Polyacrylonitrile fiber and preparation method thereof

By controlling the fiber width and draft multiple in the production process of polyacrylonitrile fibers, the problem of unstable performance of domestic carbon fibers is solved, and homogenized production and performance improvement are achieved.

CN118932508AActive Publication Date: 2024-11-12SHANXI GANGKE CARBON MATERIAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411029819.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-12
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

Domestic carbon fibers have unstable performance, and there are problems such as uneven width, uneven scattering, and stacking of each other, resulting in unstable quality of raw silk production and affecting the yield and performance of carbon fibers.

Method used

By controlling the fiber width and drafting multiple in the steps of water washing treatment, hot water drafting treatment, oiling treatment and drying densification treatment, the D×E×N/A=constant conditions are met, and the fiber is sufficiently solidified and formed. Treatment uniformity and homogenized polyacrylonitrile fibers were prepared.

Benefits of technology

The homogenization production of fibers of different specifications is achieved, which reduces the surface defects and hot melt caused by uneven fiber widths, and improves the density and performance consistency of fibers.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a polyacrylonitrile fiber and a preparation method thereof, and relates to the technical field of polyacrylonitrile-based carbon fiber production, and the preparation method comprises the following steps: sequentially carrying out water washing treatment, hot water drafting treatment, oiling treatment, drying densification treatment and steam drafting treatment on a nascent fiber to obtain the polyacrylonitrile fiber; in any one of the water washing treatment step, the hot water drafting treatment step, the oiling treatment step and the drying densification treatment step, D * E * N / A is equal to a constant; wherein D is the monofilament diameter of the polyacrylonitrile fiber; a is the fiber breadth in the first step; e is the accumulation of the draft multiples applied to the fibers in each step in the second step; n is the K number of the polyacrylonitrile fiber. According to the method, matching of breadth production processes and drafting speeds of all sections is provided for fibers of different specifications, the fibers are fully solidified, washed, oiled, dried and drafted, monofilaments in multifilaments are prevented from being uneven, and the homogenized polyacrylonitrile fibers are prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyacrylonitrile-based carbon fiber production, and specifically relates to polyacrylonitrile fiber and a preparation method thereof. Background Art

[0002] Carbon fiber is an emerging fiber material with high strength and high modulus. It is widely used in military and civilian materials due to its excellent properties such as high strength, high modulus, low density, low resistance, fatigue resistance, high temperature resistance, etc. Among them, polyacrylonitrile-based carbon fiber has good production stability, occupies a leading position among various carbon fibers, and has broad market prospects.

[0003] At present, the main problems of domestic carbon fiber are unstable performance, large discrete coefficient, hairy and broken wires, and large deviations in appearance. Among them, the instability of the quality of raw silk production is one of the key factors. In the process of raw silk production, wet spinning and dry-jet wet spinning generally need to go through coagulation molding, water washing, oiling, drying and other processes in the medium. In these processes, the tows will inevitably have uneven spreading, such as uneven scattering and stacking. From the perspective of each process, in the coagulation bath, the uneven width of the tow means that the degree of double diffusion of the tow in the coagulation bath is inconsistent, which easily leads to the inconsistency of the morphological structure of the primary fiber; in the water washing, the uneven width causes the poor washing effect of individual tows, resulting in solvent residue, and finally leading to many defects on the surface of the tow, and even hot melting during subsequent carbonization and oxidation; when oiling, the uneven width will affect the oiling effect. Ultimately, the yield of raw silk and carbon fiber is low and the performance is poor.

[0004] Therefore, effectively controlling the width of each segment of the tow is a prerequisite for preparing homogenized polyacrylonitrile fiber and polyacrylonitrile-based carbon fiber. In the prior art, the width of the tow is controlled by a width device, but there is no relevant research content on the specific parameters of the width control. For fibers of different specifications, it is impossible to ensure the preparation of homogenized polyacrylonitrile fibers. Summary of the invention

[0005] Therefore, the present invention provides a polyacrylonitrile fiber and a preparation method thereof, the main purpose of which is to control the fiber width in each process step for fibers of different specifications, thereby preparing homogenized polyacrylonitrile fibers.

