Multicolor electroluminescent fiber and electrostatic spinning preparation method thereof

The electroluminescent material is combined with fluorescent dye through the electrospinning preparation method to form multi-color electroluminescent fibers, which solves the problem of limited color adjustment range in the prior art and achieves high brightness and wide application effects.

CN118932523AActive Publication Date: 2024-11-12ZHEJIANG SCI-TECH UNIV

Patent Information

Application Number
CN202410989957.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

The existing electroluminescent fiber color adjustment range is limited, making it difficult to meet the demand for multiple colors in practical applications.

Method used

Through the electrospinning preparation method, electroluminescent materials are combined with fluorescent dyes to form multi-color electroluminescent fibers, including conductive fibers, luminescent layers, color conversion layers, dielectric layers and external electrodes, and the color range is expanded by using fluorescent dyes.

Benefits of technology

It has achieved a large range of color adjustment, broadened the application field of electroluminescent fibers, and has high brightness, flexibility and excellent mechanical properties, which is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932523A_ABST
    Figure CN118932523A_ABST
Patent Text Reader

Abstract

The invention discloses a multicolor electroluminescent fiber and an electrostatic spinning preparation method thereof. The preparation method comprises the following steps: (1) preparing a luminescent layer through electrostatic spinning: loading an electroluminescent material to the surface of a conductive fiber through electrostatic spinning; (2) dip-dyeing to prepare a color conversion layer: dipping the fiber loaded with the electroluminescent material into a fluorescent dye solution, so that the surface of the fiber is colored to form the color conversion layer; (3) preparing a dielectric layer by dip-coating: immersing the fiber dyed with the fluorescent dye into a PDMS diluent to prepare the dielectric layer; (4) constructing an outer electrode: loading the outer electrode on the surface of the dielectric layer in a winding or coating manner; and (5) insulating packaging: finally coating a transparent insulating polymer for packaging. According to the method, the color of the electroluminescent fiber is widened by introducing different colors of fluorescent dyes, and the method has high application value in the fields of intelligent clothes and pattern decoration. The preparation process is simple, mild in condition, low in cost and suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of wearable intelligent clothing, and specifically relates to a multicolor electroluminescent fiber and an electrostatic spinning preparation method thereof. Background Art

[0002] In recent years, wearable electronic products have attracted widespread attention due to their advantages such as lightness, flexibility, portability and low power consumption. By combining multiple functional materials by physical or chemical methods, wearable electronic devices can have various basic functions, such as luminescence, thermal management, power generation and sensing. Traditional planar and thin-film wearable electronic products show excellent and stable optoelectronic properties, but lack breathability and comfort. In contrast, emerging wearable electronic products based on functional fibers have become more attractive, with the advantages of flexible wearability, good wearability, scalable preparation and multifunctional integration.

[0003] Among the wide range of functional fiber electronics, electroluminescent fibers have been widely studied for various applications, including wearable and portable lighting, displays, and signage. For example, smart wearable luminous textiles are being developed to manufacture traffic safety vests to prevent nighttime traffic accidents. In addition, wearable luminous textiles can also be used for fabric displays and entertainment decorations. Although electroluminescent fibers enable the integration of functional luminescent fibers into textiles by knitting, weaving, or braiding, electroluminescent fibers have only a small number of colors to choose from due to the limited variety of electroluminescent materials.

[0004] From the perspective of application, various color expression technologies can broaden the application field of AC electroluminescent fibers. Although there have been reports of color adjustment by mixing luminescent powders of different colors or changing the concentration of dopants, only a small range of color adjustment can be achieved. Therefore, it is necessary to develop a feasible and universal method for a wider range of color expression to meet the color needs of practical applications. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention provides a multicolor electroluminescent fiber and an electrostatic spinning preparation method thereof.

