Single-crystal molecular ferroelectric and preparation and application thereof
By introducing single-crystal molecular ferroelectric bodies with SbI6 octahedral zigzag chains with shared edges and corners and independent organic molecules into traditional ferroelectric materials, the high-temperature sintering and rare earth metal dependence are solved by hydrothermal reaction and low-temperature preparation. The problem of this paper has achieved efficient and low-cost ferroelectric material preparation, and is suitable for the fields of photoelectric thin film devices and other fields.
Patent Information
- Application Number
- CN202411011808.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-12
AI Technical Summary
Traditional inorganic oxide ferroelectric materials have problems such as high energy consumption, waste of resources, environmental pollution and rare earth metal dependence in preparation and application, and are poor in applicability in flexible electronic devices and fine process control.
A single crystal molecular ferroelectric material consisting of SbI6 octahedral zigzag chain with shared edges and corners and independent organic molecules is prepared through hydrothermal reactions to achieve low temperature preparation of high-efficiency ferroelectric materials, reducing costs and improving the electrical properties of the materials.
It realizes the low-cost and efficient preparation of single-crystal molecular ferroelectrics, which is suitable for large-scale production, improves the electrical performance and sustainability of materials, and is suitable for fields such as photoelectric thin film devices.
Smart Images

Figure CN118932493A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of optoelectronic technology, and in particular to a single crystal molecular ferroelectric and its preparation and application. Background Art
[0002] Ferroelectric materials are a class of materials with spontaneous polarization that is easily regulated by temperature changes, electric field changes, and mechanical stress changes. Due to the breaking of central symmetry, ferroelectric materials have very excellent dielectric, piezoelectric, pyroelectric, and electro-optical properties, and can play an important role in data storage, energy collection (capacitors, etc.), sensing, integrated optoelectronic devices, and other fields. At present, although inorganic oxide ferroelectric materials such as PbTiO 3 and BaTiO 3 Although it has excellent ferroelectric properties, there are still some significant problems to be solved in its preparation and application. 3 Ferroelectrics usually require high-temperature sintering to obtain the desired crystal structure and properties, which is not only energy-intensive but also may lead to resource waste and environmental pollution. Secondly, many materials contain expensive rare earth metals, which increase costs and pose challenges to resource recycling, and their mining and processing also have environmental impacts. In addition, due to their rigid structure and composition limitations, these materials are less suitable for flexible electronic devices and fine process control.
[0003] Therefore, future research and development directions need to be committed to solving these problems: developing low-temperature preparation of efficient ferroelectric materials, reducing dependence on rare earth metals, improving material sustainability and environmental protection, and exploring new structural designs to meet the needs of electronic devices. Summary of the invention
[0004] In order to solve the above problems, the purpose of the present invention is to provide a single crystal molecular ferroelectric and its preparation and application. The single crystal molecular ferroelectric of the present invention is composed of SbI with corner sharing. 6 Octahedral zigzag chains and independent organic molecules. SbI 6 The octahedron is slightly distorted in the coordination environment. This structural design makes the charge centers of positive ions and anions non-overlapping, resulting in the spontaneous polarization of the material. Compared with the traditional ferroelectric organic molecular structure, this structural design shows a more complex and precise charge distribution, improves the electrical properties of the material, and the preparation method is simple and cost-effective, suitable for large-scale production.
[0005] The purpose of the present invention can be achieved by the following technical solutions:
[0006] The first object of the present invention is to provide a single crystal molecular ferroelectric material, the chemical formula of which is [C 8 N 4 H 28 ][Sb2 I 10 ].
[0007] A second object of the present invention is to provide a method for preparing a single crystal molecular ferroelectric material, comprising the following steps:
[0008] (S1) Sb 2 O 3 Mix with solvent to obtain SbI 3 Solution;
[0009] (S2) adding 1,4-diaminobutane to the SbI obtained in step (S1) 3 In solution, single crystal molecular ferroelectric material is obtained by post-treatment after hydrothermal reaction;
[0010] The solvent is HI.
[0011] In one embodiment of the present invention, in step (S1), Sb 2 O 3 The dosage ratio to the solvent is 1mmol:2~5mL.
[0012] In one embodiment of the present invention, in step (S2), Sb 2 O 3 The molar ratio of 1,4-diaminobutane is 1:1-2;
[0013] During the hydrothermal reaction, the temperature is 120-180°C and the time is 12-72 hours.
