Coupling current electrolysis method for manganese electrodeposition

By combining the coupled current electrolysis method of DC and chaotic circuits, the problems of high energy consumption and concentration polarization in traditional manganese electrolysis are solved, and more efficient and denser manganese electrodeposition is achieved, thereby improving electrolytic efficiency and product quality.

CN118932424AActive Publication Date: 2024-11-12CHONGQING UNIV +1

Patent Information

Application Number
CN202411096875.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-12
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

In traditional electrolytic manganese processes, there are problems such as high tank pressure, high electrolytic energy consumption and low product quality. It is mainly due to the single concentration polarization and current amplitude changes caused by DC electrodeposition, so it is impossible to effectively couple the electrolytic process.

Method used

The coupled current electrolysis method is adopted to provide continuous, nonlinear, adjustable current power supply through the combination of DC circuit and chaotic circuit, and adjust the current ratio of DC and chaotic circuits to change the current amplitude and achieve efficient electrolysis of manganese electrodeposition.

Benefits of technology

The current efficiency is improved, the electrolytic energy consumption is reduced, the quality and density of manganese deposited are improved, the anode sludge is reduced, and the lead content of electrolytic products is reduced, achieving a more efficient manganese electrolysis process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932424A_ABST
    Figure CN118932424A_ABST
Patent Text Reader

Abstract

The invention discloses a coupling current electrolysis method for manganese electrodeposition. The method comprises the following steps: (1) adding a manganese sulfate solution system into an electrolytic bath; (2) switching on a coupling current source for electrolysis; the coupling current source comprises a direct-current circuit and a chaotic circuit, the anode of the direct-current circuit and the anode of the chaotic circuit are connected with the anode of the electrolytic bath, and the cathode of the direct-current circuit and the cathode of the chaotic circuit are connected with the cathode of the electrolytic bath. The current output by the coupling current source continuously and periodically changes in time, the current amplitude is adjustable, the coupling electrolysis operation mode is simple, the current efficiency is high, the electrolysis energy consumption is low, meanwhile, the electrodeposition effect is improved, the lead content in an electrolysis product is reduced, nucleation of manganese is facilitated, uniform and compact deposition of manganese is achieved, and the service life of the device is prolonged. The quality of a manganese product is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of electrolytic manganese technology, and in particular to a coupled current electrolytic method for manganese electrodeposition. Background Art

[0002] Manganese is one of the important metals, widely used in steel smelting, alloys, new energy and other industries, and is an indispensable raw material for basic industries. At present, the traditional electrolytic manganese industry is powered by a DC power supply. In the DC electrodeposition process, the obtained Mn deposition layer is loose and porous, and the density is weak. In addition, the manganese reduction potential is too negative during the electrodeposition process, which causes the problem of high cell pressure and high electrolysis energy consumption. The DC power consumption per ton of manganese is 5800-6200kW·h, while the electrolysis efficiency is only 65%-74%. Under DC electrolysis, due to serious concentration polarization problems, high cell pressure and high electrolysis energy consumption will occur, resulting in reduced quality of manganese products. Some researchers have regulated the electrolysis of metallic manganese by changing the power supply to pulse current electrolysis. The results show that pulse current electrolysis has a certain effect of energy saving and improving the quality of manganese deposition, but the pulse current is continuously powered on and off, and concentration polarization still occurs during the electrodeposition process, causing cathode dendrite growth; more importantly, the single electrolysis current has a single current amplitude change, which cannot effectively couple the electrolysis process. Therefore, changing the power supply of the electrolysis process and finding an electrolysis method with adjustable current amplitude and continuous current change characteristics is expected to become a new breakthrough in achieving energy conservation and consumption reduction in the manganese metal electrolysis process. Summary of the invention

[0003] In view of this, the present invention provides a novel coupled current electrolysis method for manganese electrodeposition, which aims to achieve continuous, nonlinear, and adjustable power supply, solve the concentration polarization technical problem of manganese electrodeposition, and achieve energy saving and consumption reduction in the long-term manganese electrodeposition process, thereby improving current efficiency and improving the quality and quality of manganese deposition. In detail, the coupled current electrolysis method for manganese electrodeposition provided by the present invention comprises the following steps:

[0004] (1) adding a manganese sulfate solution system into an electrolytic cell;

[0005] (2) connecting a coupled current source to perform electrolysis;

[0006] The coupling current source includes a DC circuit and a chaotic circuit, the anode of the DC circuit and the anode of the chaotic circuit are connected to the anode of the electrolytic cell, and the cathode of the DC circuit and the cathode of the chaotic circuit are connected to the cathode of the electrolytic cell; the coupling current source is turned on by turning on the power switch of the DC circuit and the power switch of the chaotic circuit.