[0006] In order to solve the above problems, the present invention provides a method for preparing polyacrylonitrile fiber, comprising the following steps: sequentially subjecting the raw fiber to a water washing treatment step, a hot water drawing treatment step, an oiling treatment step, a drying and densification treatment step, and a steam drawing treatment step to obtain the polyacrylonitrile fiber;

[0007] Among them, in any of the steps of the water washing treatment step, the hot water drawing treatment step, the oiling treatment step, and the drying and densification treatment step, the following conditions must be met:

[0008] D×E×N / A=constant;

[0009] Wherein, D is the single filament diameter of polyacrylonitrile fiber;

[0010] A is the fiber width in the first step;

[0011] E is the accumulation of the drafting multiples applied to the fiber in each step in the second step;

[0012] N is the K number of polyacrylonitrile fiber;

[0013] The first step is any one of a water washing step, a hot water drawing step, an oiling step, and a drying and densification step; the second step is a step after the first step;

[0014] If the first step is a water washing step, the constant is 20±5;

[0015] If the first step is a hot water drawing treatment step or an oiling treatment step, the constant is 15±5;

[0016] If the first step is a drying and densification step, the constant is 12±5.

[0017] Furthermore, before the water washing step, the method further comprises:

[0018] The step of preparing the nascent fiber is: subjecting the polyacrylonitrile spinning solution to spinning and coagulation forming treatment to obtain the nascent fiber; wherein the polyacrylonitrile spinning solution is ejected from a spinneret having a pore size of 0.10-0.15 mm; and / or

[0019] The spinning speed is 7-11 m / min.

[0020] Furthermore, during the solidification forming process, the wire drawing speed is 15-35 m / min.

[0021] Furthermore, in the washing step: the fiber is run at a speed of 15-35 m / min; and / or

[0022] The fiber width in the washing step is 20-60 mm;

[0023] Preferably, if the fiber is 3K fiber, the fiber width in the washing step is 20-30 mm;

[0024] If the fiber is 6K fiber, the fiber width in the washing step is 30-40 mm;

[0025] If the fiber is 12K fiber, the fiber width in the water washing step is 50-60 mm.

[0026] Furthermore, in the hot water drawing treatment step and the oiling treatment step: the running speed of the fiber is 35-90 m / min; and / or

[0027] The fiber width in the hot water drawing step and the oiling step is 10-50 mm;

[0028] Preferably, if the fiber is 3K fiber, the fiber width in the hot water drawing step and the oiling step is 10-20 mm;

[0029] If the fiber is 6K fiber, the fiber width in the hot water drawing step and the oiling step is 20-30 mm;

[0030] If the fiber is 12K fiber, the fiber width after the hot water drawing treatment step and in the oiling treatment step is 40-50 mm.

[0031] Furthermore, in the drying and densification step: the fiber running speed is 35-90 m / min; and / or

[0032] The fiber width in the drying and densification step is 15-55 mm;

[0033] Preferably, if the fiber is 3K fiber, the fiber width in the drying and densification step is 15-25 mm;

[0034] If the fiber is 6K fiber, the fiber width in the drying and densification step is 25-35 mm;

[0035] If the fiber is 12K fiber, the fiber width in the drying and densification step is 45-55 mm.

[0036] Furthermore, in the steam drawing treatment step, the running speed of the fiber is 200-400 m / min.

[0037] In another aspect, the present invention provides a polyacrylonitrile fiber, wherein the monofilament diameter of the polyacrylonitrile fiber is 8-12 μm.

[0038] Furthermore, the inter-batch dispersion coefficient and the intra-batch dispersion coefficient of the linear density of the polyacrylonitrile fiber are both ≤0.5%; and / or

[0039] The inter-batch dispersion coefficient and the intra-batch dispersion coefficient of the oil uptake rate of the polyacrylonitrile fiber are both ≤1.0%; and / or

[0040] The inter-batch dispersion coefficient and the intra-batch dispersion coefficient of the tensile strength, elastic modulus and elongation of the polyacrylonitrile fiber are both less than or equal to 1.5%.

[0041] Furthermore, the polyacrylonitrile fiber is prepared by any of the methods described above.

[0042] The polyacrylonitrile fiber and the preparation method thereof provided by the present invention have the following beneficial effects:

[0043] 1. The present invention aims at preparing homogenized polyacrylonitrile fiber by controlling the fiber width in the washing step, the hot water drawing step, the oiling step and the drying and densification step for fibers of different specifications, so that the fiber width is matched with other processes and parameters (such as the diameter of the single filament, the drawing multiple of the fiber, etc.), so that the fiber is fully solidified, washed, oiled, dried and drawn, etc., and the unevenness of the single filaments in the multifilament is avoided; specifically, the processes of the washing step, the hot water drawing step, the oiling step and the drying and densification step meet the condition: D×E×N / A=constant; wherein D is the single filament diameter of the polyacrylonitrile fiber; A is the fiber width in the first step; E is the cumulative drawing multiple applied to the fiber in each step in the second step; N is the K number of the polyacrylonitrile fiber; the constant in the washing step is 20±5; the constant in the hot water drawing step and the oiling step is 15±5; the fiber constant in the drying and densification step is 12±5.