[0014] In one embodiment of the present invention, in step (S2), the post-treatment is washing and drying in sequence;
[0015] During the washing process, the detergent is ethyl acetate; during the drying process, the temperature is 60°C.
[0016] The third object of the present invention is to provide an application of a single crystal molecular ferroelectric material in the preparation of a back electrode for a photoelectric thin film device.
[0017] The fourth object of the present invention is to provide a back electrode for a photoelectric thin film device, wherein the back electrode for a photoelectric thin film device is made of a single crystal molecular ferroelectric material.
[0018] A fifth object of the present invention is to provide a method for preparing a back electrode for a photovoltaic thin film device, comprising the following steps:
[0019] (A1) mixing a single crystal molecular ferroelectric material and N,N-dimethylformamide to obtain a mixed solution;
[0020] (A2) spin coating the mixed solution prepared in step (A1) on a conductive substrate, and performing vacuum annealing to obtain a molecular ferroelectric thin film;
[0021] (A3) The molecular ferroelectric film prepared in step (A2) is used as a back electrode for a photoelectric thin film device by screen printing silver paste.
[0022] In one embodiment of the present invention, in step (A1), the ratio of the single crystal molecular ferroelectric material to N,N-dimethylformamide is 3 g: 1-2 mL.
[0023] In one embodiment of the present invention, in step (A2), the conductive substrate is glass, and before use, the glass is thoroughly cleaned with detergent, and then ultrasonically cleaned with acetone, alcohol, and deionized water for 15 minutes in sequence, and then the cleaned glass is placed in an oven for drying.
[0024] During the spin coating process, a glue spreader is used, and its process parameters are: rotation speed 1000-3000 rpm / min, spin coating times 2-5 times, spin coating volume 40-60 μL / time, spin coating time 10-30 s / time;
[0025] During the vacuum annealing treatment, the temperature is raised to 100-150°C at a rate of 1-2°C / min for 1-3 hours, and then cooled to room temperature under vacuum;
[0026] The thickness of the molecular ferroelectric thin film obtained by spin coating the mixed solution is 2.73-5.76 μm (preferably, the thickness is 3.68 μm).
[0027] A sixth object of the present invention is to provide an application of a back electrode for a photovoltaic thin film device in the preparation of a photovoltaic thin film device.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] The single crystal molecular ferroelectric material preparation method of the present invention is simple, low-cost and easy to operate; the [C 8 N 4 H 28 ][Sb 2 I 10 ]Molecular ferroelectric materials are of high purity and are suitable for preparing high-quality thin films, especially by spin coating, which can produce thin films with regular structure and excellent quality. These characteristics make the material have broad application prospects in many fields such as optoelectronic devices, biomedicine and information storage, especially in solar cells and photodetectors. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1The single crystal molecular ferroelectric material prepared in Example 1 [C 8 N 4 H 28 ][Sb 2 I 10 ]’s XRD pattern;
[0031] Figure 2 The single crystal molecular ferroelectric material prepared in Example 1 [C 8 N 4 H 28 ][Sb 2 I 10 ] structure diagram (I);
[0032] Figure 3 The single crystal molecular ferroelectric material prepared in Example 1 [C 8 N 4 H 28 ][Sb 2 I 10 ] structure diagram (II);
[0033] Figure 4 The single crystal molecular ferroelectric material prepared in Example 1 [C 8 N 4 H 28 ][Sb 2 I 10 ] optical photographs;
[0034] Figure 5 The single crystal molecular ferroelectric material prepared in Example 1 [C 8 N 4 H 28 ][Sb 2 I 10 ]’s absorption-bandgap diagram;
[0035] Figure 6 For Example 5 [C 8 N 4 H 28 ][Sb 2 I 10 ]PE diagram of photovoltaic film;
[0036] Figure 7 For Example 5 [C 8 N 4 H 28 ][Sb 2 I 10 ]IT curve of photoelectric thin film materials at different polarization voltages. DETAILED DESCRIPTION
[0037] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0038] In the following examples, unless otherwise specified, all reagents used are commercially available reagents, and all detection means and methods used are conventional detection means and methods in the art.