[0006] The present invention is achieved through the following technical solutions:

[0007] A method for preparing multicolor electroluminescent fibers by electrospinning, the method comprising the following steps:

[0008] (1) Preparation of the light-emitting layer by electrospinning: an electroluminescent material, a solvent and a polymer as a binder are mixed and stirred to obtain a light-emitting spinning solution, and the electroluminescent material is loaded onto the surface of the conductive fiber by electrospinning to obtain a conductive fiber with a light-emitting layer;

[0009] The electroluminescent material is selected from one or more of zinc sulfide-doped luminescent powders ZnS:Mn, ZnS:Cl, ZnS:Cu, ZnS:Sm, ZnS:Tm, ZnS:Cu,Cl and ZnS:Mn,Cu,Cl, and the mass ratio of the electroluminescent material to the polymer is (1-5):1;

[0010] (2) Preparation of color conversion layer by dyeing: The conductive fiber with the luminescent layer is dipped into a fluorescent dye solution to dye the fiber surface, and then dried to form a color conversion layer;

[0011] (3) Dip-coating to prepare the dielectric layer: The conductive fiber dyed with fluorescent dye is immersed in the PDMS dilution solution, then slowly pulled out at a uniform speed, and dried to obtain a uniformly loaded dielectric layer;

[0012] The PDMS diluent is a mixture of PDMS and n-hexane in a mass ratio of 1: (1-5);

[0013] (4) constructing an external electrode: loading the external electrode on the surface of the dielectric layer by winding or coating to obtain an electroluminescent fiber;

[0014] (5) Insulation packaging: A transparent insulating polymer is coated on the outside of the electroluminescent fiber, and after drying, a multi-color electroluminescent fiber with a transparent packaging layer as the outermost layer is obtained.

[0015] Preferably, the electroluminescent material is one or more of ZnS:Mn, ZnS:Cl, ZnS:Cu, ZnS:Cu,Cl and ZnS:Mn,Cu,Cl; the mass ratio of the electroluminescent material to the polymer is (2-4):1. The best case is that the mass ratio of ZnS:Cu luminescent powder to polyvinylidene fluoride-hexafluoropropylene is 3:1.

[0016] Preferably, in the PDMS dilution solution, the mass ratio of PDMS to n-hexane is 1:(2-4). The most preferred mass ratio of PDMS to n-hexane is 1:(3-4).

[0017] Preferably, in step (1),

[0018] The conductive fiber includes one or more of metal conductive fiber, metal particle plated chemical fiber, carbon fiber, ion gel fiber, and conductive polymer composite fiber;

[0019] The particle size of the electroluminescent material is 10 to 50 μm, preferably 10 to 30 μm;

[0020] The solvent is a mixture of N,N-dimethylformamide and acetone in a mass ratio of (1-2):1;

[0021] The polymer is selected from one of styrene-butadiene-styrene, polyurethane, and polyvinylidene fluoride-hexafluoropropylene;

[0022] Preferably, in step (1),

[0023] The steps of preparing the luminescent spinning solution are: firstly preparing the polymer into a polymer solution with a solid content of 10% to 20%, then adding the electroluminescent material and mixing to obtain the luminescent spinning solution.

[0024] Preferably, in step (1), the process parameters of electrospinning are: flow rate 0.3-1.5 mL / hr, rotation speed 140-260 rpm, and moving speed 0.5-2.5 mm / s.

[0025] Preferably, in step (2), the fluorescent dye is one or more of cyanine dyes, rhodamine dyes, fluorescein dyes, coumarins and their derivatives, benzanthrone dyes, nelcarboxylic acid derivatives, anthraquinone derivatives, and naphthoquinone derivatives.

[0026] Preferably, in step (2), the drying conditions are: temperature 60-100° C., time 5-10 min; in step (3), the drying conditions are: temperature 80-120° C., time 15-30 min.

[0027] Preferably, in step (4), the external electrode comprises a metal wire or metal particles, the metal wire comprises a silver wire, a copper wire, a silver-plated copper wire, a steel wire, a titanium wire or a tungsten wire, and the metal particles comprise a conductive silver paste, a silver nanowire, a copper nanowire or a silver nanowire.