[0044] 2. Furthermore, the present invention controls the running speed of the fiber in the water washing step, the hot water stretching step, the oiling step, the drying densification step and the steam stretching step to obtain the stretching multiple of the fiber in each step in the second step.

[0045] 3. The present invention prepares homogenized polyacrylonitrile fiber through the above method, and the monofilament diameter is 8-12μm, the batch-to-batch dispersion coefficient of linear density and the intra-batch dispersion coefficient are both ≤0.5%, the batch-to-batch dispersion coefficient of oiling rate and the intra-batch dispersion coefficient are both ≤1.0%, and the batch-to-batch dispersion coefficient of tensile strength, elastic modulus and elongation and the intra-batch dispersion coefficient are all ≤1.5%. DETAILED DESCRIPTION

[0046] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the implementation methods or the technical solutions in the prior art description. The following description is only exemplary, and for ordinary technicians in this field, other implementations can be obtained based on the provided extensions without creative work.

[0047] The purpose of the present invention is to provide a method for preparing polyacrylonitrile fiber, and to propose matching of the width and draft multiple of each section for fibers of different specifications, so that the fiber can be fully coagulated, washed, oiled, dried, and drafted, and the unevenness of the single fibers in the multifilament can be avoided, so as to prepare homogenized polyacrylonitrile fiber. The specific scheme is as follows:

[0048] On the one hand, the present invention provides a method for preparing polyacrylonitrile fiber, comprising the following steps: sequentially subjecting the raw fiber to a water washing step, a hot water drawing step, an oiling step, a drying and densification step, and a steam drawing step to obtain the polyacrylonitrile fiber;

[0049] Among them, in any of the steps of the water washing treatment step, the hot water drawing treatment step, the oiling treatment step, and the drying and densification treatment step, the following conditions must be met:

[0050] D×E×N / A=constant;

[0051] Wherein, D is the single filament diameter of polyacrylonitrile fiber;

[0052] A is the fiber width in the first step;

[0053] E is the cumulative draft multiple applied to the fiber in each step in the second step;

[0054] N is the K number of polyacrylonitrile fiber;

[0055] Among them, the first step is any one of the water washing treatment step, the hot water drawing treatment step, the oiling treatment step, and the drying and densification treatment step; the second step is the step after the first step; that is, if the first step is the water washing treatment step, the second step is all the steps including the hot water drawing treatment step, the oiling treatment step, the drying and densification treatment step, and the steam drawing treatment step; if the first step is the hot water drawing treatment step, the second step is all the steps including the oiling treatment step, the drying and densification treatment step, and the steam drawing treatment step; if the first step is the oiling treatment step, the second step is the drying and densification treatment step and the steam drawing treatment step; if the first step is the drying and densification treatment step, the second step is the steam drawing step;

[0056] If the first step is a water washing treatment step, the constant is in the range of 20 ± 5;

[0057] If the first step is a hot water drawing treatment step or an oiling treatment step, the constant is within the range of 15±5;

[0058] If the first step is a drying and densification step, the constant is in the range of 12±5.

[0059] The K number of polyacrylonitrile fiber is the number of filaments contained in a bundle of fiber filaments, for example, 3K means there are 3000 filaments;

[0060] Among them, E (i.e., the accumulation of the stretching multiples applied to the fiber in each step in the second step) is obtained by multiplying the stretching multiples applied to the fiber in each step in the second step. For example, if the fiber width of the water washing treatment step is calculated, the E value is the product of the stretching multiples in the hot water stretching treatment step, the stretching multiples in the oiling treatment step, the stretching multiples in the drying and densification treatment step, and the stretching multiples in the steam stretching treatment step. The stretching multiple in each step is the ratio of the transmission running speed at the end of the step to the transmission running speed at the beginning of the step.

[0061] In some embodiments, before the water washing step, the method further comprises:

[0062] The step of preparing the nascent fiber is: subjecting the polyacrylonitrile spinning solution to spinning and coagulation forming treatment to obtain the nascent fiber; wherein the polyacrylonitrile spinning solution is ejected from a spinneret having a pore size of 0.10-0.15 mm; and / or

[0063] The spinning speed is 7-11m / min. The spinning speed affects the solidification effect. Too fast speed will lead to broken wires, discontinuous spinning, and incomplete solidification; too slow speed will easily cause uneven diffusion between the surface and the core. In addition, the spinning speed must also match and coordinate with the coagulation bath drawing speed and other processes.

[0064] In some embodiments, during the solidification forming process, the wire drawing speed is 15-35 m / min.