[0039] Example 1
[0040] This embodiment provides a hydrothermal synthesis method of a single crystal molecular ferroelectric material, which specifically includes the following steps:
[0041] (S1) 5 mmol of Sb 2 O 3 Add the powder to 25 ml HI and mix well to obtain SbI 3 Solution;
[0042] (S2) Add 5 mmol of 1,4-diaminobutane to the SbI obtained in step (S1) 3 The solution is stirred and mixed to obtain a mixed solution;
[0043] (S3) transferring the mixture prepared in step (S2) into a reactor with a filling degree of less than 70%, reacting in an oven at 120° C. for 12 hours, cooling the reactor to room temperature, and releasing the pressure; washing the product with ethyl acetate several times, and ultrasonically treating it in an ultrasonic oscillator, skimming off the supernatant, leaving a red precipitate at the bottom, obtaining a sample, and drying the obtained sample in an oven at 60° C. to finally obtain a single crystal molecular ferroelectric material [C 8 N 4 H 28 ][Sb 2 I 10 ](Powder form).
[0044] Performance Test:
[0045] The X-ray diffractometer was used to detect the 8 N 4 H 28 ][Sb 2 I 10 ]Single crystal powder, its XRD pattern is as follows Figure 1 As shown, it can be seen that the obtained samples are all pure phases.
[0046] Using graphite monochromatized Mo Kα radiation The single crystal X-ray diffraction (XRD) was collected on the diffractometer using the ω-2θ scanning method, and the structure diagram is shown in Figures 2-3 As shown, according to the RT single crystal XRD data, the material has a polar orthorhombic structure of Pn space group, and the crystal structure consists of one-dimensional (1D) angle sharing Sbl 6 The octahedral zigzag structure is composed of chains along the b-axis and independent 1,4-diaminobutane molecules.
[0047] Table 1[C 8 N 4 H 28 ][Sb 2 I 10 ]Unit cell parameters of molecular ferroelectric single crystals
[0048]
[0049]
[0050] The single crystal molecular ferroelectric material [C 8 N 4 H 28 ][Sb 2 I 10 ], such as Figure 4 The material was found to be dark red rod-shaped with a smooth surface and no defects.
[0051] UV-Vis-NIR spectrophotometer was used to measure [C 8 N 4 H 28 ][Sb 2 I 10 ] single crystal absorption and band gap, such as Figure 5 As shown, it shows that the single crystal molecular ferroelectric material [C 8 N 4 H 28 ][Sb 2 I 10 ] has an absorption edge at 699nm and an optical band gap of 1.89eV.
[0052] Example 2
[0053] This embodiment provides a hydrothermal synthesis method of a single crystal molecular ferroelectric material, which specifically includes the following steps:
[0054] (S1) 5 mmol of Sb 2 O 3 Add the powder to 25 ml HI and mix well to obtain SbI 3 Solution;
[0055] (S2) Add 5 mmol of 1,4-diaminobutane to the SbI obtained in step (S1) 3 The solution is stirred and mixed to obtain a mixed solution;
[0056] (S3) transferring the mixture prepared in step (S2) into a reactor with a filling degree of less than 70%, reacting in an oven at 160° C. for 12 hours, cooling the reactor to room temperature, and releasing the pressure; washing the product with ethyl acetate several times, and ultrasonically treating it in an ultrasonic oscillator, skimming off the supernatant, leaving a red precipitate at the bottom, obtaining a sample, and drying the obtained sample in an oven at 60° C. to finally obtain a single crystal molecular ferroelectric material [C 8 N 4 H 28 ][Sb 2 I 10 ].
[0057] Example 3
[0058] This embodiment provides a hydrothermal synthesis method of a single crystal molecular ferroelectric material, which specifically includes the following steps:
[0059] (S1) 5 mmol of Sb 2 O 3 Add the powder to 25 ml HI and mix well to obtain SbI 3 Solution;
[0060] (S2) Add 5 mmol of 1,4-diaminobutane to the SbI obtained in step (S1) 3 The solution is stirred and mixed to obtain a mixed solution;
[0061] (S3) transferring the mixture prepared in step (S2) into a reactor with a filling degree of less than 70%, reacting in an oven at 120° C. for 24 hours, cooling the reactor to room temperature, and releasing the pressure; washing the product with ethyl acetate several times, and ultrasonically treating it in an ultrasonic oscillator, skimming off the supernatant, leaving a red precipitate at the bottom, obtaining a sample, and drying the obtained sample in an oven at 60° C. to finally obtain a single crystal molecular ferroelectric material [C 8 N 4 H 28 ][Sb 2 I 10 ].
