anhydrous ethanol: DMF = 1:1:14 to obtain 40 mL of solvent A, and the precursor iron salt and the organic ligand terephthalic acid are dissolved in the solvent A in a molar ratio of precursor iron salt: terephthalic acid = 1:3 to obtain solution B and stir, the speed is controlled to be 500r / min, and the stirring time is 0.1-2 hours; Step 2: Evenly distribute solvent A into three 50 mL polytetrafluoroethylene liners, put the nickel foam NF that has been ultrasonically treated in the first step into each liner, and install the liner into a stainless steel reactor; Step 3: Place the reactor in a forced air drying oven and perform a hydrothermal reaction at 110-130°C for 10-18 hours. After the reaction is completed, wait for the reactor to cool naturally, take out the sample, and rinse it with N,N-dimethylformamide, anhydrous ethanol and deionized water in sequence to obtain MIL-53 / NF; Step 4: Dissolve 0.4-0.6 mg of the precursor cobalt salt in 30 mL of deionized water according to a mass volume ratio to obtain solution C, take the organic ligand 2-methylimidazole at a molar ratio of precursor cobalt salt: 2-methylimidazole = 1:8, take the sulfur source at a mass ratio of precursor cobalt salt: sulfur source = 1:0.5-2, dissolve the organic ligand 2-methylimidazole and the sulfur source in 30 mL of deionized water to obtain solution D, stir solutions C and D for 5 minutes respectively, and quickly pour solution C into solution D to obtain solution E; Step 5: Place MIL-53 / NF into solution E and stir it, control the speed to 300 r / min, and stir for 1-2 hours; let the sample stand for aging. After the reaction is completed, clean the sample and place it in a vacuum drying oven. Dry it in a vacuum at 60°C for 8 hours to finally generate the S-doped dual MOF heterostructure catalyst S-ZIF-67@MIL-53 / NF.
2. The method for preparing a sulfur-doped dual MOF heterostructure catalyst S-ZIF-67@MIL-53-NF according to claim 1, characterized in that: The size of the nickel foam is 2 cm*3 cm, and the raw materials in solvent A are 2.5 mL of deionized water, 2.5 mL of anhydrous ethanol and 35 mL of N,N-dimethylformamide.
3. The method for preparing a sulfur-doped dual MOF heterostructure catalyst S-ZIF-67@MIL-53-NF according to claim 1, characterized in that: In the reaction solution B, the concentration of iron ions is 25 mmol / L, and the molar ratio of the precursor iron salt to the organic ligand terephthalic acid is 1:3; the concentration of cobalt ions in solution E is 25 mmol / L, and the molar ratio of the precursor cobalt salt to 2-methylimidazole in solution E is 1:
8.
4. The method for preparing a sulfur-doped dual MOF heterostructure catalyst S-ZIF-67@MIL-53-NF according to claim 1, characterized in that: The precursor iron salt is ferric nitrate nonahydrate; the precursor cobalt salt is cobalt nitrate hexahydrate.
5. The method for preparing a sulfur-doped dual MOF heterostructure catalyst S-ZIF-67@MIL-53-NF according to claim 1, characterized in that: The sulfur source is sodium thiosulfate pentahydrate and / or thiourea.
6. The method for preparing a sulfur-doped dual MOF heterostructure catalyst S-ZIF-67@MIL-53-NF according to claim 1, characterized in that: The static aging reaction temperature in the fifth step is room temperature, and the reaction time is 1-3 hours.
7. The method for preparing a sulfur-doped dual MOF heterostructure catalyst S-ZIF-67@MIL-53-NF according to claim 1, characterized in that: The solvents for cleaning the samples in the third step are N,N-dimethylformamide, anhydrous ethanol and deionized water in sequence, and the amount of each cleaning agent is 15-30 mL.
8. The method for preparing a sulfur-doped dual MOF heterostructure catalyst S-ZIF-67@MIL-53-NF according to claim 1, characterized in that: The solvent for cleaning the sample in the fifth step is ethanol.
Citation Information
Cited By
Oxygen-deficient iron / tin heterojunction nano electro-catalytic material as well as preparation method and application of oxygen-deficient iron / tin heterojunction nano electro-catalytic material
CN120272970A
Difunctional electro-catalytic water decomposition material as well as preparation and application thereof
CN120666390A
ZIFs / polyaniline multilevel structure composite material as well as preparation method and application thereof
CN121853044A