[0065] In some embodiments, during the water washing step: the fiber is run at a speed of 15-35 m / min; and / or

[0066] The fiber width in the washing step is 20-60 mm;

[0067] Preferably, if the fiber is 3K fiber, the fiber width in the washing step is 20-30 mm;

[0068] If the fiber is 6K fiber, the fiber width in the washing step is 30-40 mm;

[0069] If the fiber is 12K fiber, the fiber width in the water washing step is 50-60 mm.

[0070] In some embodiments, in the hot water drawing treatment step and the oiling treatment step: the running speed of the fiber is 35-90 m / min; and / or

[0071] The fiber width in the hot water drawing step and the oiling step is 10-50 mm;

[0072] Preferably, if the fiber is 3K fiber, the fiber width in the hot water drawing step and the oiling step is 10-20 mm;

[0073] If the fiber is 6K fiber, the fiber width in the hot water drawing step and the oiling step is 20-30 mm;

[0074] If the fiber is 12K fiber, the fiber width in the hot water drawing treatment step and the oiling treatment step is 40-50 mm.

[0075] In some embodiments, during the drying and densification step: the fiber running speed is 35-90 m / min; and / or

[0076] The fiber width in the drying and densification step is 15-55 mm;

[0077] Preferably, if the fiber is 3K fiber, the fiber width in the drying and densification step is 15-25 mm;

[0078] If the fiber is 6K fiber, the fiber width in the drying and densification step is 25-35 mm;

[0079] If the fiber is 12K fiber, the fiber width in the drying and densification step is 45-55 mm.

[0080] In some embodiments, during the steam drawing step, the fiber runs at a speed of 200-400 m / min.

[0081] In another aspect, the present invention provides a polyacrylonitrile fiber, wherein the monofilament diameter of the polyacrylonitrile fiber is 8-12 μm.

[0082] In some embodiments, the inter-batch coefficient of variation and the intra-batch coefficient of variation of the linear density of the polyacrylonitrile fiber are both ≤ 0.5%; and / or

[0083] The inter-batch dispersion coefficient and intra-batch dispersion coefficient of the oil uptake rate of polyacrylonitrile fiber are both ≤ 1.0%; and / or

[0084] The inter-batch and intra-batch dispersion coefficients of the tensile strength, elastic modulus and elongation of the polyacrylonitrile fiber are both ≤1.5%.

[0085] In some embodiments, the polyacrylonitrile fiber is prepared by any of the above methods.

[0086] The present invention is further described below with reference to specific embodiments and comparative examples.

[0087] Example 1

[0088] This embodiment provides a method for preparing T800S-12K polyacrylonitrile fiber, which specifically includes the following steps:

[0089] Preparation of nascent fibers: The polyacrylonitrile spinning solution is ejected from a spinneret with a hole diameter of 0.12 mm at a spinning speed of 8 m / min, then enters a coagulation bath for coagulation and forming, and is drawn out of the coagulation bath at a drawing speed of 22 m / min to obtain nascent fibers;

[0090] Washing treatment steps: the raw fiber enters the washing tank under the traction of the transmission roller, and the fiber width is controlled to 60mm by the beating roller and the stenter frame, and the running speed of the fiber during the washing process is 22m / min;

[0091] Hot water drawing treatment steps: the washed fibers enter the hot drawing tank under the traction of the transmission roller for hot water drawing treatment;

[0092] Oiling treatment step: oiling the fiber after hot water drawing treatment;

[0093] The fiber width in the hot water drawing step and the oiling step is 50 mm, and the fiber running speed in the hot water drawing process is 57 m / min.

[0094] Drying and densification treatment steps: the oiled fibers pass through the oil-distributing roller and enter the drying and densification section; the fiber width is 55 mm and the fiber running speed is 57 m / min;

[0095] Steam drawing treatment step: the fibers after drying and densification are treated by steam drawing section to obtain polyacrylonitrile fibers; wherein the running speed of the fibers is 272 m / min.

[0096] The monofilament diameter of the polyacrylonitrile fiber prepared in this embodiment is 9 μm, and the CV values ​​of the linear density of the polyacrylonitrile fiber between batches and within batches are 0.5% and 0.3% respectively, and the CV values ​​of the oiling rate between batches and within batches are 1.0% and 0.8% respectively; the CV values ​​of the tensile strength, elastic modulus and elongation between batches and within batches are all ≤1.0%.