[0062] Example 4
[0063] This embodiment provides a hydrothermal synthesis method of a single crystal molecular ferroelectric material, which specifically includes the following steps:
[0064] (S1) 5 mmol of Sb 2 O 3 Add the powder to 25 ml HI and mix well to obtain SbI 3 Solution;
[0065] (S2) Add 5 mmol of 1,4-diaminobutane to the SbI obtained in step (S1)3 The solution is stirred and mixed to obtain a mixed solution;
[0066] (S3) transferring the mixture prepared in step (S2) into a reactor with a filling degree of less than 70%, reacting in an oven at 120° C. for 48 hours, cooling the reactor to room temperature, and releasing the pressure; washing the product with ethyl acetate several times, and ultrasonically treating it in an ultrasonic oscillator, skimming off the supernatant, leaving a red precipitate at the bottom, obtaining a sample, and drying the obtained sample in an oven at 60° C. to finally obtain a single crystal molecular ferroelectric material [C 8 N 4 H 28 ][Sb 2 I 10 ].
[0067] Example 5
[0068] This embodiment provides a method for preparing a molecular ferroelectric photoelectric thin film device, which specifically includes the following steps:
[0069] (A1) 0.3 g of the single crystal molecular ferroelectric material [C 8 N 4 H 28 ][Sb 2 I 10 ] powder was dissolved into 0.15 mL of DMF solution and stirred thoroughly to make [C 8 N 4 H 28 ][Sb 2 I 10 ]The single crystal powder is completely dissolved to obtain a mixed solution;
[0070] (A2) Take 60 μL of the mixed solution obtained in step (A1) and spin coat it on an ITO conductive substrate (1*1 cm 2 ) was formed on the surface of the substrate, the spin coating amount was 60 μL, the speed of the coating machine was set to 3000 rpm, the spin coating time was 30 s, and the spin coating was performed 4 times to obtain the spin coating sample; the obtained spin coating sample was placed in a tube furnace, heated to 120°C at a rate of 1°C / min, and vacuum calcined for 0.5 h; cooled to room temperature under vacuum to obtain [C 8 N 4 H 28 ][Sb 2 I 10 ] Photoelectric thin films;
[0071] The oscilloscope was used to record the 8 N 4 H 28 ][Sb 2 I 10 ]PE curve of photoelectric film, such as Figure 6As shown, it is found that the PE ring is tilted and the saturation polarization is small, indicating that the ferroelectricity of the sample is weak and the leakage is large.
[0072] (A3) the [C 8 N 4 H 28 ][Sb 2 I 10 ] photoelectric film by screen printing silver paste as the back electrode, and then the ITO conductive substrate is placed above the back electrode, and the Ag electrode is placed below the back electrode to obtain the molecular ferroelectric ([C 8 N 4 H 28 ][Sb 2 I 10 ]) Photoelectric thin film devices.
[0073] Using Keithley 2450 as the source meter, under a xenon lamp with a power of 500W (AM 1.5G), the ITO / [C 8 N 4 H 28 ][Sb 2 I 10 ] The photoelectric response of the device under zero bias voltage. When the voltage is applied, the current will change. The overall photocurrent increases first and then decreases with the increase of polarization voltage. When negatively polarized, the peak value at -7V is 18.52μA / / cm 2 , when positively polarized, at 6V, the maximum reaches -0.85μA / / cm 2 Therefore, the best photocurrent is obtained under -8V condition ( Figure 7 ).
[0074] Comparative Example 1
[0075] The difference between this comparison and implementation case 1 is that the hydrothermal temperature is different.
[0076] (S1) 5 mmol of Sb 2 O 3 Add the powder to 25 ml HI and mix well to obtain SbI 3 Solution;
[0077] (S2) Add 5 mmol of 1,4-diaminobutane to the SbI obtained in step (S1) 3 The solution is stirred and mixed to obtain a mixed solution;
[0078] (S3) transferring the mixture prepared in step (S2) into a reactor with a filling degree of less than 70%, reacting in an oven at 200° C. for 12 hours, cooling the reactor to room temperature, and releasing the pressure; washing the product with ethyl acetate several times, and ultrasonically treating it in an ultrasonic oscillator, skimming off the supernatant, leaving a red precipitate at the bottom, obtaining a sample, and drying the obtained sample in an oven at 60° C. to finally obtain a single crystal molecular ferroelectric material [C 8 N 4 H 28 ][Sb 2 I 10 ]. It was found that the crystals had irregular morphology and defects because at high temperatures, the diffusion rate of solute molecules in the solution increased, causing the solute to deposit unevenly on the crystal surface or form granular substances, thus affecting the morphology and quality of the crystals.