[0007] Preferably, the manganese sulfate solution system in step (1) is: the ammonium sulfate concentration is 120 g·L -1 , manganese ion concentration is 30g·L -1, SeO2 concentration is 30 mg·L -1 , pH value is 7.0; the average current density of the coupling current source in step (2) is 350A / m 2 .

[0008] Preferably, the magnitudes of the currents of the DC circuit and the chaotic circuit are both adjustable.

[0009] Preferably, the current ratio of the DC circuit and the chaotic circuit is 2:8 to 8:2.

[0010] Preferably, the current ratio of the DC circuit and the chaotic circuit is 4:6.

[0011] Preferably, the anode material of the electrode of the electrolytic cell is a quaternary alloy, and the cathode material is stainless steel.

[0012] Preferably, the electrolyte temperature in the electrolytic cell is 40°C.

[0013] The coupling current source in the method of the present invention provides a continuously changing current signal through a chaotic circuit, and provides an adjustable linear term through a DC circuit to increase the current value; the current amplitude (current fluctuation range) is changed by adjusting the current ratio of the DC circuit power supply and the chaotic circuit power supply, and coupling currents of different ratios are introduced to electrolyze the manganese sulfate solution system to precipitate elemental metal manganese at the cathode; the magnitude of the current output by the coupling current source changes continuously and periodically over time; the coupling currents are combined according to different ratios; the coupling currents can output a variety of current signals with different current amplitudes under the same current parameter; and the coupling currents have different current amplitudes when they are in different ratios.

[0014] Beneficial effects: The coupled current electrolysis method for manganese electrodeposition provided by the present invention is a new type of manganese electrodeposition method. The current output by the coupled current source of the present invention changes continuously and periodically over time, the current amplitude is adjustable, and the coupled electrolysis operation is simple. Under a specific coupled current ratio, the current efficiency is 4.25% higher than that of direct current, and the electrolysis energy consumption is 5.08% lower than that of direct current. The anode mud is reduced by 27.99% respectively. At the same time, the electrodeposition effect is improved, and the lead content in the electrolysis product is reduced. This is conducive to the nucleation of manganese, realizes uniform and dense deposition of manganese, and improves the quality of manganese products. At the same time, this coupled electrolysis method is not only simple to operate, but also achieves clean and efficient electrolysis effects in the actual electrolysis process, and is operational for the hydrometallurgical industry. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 It is a schematic diagram of the electrolysis process of the present invention;

[0016] Figure 2 is a circuit structure diagram of a chaotic circuit according to an embodiment of the present invention;

[0017] Figure 3 The microscopic morphology of cathode manganese deposition under different currents of the present invention;

[0018] Figure 4 The microscopic morphology of anode mud under different currents of the present invention. DETAILED DESCRIPTION

[0019] The endpoints of any range disclosed in the present invention and any value are not limited to the precise range and / or value, and these ranges and / or values ​​can and should be understood to include values ​​close to these ranges and / or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0020] Embodiment 1: Coupling current source and its connection with electrolytic cell

[0021] The coupling current source is composed of two circuits: a DC circuit and a chaotic circuit. The DC circuit outputs a DC current, and the chaotic circuit outputs a chaotic current. That is, the coupling current is obtained by coupling the DC current and the chaotic current ( Figure 1 ). The coupling current source and the method of connecting it to the electrolytic cell are as follows: the anodes of the DC circuit and the chaotic circuit are connected to a wire at the same time, named wire 1, that is, wire 1 is the anode of the coupling current source, and then wire 1 is connected to the anode of the electrolytic cell; similarly, the cathodes of the DC circuit and the chaotic circuit are connected to another wire at the same time, named wire 2, that is, wire 2 is the cathode of the coupling current source, and then wire 2 is connected to the cathode of the electrolytic cell. When the power switches of the DC circuit and the chaotic circuit are turned on, the two currents are coupled, that is, the coupling current, and the electrolytic cell is connected to the coupling current to start electrolysis.