[0097] In this embodiment, the fiber width in the water washing step is about 60 mm, which is calculated by A=D×E×N / constant=(9 μm×12000 / 1000) mm×4.77×2.59 / 22.2; the fiber width in the hot water drawing step and the oiling step is A=(9 μm×12000 / 1000) mm×4.77 / 10.3, which is about 50 mm; the fiber width in the drying and densification step is A=(9 μm×12000 / 1000) mm×4.77 / 9.4, which is about 55 mm;

[0098] Among them, 4.77 is the stretching multiple applied to the fiber in the steam stretching treatment step, and 2.59 is the stretching multiple applied to the fiber in the hot water stretching treatment step; the stretching multiples in the oiling treatment step and the drying and densification treatment step are approximately 1, and the stretching multiples applied to the fiber during the raw silk production process are concentrated in the coagulation bath, hot water stretching, and steam stretching, and the stretching multiples in the remaining processes are approximately 1.

[0099] Example 2

[0100] This embodiment provides a method for preparing T700S-12K polyacrylonitrile fiber, which specifically includes the following steps:

[0101] Preparation of nascent fibers: The polyacrylonitrile spinning solution is ejected from a spinneret with a hole diameter of 0.12 mm at a spinning speed of 11 m / min, then enters a coagulation bath for coagulation and forming, and is drawn out of the coagulation bath at a drawing speed of 30 m / min to obtain nascent fibers;

[0102] Washing treatment steps: the raw fiber enters the washing tank under the traction of the transmission roller, and the fiber width is controlled to 60mm by the beating roller and the stenter frame, and the running speed of the fiber during the washing process is 30m / min;

[0103] Hot water drawing treatment steps: the washed fibers enter the hot drawing tank under the traction of the transmission roller for hot water drawing treatment;

[0104] Oiling treatment step: oiling the fiber after hot water drawing treatment; wherein the fiber width in the hot water drawing treatment step and the oiling treatment step is 50 mm, and the running speed of the fiber during the hot water drawing process is 70 m / min;

[0105] Drying and densification treatment steps: the oiled fibers pass through an oil-distributing roller and enter drying and densification; the fiber width is 55 mm and the fiber running speed is 70 m / min;

[0106] Steam drawing treatment step: the fibers after drying and densification are treated by steam drawing section to obtain polyacrylonitrile fibers; wherein the running speed of the fibers is 260 m / min.

[0107] The monofilament diameter of the polyacrylonitrile fiber prepared in this embodiment is 12 μm, and the CV values ​​of the linear density of the polyacrylonitrile fiber between batches and within batches are 0.5% and 0.5% respectively, and the CV values ​​of the oiling rate between batches and within batches are 1.0% and 1.0% respectively; the CV values ​​of the tensile strength, elastic modulus and elongation between batches and within batches are all ≤1.5%.

[0108] In this embodiment, the fiber width in the water washing step is about 60 mm, which is calculated by A=D×E×N / constant=(12 μm×12000 / 1000) mm×3.71×2.33 / 21; the fiber width in the hot water drawing step and the oiling step is A=(12 μm×12000 / 1000) mm×3.71 / 10.6, which is about 50 mm; the fiber width in the drying and densification step is A=(12 μm×12000 / 1000) mm×3.71 / 9.7, which is about 55 mm;

[0109] Among them, 3.71 is the stretching multiple applied to the fiber in the steam stretching treatment step, and 2.33 is the stretching multiple applied to the fiber in the hot water stretching treatment step; the stretching multiples in the oiling treatment step and the drying and densification treatment step are approximately 1, and the stretching multiples applied to the fiber during the raw silk production process are concentrated in the coagulation bath, hot water stretching, and steam stretching, and the stretching multiples in the remaining processes are approximately 1.

[0110] Example 3

[0111] This embodiment provides a method for preparing T700S-3K polyacrylonitrile fiber, which specifically includes the following steps:

[0112] Preparation of nascent fibers: The polyacrylonitrile spinning solution is ejected from a spinneret with a hole diameter of 0.12 mm at a spinning speed of 11 m / min, then enters a coagulation bath for coagulation and forming, and is drawn out of the coagulation bath at a drawing speed of 30 m / min to obtain nascent fibers;

[0113] Washing treatment steps: the raw fiber enters the washing tank under the traction of the transmission roller, and the fiber width is controlled to 20mm by the beating roller and the stenter frame, and the fiber running speed during the washing process is 30m / min;

[0114] Hot water drawing treatment steps: the washed fibers enter the hot drawing tank under the traction of the transmission roller for hot water drawing treatment;

[0115] Oiling treatment step: oiling the fiber after hot water drawing treatment; wherein the fiber width in the hot water drawing treatment step and the oiling treatment step is 12 mm, and the running speed of the fiber during the hot water drawing process is 70 m / min;

[0116] Drying and densification treatment steps: the oiled fibers pass through an oil-distributing roller and enter drying and densification; the fiber width is 18 mm and the fiber running speed is 70 m / min;

[0117] Steam drawing treatment step: the fibers after drying and densification are treated by steam drawing section to obtain polyacrylonitrile fibers; wherein the running speed of the fibers is 260 m / min.