[0079] Comparative Example 2
[0080] The difference between this comparison and implementation case 1 is that the hydrothermal time is different.
[0081] (S1) 5 mmol of Sb 2 O 3 Add the powder to 25 ml HI and mix well to obtain SbI 3 Solution;
[0082] (S2) Add 5 mmol of 1,4-diaminobutane to the SbI obtained in step (S1) 3 The solution is stirred and mixed to obtain a mixed solution;
[0083] (S3) transferring the mixture prepared in step (S2) into a reactor with a filling degree of less than 70%, reacting in an oven at 120° C. for 6 hours, cooling the reactor to room temperature, and releasing the pressure; washing the product with ethyl acetate several times, and ultrasonically treating it in an ultrasonic oscillator, skimming off the supernatant, leaving a red precipitate at the bottom, obtaining a sample, and drying the obtained sample in an oven at 60° C. to finally obtain a single crystal molecular ferroelectric material [C 8 N 4 H 28 ][Sb 2 I 10 ]. It was found that the product contained impurities and had an uneven surface because the reactants did not have enough time to undergo a full conversion, and unreacted raw materials or impurities may remain in the crystals, reducing the purity of the crystals.
[0084] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the explanation of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A single crystal molecular ferroelectric material, characterized in that: Its chemical formula is [C8N4H 28 ][Sb2I 10 ], and its unit cell parameters are and α=90°, β=94.931(11)°, γ=90°.
2. A method for preparing a single crystal molecular ferroelectric material as claimed in claim 1, characterized in that: The following steps are involved: (S1) Sb2O3 and HI are mixed to obtain a SbI3 solution; (S2) adding 1,4-diaminobutane to the SbI3 solution obtained in step (S1), and performing post-treatment after hydrothermal reaction to obtain a single crystal molecular ferroelectric material.
3. The method for preparing a single crystal molecular ferroelectric material according to claim 2, characterized in that: In step (S1), the usage ratio of Sb2O3 to HI is 1 mmol: 2-5 mL.
4. The method for preparing a single crystal molecular ferroelectric material according to claim 2, characterized in that: In step (S2), the molar ratio of Sb2O3 to 1,4-diaminobutane is 1:1-2; During the hydrothermal reaction, the temperature is 120-180°C and the time is 12-72 hours.
5. Use of the single crystal molecular ferroelectric material as claimed in claim 1 in preparing a back electrode for a photoelectric thin film device.
6. A back electrode for a photoelectric thin film device, characterized in that: The back electrode for the photoelectric thin film device is prepared from the single crystal molecular ferroelectric material according to claim 1.
7. A method for preparing a back electrode for a photovoltaic thin film device as claimed in claim 6, characterized in that: The following steps are involved: (A1) mixing the single crystal molecular ferroelectric material according to claim 1 with N,N-dimethylformamide to obtain a mixed solution; (A2) spin coating the mixed solution prepared in step (A1) on a conductive substrate, and performing vacuum annealing to obtain a molecular ferroelectric thin film; (A3) The molecular ferroelectric film prepared in step (A2) is used as a back electrode for a photoelectric thin film device by screen printing silver paste.
8. The method for preparing a back electrode for a photoelectric thin film device according to claim 7, characterized in that: In step (A1), the ratio of the single crystal molecular ferroelectric material to N,N-dimethylformamide is 3 g: 1-2 mL.
9. The method for preparing a back electrode for a photoelectric thin film device according to claim 7, characterized in that: In step (A2), during the vacuum annealing treatment, the temperature is 100 to 150° C. and the time is 1 to 3 hours; The thickness of the molecular ferroelectric film obtained by spin coating the mixed solution is 2.73 to 5.76 μm.
10. Use of the back electrode for a photovoltaic thin film device as claimed in claim 6 in the preparation of a photovoltaic thin film device.