[0028] Preferably, when the outer electrode is prepared by winding method, the pitch is 0.2 to 0.8 mm;

[0029] When the coating method is used to load the external electrode, the surface of the dielectric layer needs to be plasma treated to improve the hydrophilicity. The plasma treatment power is 100-150W, the treatment time is 1-5min, and then the conductive solution is dipped for 5-30s and 2-5 times. After dipping, it is dried at a temperature of 60-150°C, preferably 80-100°C.

[0030] Preferably, in step (5), the insulating polymer is one or more of epoxy resin, acrylate resin, polyurethane resin, polytetrafluoroethylene resin, polyvinylidene fluoride resin or silicone resin; the drying conditions are: temperature 80-150°C, time 20-40 minutes. The best choice of insulating polymer is one or more of epoxy resin, polyurethane resin, polyvinylidene fluoride resin or silicone resin.

[0031] A multicolor electroluminescent fiber prepared by the preparation method of the present invention, the multicolor electroluminescent fiber comprises, from the inside to the outside, a conductive fiber, a luminescent layer, a color conversion layer, a dielectric layer and a packaging layer, the outer surface of the dielectric layer is wound or coated with an external electrode, and the external electrode is a metal wire or metal particle. (1) Conductive fiber, serving as a fiber base electrode; (2) The luminescent layer, a functional layer for generating electroluminescence; (3) The color conversion layer, utilizing the light absorption and emission characteristics of fluorescent dyes to perform color processing on electroluminescence; (4) The dielectric layer, preventing the device from short-circuiting; (5) The external electrode, together with the fiber base electrode, provides the electric field required for electroluminescence; (6) The transparent packaging layer, serving to insulate and protect the electroluminescent fiber.

[0032] Compared with the prior art, the positive and progressive effects of the present invention are:

[0033] (1) The method of the present invention changes the color of the electroluminescent fiber by introducing fluorescent dyes of different colors, thus greatly broadening the range of luminescent colors and having high application value in the fields of smart clothing and pattern decoration;

[0034] (2) The process of the present invention combines electrospinning and solution coating, and can realize the continuous preparation of electroluminescent fibers through equipment assembly and modification. Moreover, the technology is simple, efficient, mild, low-cost, green and environmentally friendly, and suitable for industrial production;

[0035] (3) The electroluminescent fiber of the present invention has good flexibility, good brightness, and excellent mechanical properties, and can be knitted, woven, braided, sewn, embroidered, etc. using industrial textile equipment. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is a schematic diagram of the structure of the electroluminescent fiber of the present invention;

[0037] Figure 2 It is a purple electroluminescent fiber;

[0038] Figure 3 It is a green electroluminescent fiber;

[0039] Figure 4 It is a blue electroluminescent fiber;

[0040] Figure 5 The effect of the mass ratio of n-hexane to PDMS on the brightness of the luminescent fiber;

[0041] Figure 6 The effect of the mass ratio of electroluminescent material to polymer on the brightness of luminescent fiber;

[0042] Figure 7 It is an electroluminescent fiber without silver nanowire outer electrode;

[0043] Figure 8This is a photo of the embroidered luminous LOGO on the jacket. DETAILED DESCRIPTION

[0044] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.

[0045] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0046] The present invention is now further described in conjunction with specific examples. The following examples are only for explaining the present invention, but do not constitute a limitation of the present invention. The test samples and test processes used in the following examples include the following (if the specific experimental conditions are not indicated in the examples, they are usually in accordance with conventional conditions or the conditions recommended by the reagent company; the reagents, consumables, etc. used in the following examples, if not otherwise specified, can all be obtained from commercial channels).

[0047] The structural schematic diagram of the electroluminescent fiber of the present invention is shown in Figure 1 The multicolor electroluminescent fiber includes a conductive fiber, a light-emitting layer, a color conversion layer, a dielectric layer and a packaging layer from the inside to the outside. The outer surface of the dielectric layer is wound or coated with an external electrode, and the external electrode is a metal wire or a metal particle.