[0118] The monofilament diameter of the polyacrylonitrile fiber prepared in this embodiment is 12 μm, and the CV values ​​of the linear density of the polyacrylonitrile fiber between batches and within batches are 0.5% and 0.4% respectively, and the CV values ​​of the oiling rate between batches and within batches are 1.0% and 1.0% respectively; the CV values ​​of the tensile strength, elastic modulus and elongation between batches and within batches are all ≤1.3%.

[0119] In this embodiment, the fiber width in the water washing step is about 20 mm, which is calculated by A=D×E×N / constant=(12 μm×3000 / 1000) mm×3.71×2.33 / 15.5; the fiber width in the hot water drawing step and the oiling step is A=(12 μm×3000 / 1000) mm×3.71 / 11, which is about 12 mm; the fiber width in the drying and densification step is A=(12 μm×3000 / 1000) mm×3.71 / 7.4, which is about 18 mm;

[0120] Among them, 3.71 is the stretching multiple applied to the fiber in the steam stretching treatment step, and 2.33 is the stretching multiple applied to the fiber in the hot water stretching treatment step; the stretching multiples in the oiling treatment step and the drying and densification treatment step are approximately 1, and the stretching multiples applied to the fiber during the raw silk production process are concentrated in the coagulation bath, hot water stretching, and steam stretching, and the stretching multiples in the remaining processes are approximately 1.

[0121] Example 4

[0122] This embodiment provides a method for preparing T800S-12K polyacrylonitrile fiber, which specifically includes the following steps:

[0123] Preparation of nascent fibers: The polyacrylonitrile spinning solution is ejected from a spinneret with a hole diameter of 0.12 mm at a spinning speed of 7 m / min, then enters a coagulation bath for coagulation and forming, and is drawn out of the coagulation bath at a drawing speed of 21 m / min to obtain nascent fibers;

[0124] Washing treatment steps: the raw fiber enters the washing tank under the traction of the transmission roller, and the fiber width is controlled to 50mm by the beating roller and the stenter frame, and the running speed of the fiber during the washing process is 21m / min;

[0125] Hot water drawing treatment steps: the washed fibers enter the hot drawing tank under the traction of the transmission roller for hot water drawing treatment;

[0126] Oiling treatment step: oiling the fiber after hot water drawing treatment;

[0127] The fiber width in the hot water drawing step and the oiling step is 40 mm, and the fiber running speed during the hot water drawing process is 52 m / min.

[0128] Drying and densification treatment steps: the oiled fibers pass through the oil-distributing roller and enter the drying and densification section; the fiber width is 45 mm and the fiber running speed is 52 m / min;

[0129] Steam drawing treatment step: the fibers after drying and densification are treated by steam drawing section to obtain polyacrylonitrile fibers; wherein the running speed of the fibers is 238 m / min.

[0130] The monofilament diameter of the polyacrylonitrile fiber prepared in this embodiment is 9 μm, and the CV values ​​of the linear density of the polyacrylonitrile fiber between batches and within batches are 0.5% and 0.3% respectively, and the CV values ​​of the oiling rate between batches and within batches are 1.0% and 0.8% respectively; the CV values ​​of the tensile strength, elastic modulus and elongation between batches and within batches are all ≤1.0%.

[0131] In this embodiment, the fiber width in the water washing step is about 50 mm, which is calculated by A=D×E×N / constant=(9μm×12000 / 1000)mm×4.58×2.48 / 24.5; the fiber width in the hot water drawing step and the oiling step is A=(9μm×12000 / 1000)mm×4.58 / 12.4, which is about 40 mm; the fiber width in the drying and densification step is A=(9μm×12000 / 1000)mm×4.58 / 11, which is about 45 mm;

[0132] Among them, 4.58 is the stretching multiple applied to the fiber in the steam stretching treatment step, and 2.48 is the stretching multiple applied to the fiber in the hot water stretching treatment step; the stretching multiples in the oiling treatment step and the drying and densification treatment step are approximately 1, and the stretching multiples applied to the fiber during the raw silk production process are concentrated in the coagulation bath, hot water stretching, and steam stretching, and the stretching multiples in the remaining processes are approximately 1.