[0022] The DC circuit of the coupled current source is: a DC current power supply that can be adjusted and generate different current magnitudes.

[0023] The chaotic circuit of the coupled current source is: a chaotic current power supply that can adjust and generate different current sizes. The circuit structure of the power supply includes a chaotic module and a current amplification module. The chaotic module generates chaotic current, and the current amplification module can amplify and adjust the size of the chaotic current.

[0024] Circuit structure of chaos module ( Figure 2 ) is: the VS+ terminal of the analog multiplier U6 is connected to the positive end of the DC power supply, and the VS- terminal is connected to the negative end of the DC power supply, and the DC power supply provides a 15V voltage signal for the circuit;

[0025] The Z terminal, X2 terminal, Y1 terminal and Y2 terminal of the analog multiplier U6 are grounded;

[0026] The X1 terminal of the analog multiplier U6 receives the signal fed back by the operational amplifier L1;

[0027] The Y1 terminal of the analog multiplier U6 receives the signal fed back by the operational amplifier L7;

[0028] The analog multiplier U6 multiplies the received signals to obtain a multiplied signal;

[0029] The W terminal of the analog multiplier U6 transmits the multiplied signal to the negative input terminal of the operational amplifier L1 through the resistor R3;

[0030] The negative input terminal of the operational amplifier L1 receives the signal fed back by the operational amplifier L2 through the resistor R1;

[0031] The negative input terminal of the operational amplifier L1 receives the signal fed back by the operational amplifier L3 through the resistor R2;

[0032] The negative input terminal of the operational amplifier L1 receives a signal fed back by the operational amplifier L4 through the resistor R4;

[0033] The positive input terminal of the operational amplifier L1 is grounded;

[0034] The output terminal of the operational amplifier L1 is connected in series with the capacitor C1 and then connected to the negative input terminal of the operational amplifier L1;

[0035] The output terminal of the operational amplifier L1 is connected in series with a resistor R13 and then connected to the negative input terminal of the operational amplifier L2;

[0036] The positive input terminal of the operational amplifier L2 is grounded;

[0037] The signal output from the output terminal of the operational amplifier L2 enters the negative input terminal of the operational amplifier L3 through the resistor R5;

[0038] The output terminal of the operational amplifier L2 is connected in series with a resistor R14 and then connected to the negative input terminal of the operational amplifier L2;

[0039] The negative input terminal of the operational amplifier L3 receives the signal fed back by the operational amplifier L3 through the resistor R6;

[0040] The positive input terminal of the operational amplifier L3 is grounded;

[0041] The output terminal of the operational amplifier L3 is connected in series with the capacitor C2 and then connected to the negative input terminal of the operational amplifier L3;

[0042] The negative input terminal of the operational amplifier L4 receives the signal fed back by the operational amplifier L2 through the resistor R7;

[0043] The positive input terminal of the operational amplifier L4 is grounded;

[0044] The output terminal of the operational amplifier L4 is connected in series with the capacitor C3 and then connected to the negative input terminal of the operational amplifier L4;

[0045] The circuit structure of the current amplifier module ( Figure 2 ) is: the Z terminal, X2 terminal, Y1 terminal and Y2 terminal of the analog multiplier U7 are grounded;

[0046] The X1 terminal of the analog multiplier U7 receives the signal fed back by the operational amplifier L2;

[0047] The Y1 terminal of the analog multiplier U7 receives the signal fed back by the operational amplifier L1;

[0048] The VS+ terminal of the analog multiplier U7 is connected to the positive end of the DC power supply, and the VS- terminal is connected to the negative end of the DC power supply;

[0049] The analog multiplier U7 multiplies the received signals to obtain a multiplied signal;

[0050] The W terminal of the analog multiplier U7 transmits the multiplied signal to the negative input terminal of the operational amplifier L5 through the resistor R9;

[0051] The negative input terminal of the operational amplifier L5 receives the electrical signal flowing through the resistor R16 through the resistor R17;

[0052] The negative input terminal of the operational amplifier L5 is connected in series with a capacitor C4 and then connected to the output terminal of the operational amplifier L5;

[0053] The positive input terminal of the operational amplifier L5 is grounded;