[0048] Example 1 (color conversion layer is rhodamine B dye solution)

[0049] A multicolor electroluminescent fiber, the preparation method thereof has the following steps:

[0050] (1) Preparation of the light-emitting layer by electrospinning: First, N,N-dimethylformamide and acetone were mixed (mass ratio 1.5:1) as solvents to prepare a polyvinylidene fluoride-hexafluoropropylene solution with a solid content of 10%, and then ZnS:Cu luminescent powder was added according to a mass ratio of ZnS:Cu luminescent powder to polyvinylidene fluoride-hexafluoropropylene of 2:1, and the mixture was stirred to obtain a luminescent spinning solution. The electroluminescent material was loaded onto the surface of the silver-plated nylon fiber by electrospinning, and the spinning process parameters were: flow rate 0.8mL / hr, rotation speed 160rpm, and moving speed 1.0mm / s.

[0051] (2) Preparation of color conversion layer by dyeing: The fiber loaded with electroluminescent material is immersed in rhodamine B dye solution to dye the fiber surface, and then dried at 80°C for 8 minutes to completely evaporate the solvent.

[0052] (3) Preparation of dielectric layer by dip coating: Prepare a PDMS diluent mixed with PDMS and n-hexane in a mass ratio of 1:2, immerse the fluorescent dye-dyed fiber in the PDMS diluent, then slowly pull it out at a uniform speed, and dry it at 100°C for 20 min to obtain a uniformly loaded dielectric layer.

[0053] (4) Construction of external electrode: Copper wire (diameter 0.05 mm) was wound around the dielectric layer at a pitch of 0.4 mm, and then plasma treated (100 W, 2 min). The fiber was then immersed in a silver nanowire dispersion for 10 s, taken out and dried at 80 °C. After repeating this process 5 times, a uniformly distributed silver nanowire external electrode was formed on the surface of the dielectric layer.

[0054] (5) Insulation packaging: Silicone resin is coated on the outside of the electroluminescent fiber and dried at 100°C for 30 minutes to obtain a transparent packaging layer.

[0055] The prepared electroluminescent fibers Figure 2 As shown, after applying an AC driving voltage, purple light is emitted (the superposition of the blue light of the ZnS:Cu luminescent powder and the red light of Rhodamine B), and it can still work stably and normally after bending, compression, and water washing.

[0056] Example 2 (color conversion layer is fluorescent yellow 3G dye solution)

[0057] A multicolor electroluminescent fiber, the preparation method thereof has the following steps:

[0058] (1) Preparation of the light-emitting layer by electrospinning: First, N,N-dimethylformamide and acetone were mixed (mass ratio 1.5:1) as solvents to prepare a polyvinylidene fluoride-hexafluoropropylene solution with a solid content of 10%, and then ZnS:Cu luminescent powder was added according to a mass ratio of ZnS:Cu luminescent powder to polyvinylidene fluoride-hexafluoropropylene of 2:1, and the mixture was stirred to obtain a luminescent spinning solution. The electroluminescent material was loaded onto the surface of the silver-plated nylon fiber by electrospinning, and the spinning process parameters were: flow rate 0.8mL / hr, rotation speed 160rpm, and moving speed 1.0mm / s.

[0059] (2) Preparation of color conversion layer by dyeing: The fiber loaded with electroluminescent material is immersed in fluorescent yellow 3G dye solution to dye the fiber surface, and then dried at 80°C for 8 minutes to completely evaporate the solvent.

[0060] (3) Preparation of dielectric layer by dip coating: Prepare a PDMS diluent mixed with PDMS and n-hexane in a mass ratio of 1:2, immerse the fluorescent dye-dyed fiber in the PDMS diluent, then slowly pull it out at a uniform speed, and dry it at 100°C for 20 min to obtain a uniformly loaded dielectric layer.

[0061] (4) Construction of external electrode: Copper wire (diameter 0.05 mm) was wound around the dielectric layer at a pitch of 0.4 mm, and then plasma treated (100 W, 2 min). The fiber was then immersed in a silver nanowire dispersion for 10 s, taken out and dried at 80 °C. After repeating this process 5 times, a uniformly distributed silver nanowire external electrode was formed on the surface of the dielectric layer.