[0133] Comparative Example 1

[0134] This comparative example provides a method for preparing T800S-12K polyacrylonitrile fiber, which specifically comprises the following steps:

[0135] Preparation of nascent fibers: The polyacrylonitrile spinning solution is ejected from a spinneret with a hole diameter of 0.12 mm at a spinning speed of 8 m / min, then enters a coagulation bath for coagulation and forming, and is drawn out of the coagulation bath at a drawing speed of 22 m / min to obtain nascent fibers;

[0136] Washing treatment steps: the raw fiber enters the washing tank under the traction of the transmission roller, and the fiber width is controlled to 30mm by the beating roller and the stenter frame, and the running speed of the fiber during the washing process is 22m / min;

[0137] Hot water drawing treatment: The washed fibers are drawn into the hot drawing tank by the driving roller for hot water drawing treatment;

[0138] Oiling treatment step: oiling the fiber after hot water drawing treatment; wherein the fiber width in the hot water drawing treatment step and the oiling treatment step is 35 mm, and the running speed of the fiber during the hot water drawing process is 57 m / min;

[0139] Drying and densification treatment steps: the oiled fibers pass through an oil-distributing roller and enter drying and densification; the fiber width is 55 mm and the fiber running speed is 57 m / min;

[0140] Steam drawing treatment step: the fibers after drying and densification are treated by steam drawing section to obtain polyacrylonitrile fibers; wherein the running speed of the fibers is 272 m / min.

[0141] The CV values ​​of the linear density of the polyacrylonitrile fiber prepared in this comparative example between batches and within batches are 3.0% and 2.5% respectively, and the CV values ​​of the oil pick-up rate, tensile strength, elastic modulus and elongation between batches and within batches are all greater than 3.0%.

[0142] Due to the narrow fiber width, incomplete water washing, high sulfoxide residue in the preparation process of Comparative Example 1, the fiber is prone to heat melting during the carbonization process, uneven oiling, uneven fiber oxidation and carbonization, poor drying and densification uniformity, poor fiber density, and easy fiber breakage during the steam drawing process, the tensile strength, elastic modulus and other indicators of the prepared fiber are lower than those in Example 1, and the fiber orientation degree is low.

[0143] Comparative Example 2

[0144] This comparative example provides a method for preparing T700S-3K polyacrylonitrile fiber, which specifically comprises the following steps:

[0145] Preparation of nascent fibers: The polyacrylonitrile spinning solution is ejected from a spinneret with a hole diameter of 0.12 mm at a spinning speed of 11 m / min, then enters a coagulation bath for coagulation and forming, and is drawn out of the coagulation bath at a drawing speed of 30 m / min to obtain nascent fibers;

[0146] Washing treatment steps: the raw fiber enters the washing tank under the traction of the transmission roller, and the fiber width is controlled to 60mm by the beating roller and the stenter frame, and the running speed of the fiber during the washing process is 30m / min;

[0147] Hot water drawing treatment steps: the washed fibers enter the hot drawing tank under the traction of the transmission roller for hot water drawing treatment;

[0148] Oiling treatment step: oiling the fiber after hot water drawing treatment; wherein the fiber width in the hot water drawing treatment step and the oiling treatment step is 50 mm, and the running speed of the fiber during the hot water drawing process is 70 m / min;

[0149] Drying and densification treatment steps: the oiled fibers pass through an oil-distributing roller and enter drying and densification; the fiber width is 55 mm and the fiber running speed is 70 m / min;

[0150] Steam drawing treatment step: the fibers after drying and densification are treated by steam drawing section to obtain polyacrylonitrile fibers; wherein the running speed of the fibers is 260 m / min.

[0151] In this comparative example, when controlling the fiber width in the washing step, the hot water drawing step, the oiling step and the drying and densification step, the matching with the fiber K number is not considered, that is, the condition is not satisfied in the above steps: D×E×N / A=constant; wherein D is the single filament diameter of the polyacrylonitrile fiber; A is the fiber width in the first step; E is the accumulation of the drawing multiples applied to the fiber in each step in the second step; N is the K number of the polyacrylonitrile fiber, resulting in the phenomenon of single filament floating out during the preparation process, easy roller winding and threading during operation, and unstable operation; the CV values ​​of the linear density of the prepared polyacrylonitrile fiber between batches and within batches are 4.0% and 3.5%, respectively, and the CV values ​​of the oiling rate, tensile strength, elastic modulus and elongation between batches and within batches are all greater than 5.0%.

[0152] It is easy for those skilled in the art to understand that, without conflict, the advantageous technical features of the above-mentioned methods can be freely combined and superimposed.

[0153] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention shall be included in the protection scope of the present invention. The above description is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and variations can be made without departing from the technical principles of the present invention. These improvements and variations should also be regarded as the protection scope of the present invention.