[0054] The output terminal of the operational amplifier L5 is connected to the negative input terminal of the operational amplifier L6 through the resistor R16;

[0055] The negative input terminal of the operational amplifier L6 is connected in series with a resistor R15 and then connected to the anode of the diode D3;

[0056] The positive input terminal of the operational amplifier L6 is grounded;

[0057] The output terminal of the operational amplifier L6 is connected in series with the cathode of the diode D3;

[0058] The anode of the diode D3 is connected in series with the resistor R11 and the resistor R10 in sequence and then connected to the output end of the operational amplifier L7;

[0059] The anode of the diode D3 is connected in series with the resistor R11 and then connected to the negative input terminal of the operational amplifier L7;

[0060] The negative end of the power source V1 is grounded, and the positive end is connected in series with a resistor R12 and then connected to the negative input terminal of the operational amplifier L7;

[0061] The positive input terminal of the operational amplifier L7 is grounded;

[0062] The component parameters in the above circuit structure are as follows: C1=C2=C3=C4=10nF, R1=R2=22.22kΩ, R3=R10=R12=R13=R14=R15=R16=10kΩ, R4=100kΩ, R5=R6=18.18kΩ, R7=500kΩ, sliding resistor R9=(0-10)kΩ, sliding resistor R11=(0-2.5)kΩ, power supply V1=4.5V.

[0063] The chaotic current power supply can be adjusted to generate different current magnitudes by adjusting the resistance values ​​of the sliding resistors R9 and R11 in the circuit amplification module.

[0064] Next, the coupling current source is used in a specific electrolysis experiment (see Examples 1-4 in the second embodiment below), and the DC circuit and the chaotic circuit constituting the coupling current source are also used as comparative examples for electrolysis experiments (see Comparative Examples 1-2 in the second embodiment below):

[0065] Implementation Method II: Examples and Comparative Examples Methods and Results Analysis

[0066] Embodiment 1:

[0067] 1) coupling a current source to supply power to the manganese electrolysis system;

[0068] 2) Add manganese sulfate solution to the electrolytic cell. The manganese sulfate solution system is ammonium sulfate with a concentration of 120 g·L -1 , manganese ion concentration is 30g·L -1 , SeO2 concentration is 30 mg·L -1 , pH value is about 7.0, the anode material of the electrode in the electrolytic cell is a quaternary alloy, and the cathode material is stainless steel; according to the current density of 350A / m 2 (total current 0.78A), adjust the current size output by the DC circuit and the chaotic circuit, set the DC current to 0.624A and the chaotic current to 0.156A according to the coupling current ratio of DC: chaotic current = 8:2, and the coupling current amplitude is 0.01A at this time; turn on the coupling current source, electrolyze the manganese sulfate solution, and precipitate elemental metallic manganese at the cathode.

[0069] Embodiment 2:

[0070] 1) coupling a current source to supply power to the manganese electrolysis system;

[0071] 2) Add manganese sulfate solution to the electrolytic cell. The manganese sulfate solution system is ammonium sulfate with a concentration of 120 g·L -1 , manganese ion concentration is 30g·L -1, SeO2 concentration is 30 mg·L -1 , pH value is about 7.0, the anode material of the electrode in the electrolytic cell is a quaternary alloy, and the cathode material is stainless steel; according to the current density of 350A / m 2 (total current 0.78A), adjust the current size output by the DC circuit and the chaotic circuit, set the DC current to 0.468A and the chaotic current to 0.312A according to the coupling current ratio of DC: chaotic current = 6:4, and the coupling current amplitude is 0.014A at this time; turn on the coupling current source, electrolyze the manganese sulfate solution, and precipitate elemental metallic manganese at the cathode.

[0072] Embodiment 3:

[0073] 1) coupling a current source to supply power to the manganese electrolysis system;

[0074] 2) Add manganese sulfate solution to the electrolytic cell. The manganese sulfate solution system is ammonium sulfate with a concentration of 120 g·L -1 , manganese ion concentration is 30g·L -1 , SeO2 concentration is 30 mg·L -1 , pH value is about 7.0, the anode material of the electrode in the electrolytic cell is a quaternary alloy, and the cathode material is stainless steel; according to the current density of 350A / m 2 (total current 0.78A), adjust the current size output by the DC circuit and the chaotic circuit, set the DC current to 0.312A and the chaotic current to 0.468A according to the coupling current ratio of DC: chaotic current = 4:6, and the coupling current amplitude is 0.017A at this time; turn on the coupling current source, electrolyze the manganese sulfate solution, and precipitate elemental metallic manganese at the cathode.