[0062] (5) Insulation packaging: Silicone resin is coated on the outside of the electroluminescent fiber and dried at 100°C for 30 minutes to obtain a transparent packaging layer.

[0063] The prepared electroluminescent fibers Figure 3 As shown, after applying an AC driving voltage, green light is emitted (the superposition of the blue light of the ZnS:Cu luminescent powder and the yellow light of the fluorescent yellow 3G), and it can still work stably and normally after bending, compression, and water washing.

[0064] Example 3 (Single factor experiment on the effect of PDMS dilution ratio on the brightness of luminescent fiber)

[0065] A blue electroluminescent fiber, the preparation method thereof has the following steps:

[0066] (1) Preparation of the light-emitting layer by electrospinning: First, N,N-dimethylformamide and acetone were mixed (mass ratio 1.5:1) as solvents to prepare a polyvinylidene fluoride-hexafluoropropylene solution with a solid content of 10%, and then ZnS:Cu luminescent powder was added according to the mass ratio of ZnS:Cu luminescent powder to polyvinylidene fluoride-hexafluoropropylene of 3:1, and the mixture was stirred to obtain a luminescent spinning solution. The electroluminescent material was loaded onto the surface of the silver-plated nylon fiber by electrospinning, and the spinning process parameters were: flow rate 0.5mL / hr, rotation speed 190rpm, and moving speed 1.4mm / s.

[0067] (2) Preparation of dielectric layer by dip coating: PDMS dilution solutions were prepared by mixing PDMS and n-hexane in mass ratios of 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, and 1:4. The fiber was immersed in the PDMS dilution solutions of different proportions, then slowly pulled out at a uniform speed and dried at 100°C for 20 min to obtain a uniformly loaded dielectric layer.

[0068] (3) Construction of external electrode: Copper wire (diameter 0.05 mm) was wound around the dielectric layer at a pitch of 0.4 mm, and then plasma treated (100 W, 2 min). The fiber was then immersed in a silver nanowire dispersion for 10 s, taken out and dried at 80 °C. After repeating this process 5 times, a uniformly distributed silver nanowire external electrode was formed on the surface of the dielectric layer.

[0069] (4) Insulation packaging: Silicone resin is coated on the outside of the electroluminescent fiber and dried at 100°C for 30 minutes to obtain a transparent packaging layer.

[0070] The prepared electroluminescent fibers Figure 4 As shown, no color conversion layer was added during the preparation process, and blue light was displayed after applying an AC driving voltage (only the ZnS:Cu luminescent powder emitted light, and color conversion was not achieved). It can still work stably and normally after bending, compression, and washing.

[0071] The brightness of the luminescent fiber made of PDMS dilution with different PDMS and n-hexane mass ratios was tested. The results are shown in Figure 5 .according to Figure 5 The results show that the mass ratio of PDMS to n-hexane is 1:(2-4) which is relatively bright. The best mass ratio of PDMS to n-hexane is 1:(3-4). The brightness of the luminescent fiber is the highest when the mass ratio of PDMS to n-hexane is 1:3.

[0072] Example 4 (Single factor experiment on the effect of electroluminescent material doping ratio on the brightness of luminescent fiber)

[0073] A blue electroluminescent fiber, the preparation method thereof has the following steps:

[0074] (1) Preparation of the light-emitting layer by electrospinning: First, N,N-dimethylformamide and acetone (mass ratio 1.5:1) were mixed as solvents to prepare a polyvinylidene fluoride-hexafluoropropylene solution with a solid content of 10%, and then ZnS:Cu luminescent powder was added to the polyvinylidene fluoride-hexafluoropropylene solution and mixed, and the mixture was stirred evenly to obtain a luminescent spinning solution. Luminescent spinning solutions with a mass ratio of 1:1, 2:1, 3:1, and 4:1 of electroluminescent material ZnS:Cu luminescent powder to polymer polyvinylidene fluoride-hexafluoropropylene were prepared respectively, and electrospinning was performed using luminescent spinning solutions of different ratios. The electroluminescent material was loaded onto the surface of the silver-plated nylon fiber by electrospinning, and the spinning process parameters were: flow rate 0.5mL / hr, rotation speed 190rpm, and moving speed 1.4mm / s.