Claims

1. A method for preparing polyacrylonitrile fiber, It is characterized in that The method comprises the following steps: sequentially subjecting the raw fibers to a water washing treatment step, a hot water drawing treatment step, an oiling treatment step, a drying and densification treatment step, and a steam drawing treatment step to obtain polyacrylonitrile fibers; Among them, in any of the steps of the water washing treatment step, the hot water drawing treatment step, the oiling treatment step, and the drying and densification treatment step, the following conditions must be met: D×E×N / A=constant; Wherein, D is the single filament diameter of polyacrylonitrile fiber; A is the fiber width in the first step; E is the accumulation of the drafting multiples applied to the fiber in each step in the second step; N is the K number of polyacrylonitrile fiber; The first step is any one of a water washing step, a hot water drawing step, an oiling step, and a drying and densification step; the second step is a step after the first step; If the first step is a water washing step, the constant is 20±5; If the first step is a hot water drawing treatment step or an oiling treatment step, the constant is 15±5; If the first step is a drying and densification step, the constant is 12±5.

2. The method for preparing polyacrylonitrile fiber according to claim 1, It is characterized in that Before the water washing step, the method further comprises: The step of preparing the nascent fiber is as follows: performing spinning and coagulation forming treatment on the polyacrylonitrile spinning solution to obtain the nascent fiber; Wherein, the polyacrylonitrile spinning solution is ejected from a spinneret with a pore size of 0.10-0.15 mm; and / or The spinning speed is 7-11 m / min.

3. The method for preparing polyacrylonitrile fiber according to claim 2, It is characterized in that During the solidification forming process, the wire drawing speed is 15-35m / min.

4. The method for preparing polyacrylonitrile fiber according to claim 1, It is characterized in that In the water washing step: the running speed of the fiber is 15-35 m / min; and / or The fiber width in the washing step is 20-60 mm; Preferably, if the fiber is 3K fiber, the fiber width in the washing step is 20-30 mm; If the fiber is 6K fiber, the fiber width in the washing step is 30-40 mm; If the fiber is 12K fiber, the fiber width in the water washing step is 50-60 mm.

5. The method for preparing polyacrylonitrile fiber according to claim 1, It is characterized in that In the hot water drawing treatment step and the oiling treatment step: the running speed of the fiber is 35-90 m / min; and / or The fiber width in the hot water drawing step and the oiling step is 10-50 mm; Preferably, if the fiber is 3K fiber, the fiber width in the hot water drawing step and the oiling step is 10-20 mm; If the fiber is 6K fiber, the fiber width in the hot water drawing step and the oiling step is 20-30 mm; If the fiber is 12K fiber, the fiber width in the hot water drawing treatment step and the oiling treatment step is 40-50 mm.

6. The method for preparing polyacrylonitrile fiber according to claim 1, It is characterized in that In the drying and densification step: the fiber running speed is 35-90 m / min; and / or The fiber width in the drying and densification step is 15-55 mm; Preferably, if the fiber is 3K fiber, the fiber width in the drying and densification step is 15-25 mm; If the fiber is 6K fiber, the fiber width in the drying and densification step is 25-35 mm; If the fiber is 12K fiber, the fiber width in the drying and densification step is 45-55 mm.

7. The method for preparing polyacrylonitrile fiber according to claim 1, It is characterized in that In the steam drawing treatment step, the running speed of the fiber is 200-400 m / min.

8. A polyacrylonitrile fiber, It is characterized in that The monofilament diameter of the polyacrylonitrile fiber is 8-12 μm.

9. The polyacrylonitrile fiber according to claim 8, It is characterized in that The inter-batch dispersion coefficient and the intra-batch dispersion coefficient of the linear density of the polyacrylonitrile fiber are both ≤0.5%; and / or The inter-batch dispersion coefficient and the intra-batch dispersion coefficient of the oil uptake rate of the polyacrylonitrile fiber are both ≤1.0%; and / or The inter-batch dispersion coefficient and the intra-batch dispersion coefficient of the tensile strength, elastic modulus and elongation of the polyacrylonitrile fiber are both less than or equal to 1.5%.

10. The polyacrylonitrile fiber according to claim 8 or 9, It is characterized in that The polyacrylonitrile fiber is prepared by the method according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Processing equipment and method for continuous fiber tows

    CN104790149A

  • Preparation method of polyacrylonitrile fibers

    CN111088541A

  • Carbon fiber bundle for winding forming and preparation method and application thereof

    CN112048854A

  • Polyacrylonitrile-based large-tow carbon fiber and preparation method thereof

    CN116024701A

  • Method for producing carbon fiber

    JP2009191425A