[0075] Embodiment 4:

[0076] 1) coupling a current source to supply power to the manganese electrolysis system;

[0077] 2) Add manganese sulfate solution to the electrolytic cell. The manganese sulfate solution system is ammonium sulfate with a concentration of 120 g·L -1 , manganese ion concentration is 30g·L -1 , SeO2 concentration is 30 mg·L -1 , pH value is about 7.0, the anode material of the electrode in the electrolytic cell is a quaternary alloy, and the cathode material is stainless steel; according to the current density of 350A / m 2 (total current 0.78A), adjust the current size output by the DC circuit and the chaotic circuit, set the DC current to 0.156A and the chaotic current to 0.628A according to the coupling current ratio of DC: chaotic current = 2:8, and the coupling current amplitude is 0.024A at this time; turn on the coupling current source, electrolyze the manganese sulfate solution, and precipitate elemental metallic manganese at the cathode.

[0078] Comparative Example 1:

[0079] 1) Only the DC circuit supplies power to the manganese electrolysis system;

[0080] 2) Add manganese sulfate solution to the electrolytic cell. The manganese sulfate solution system is ammonium sulfate with a concentration of 120 g·L -1 , manganese ion concentration is 30g·L -1 , SeO2 concentration is 30 mg·L -1 , pH value is about 7.0, the anode material of the electrode in the electrolytic cell is a quaternary alloy, and the cathode material is stainless steel; according to the current density of 350A / m 2 (total current 0.78A), adjust the DC current and set the DC current to 0.78A; turn on the power of the DC circuit, electrolyze the manganese sulfate solution, and precipitate elemental metallic manganese at the cathode.

[0081] Comparative Example 2:

[0082] 1) Only the chaotic circuit supplies power to the manganese electrolysis system;

[0083] 2) Add manganese sulfate solution to the electrolytic cell. The manganese sulfate solution system is ammonium sulfate with a concentration of 120 g·L -1 , manganese ion concentration is 30g·L -1 , SeO2 concentration is 30 mg·L -1 , pH value is about 7.0, the electrode is placed in the electrolytic cell, the anode material of the electrode is quaternary alloy, and the cathode material is stainless steel; according to the current density of 350A / m 2 (total current 0.78A), adjust the chaotic current, set the chaotic current to 0.78A, and the current amplitude is 0.036A; turn on the power of the chaotic circuit, electrolyze the manganese sulfate solution, and precipitate elemental metallic manganese at the cathode.

[0084] Results and comparative analysis

[0085] The weight of cathode manganese precipitation and the weight of anode mud are obtained by using the difference in the mass of the dry electrode before and after electrolysis, and the electrode voltage U during the electrolysis process is collected, and the current efficiency CE is calculated according to formula (1), and the electrolysis energy consumption EC is calculated according to formula (2), where q is the electrochemical equivalent of metallic manganese. The current efficiency and electrolysis energy consumption are used to evaluate the electrolysis performance and energy consumption during the electrolysis of manganese. The electrolysis experiment was carried out under the same conditions, and a coupled current source was used as a manganese electrolysis power source to output nonlinear currents of different currents. The current efficiency CE, electrolysis energy consumption EC, and anode mud generation are shown in Table 1. Under the single direct current electrolysis of Comparative Example 1, the current efficiency is 82.29%; under the single chaotic electrolysis of Comparative Example 2, the current efficiency is 83.25%. As can be seen from Table 1, after coupling the direct current and chaotic currents, the coupled currents at any ratio achieve better electrolysis effects. For example, when DC: chaotic current = 8:2, the current efficiency is 84.20%, which is 1.91% higher than DC; when DC: chaotic current = 2:8, the current efficiency is 85.55%, which is 3.26% higher than DC; and the best electrolysis effect is obtained when the coupling current ratio DC: chaotic current = 4:6, the current efficiency is 4.25% higher than DC, the electrolysis energy consumption is 5.08% lower than DC, and the anode mud is reduced by 27.99%, which has the most efficient energy-saving effect. Analysis of electrolysis products ( Figure 3 This is the microscopic morphology of cathode manganese deposition. Figure 4 The microscopic morphology of anode mud, where (a) represents direct current electrolysis, (b) represents coupled current electrolysis with direct current: chaotic current = 4:6, and (c) represents chaotic current electrolysis): Figure 3 As shown in (a), under direct current electrolysis, the surface of the cathode manganese deposit is uneven and the manganese dendrite particles are densely distributed. With the introduction of chaotic current, the cathode interface concentration polarization is improved and the cathode fractal growth is inhibited, and the resulting manganese coating is smoother and denser ( Figure 3 (b)). Figure 4 As shown in the figure, compared with direct current electrolysis, the anode mud deposits are denser, the anode corrosion resistance is stronger, and the anode pollution is suppressed under the coupled current. The coupled current has the effect of chaotic current regulating the growth of cathode dendrites and anode mud, while improving the energy-saving electrolysis effect of the manganese electrolysis process, and can achieve efficient production of the manganese electrolysis process. It has efficient and clean electrolysis capabilities and has great application prospects in the field of hydrometallurgy.

[0086] CE=m / (q·I·t) (1)

[0087] EC = U·1000 / (q·CE) (2)

[0088] Table 1 Electrolysis parameters and effects of different current types

[0089]

[0090] Conventional techniques in the above-described embodiments and schemes not described in detail are all well known in the art, so they are not described in detail here. The above embodiments and / or experimental examples describe the preferred embodiments of the present invention in detail, but the present invention is not limited to the specific details in the above-described embodiments. Within the technical concept of the present invention, the technical scheme of the present invention can be subjected to a variety of simple modifications, and these simple modifications all belong to the protection scope of the present invention. It should be noted that each specific technical feature described in the above-described specific embodiments can be combined in any suitable manner when there is no contradiction. In order to avoid unnecessary repetition, the present invention will not be described separately for various possible combinations. In addition, any combination can also be carried out between the various different embodiments of the present invention, as long as it does not violate the idea of ​​the present invention, it should also be regarded as the content disclosed by the present invention.

Claims

1. A coupled current electrolytic method for manganese electrodeposition, characterized in that: The following steps are involved: (1) adding a manganese sulfate solution system into an electrolytic cell; (2) connecting a coupled current source to perform electrolysis; The coupling current source includes a DC circuit and a chaotic circuit, the anode of the DC circuit and the anode of the chaotic circuit are connected to the anode of the electrolytic cell, and the cathode of the DC circuit and the cathode of the chaotic circuit are connected to the cathode of the electrolytic cell; the coupling current source is turned on by turning on the power switch of the DC circuit and the power switch of the chaotic circuit.

2. The method according to claim 1, characterized in that The manganese sulfate solution system in step (1) is: the concentration of ammonium sulfate is 120g·L -1 , manganese ion concentration is 30g·L -1 , SeO2 concentration is 30 mg·L -1 , pH value is 7.0; the average current density of the coupling current source in step (2) is 350A / m 2 .

3. The method according to claim 1 or 2, characterized in that The magnitudes of the currents of the DC circuit and the chaotic circuit can be adjusted.

4. The method according to any one of claims 1 to 3, characterized in that: The current ratio between the DC circuit and the chaotic circuit is 2:8 to 8:

2.

5. The method according to claim 4, characterized in that The current ratio of the DC circuit to the chaotic circuit is 4:

6.

6. The method according to any one of claims 1 to 4, characterized in that: The anode material of the electrode of the electrolytic cell is a quaternary alloy, and the cathode material is stainless steel.

7. The method according to any one of claims 1 to 5, characterized in that: The electrolyte temperature in the electrolytic cell is 40°C.

Citation Information

Patent Citations

  • Amplitude-adjustable chaotic signal source

    CN105871535A

  • Energy-saving process in electrolytic manganese electrolysis procedure

    CN106119891A

  • Nonlinear current electrolysis method for manganese electrodeposition and application

    CN117822050A

  • Novel adjustable hyperchaotic circuit system and application thereof in electrolysis

    CN118399896A

Cited By

  • Nonlinear current treatment method for ammonia nitrogen electrochemical oxidation of high-salt pharmaceutical wastewater

    CN121107539A