[0075] (2) Preparation of dielectric layer by dip coating: Prepare a PDMS dilution solution composed of PDMS and n-hexane in a mass ratio of 1:2.5, immerse the fiber in the PDMS dilution solution, then slowly pull it out at a uniform speed, and dry it at 100°C for 20 min to obtain a uniformly loaded dielectric layer.

[0076] (3) Construction of external electrode: Copper wire (diameter 0.05 mm) was wound around the dielectric layer at a pitch of 0.4 mm, and then plasma treated (100 W, 2 min). The fiber was then immersed in a silver nanowire dispersion for 10 s, taken out and dried at 80 °C. After repeating this process 5 times, a uniformly distributed silver nanowire external electrode was formed on the surface of the dielectric layer.

[0077] (4) Insulation packaging: Silicone resin is coated on the outside of the electroluminescent fiber and dried at 100°C for 30 minutes to obtain a transparent packaging layer.

[0078] No color conversion layer was added during the preparation process. After applying an AC driving voltage, it exhibits blue light (only the ZnS:Cu luminescent powder emits light, and color conversion is not achieved). It can still work stably and normally after bending, compression, and washing.

[0079] The brightness of the luminescent fiber was tested when the mass ratio of electroluminescent material ZnS:Cu luminescent powder to polymer polyvinylidene fluoride-hexafluoropropylene was 1:1, 2:1, 3:1, and 4:1. The results are shown in Figure 6 .from Figure 6 The data show that the brightness of the luminescent fiber is the highest when the preparation condition of electroluminescent material: polymer = 3:1.

[0080] Comparative Example 1 (External Electrode without Wrapped Metal Wire)

[0081] The difference from Example 2 is: (4) Construction of external electrode: the fiber loaded with the dielectric layer is first subjected to plasma treatment (100 W, 2 min), and then immersed in a silver nanowire dispersion for 10 s, taken out and dried at 80°C, and after repeating 5 times, a uniformly distributed silver nanowire external electrode is formed on the surface of the dielectric layer.

[0082] The prepared electroluminescent fiber did not have a metal wire outer electrode wrapped around it during the preparation process. It showed green light after applying an AC driving voltage. However, since the continuous conductive layer formed by the silver nanowire as a single outer electrode was not stable enough, it was easily disconnected during bending, compression, and washing, resulting in failure of the electroluminescent fiber. If the metal wire outer electrode was not wrapped around it during the preparation process, the prepared electroluminescent fiber would have poor stability and could not meet the needs of taking it.

[0083] Comparative Example 2 (without dielectric layer)

[0084] The difference from Example 2 is that after the color conversion layer is prepared by dip-dyeing, the dielectric layer is not loaded, and the external electrode is directly constructed to prepare the electroluminescent fiber.

[0085] The prepared electroluminescent fiber has no dielectric layer, and there is no dielectric layer protection between the inner and outer electrodes, resulting in poor device stability. When the device is working, it is easy to break down, causing the inner and outer electrodes to be connected, resulting in a short circuit of the device, and causing the electroluminescent fiber to fail. If the dielectric layer is not loaded during the preparation process, the prepared electroluminescent fiber has poor stability and cannot be prepared in batches.

[0086] Comparative Example 3 (Silver Nanowire Outer Electrode Not Coated)

[0087] The difference from Example 2 is that there is no fluorescent yellow 3G dye color conversion layer; (4) Construction of external electrode: copper wire (diameter 0.05 mm) is wound outside the dielectric layer at a pitch of 0.4 mm.

[0088] The prepared electroluminescent fibers Figure 7 As shown in the figure, the fiber surface is not coated with silver nanowire external electrodes. After applying AC driving voltage, only weak blue light is emitted around the metal wire. Since the conductive area formed by the metal wire as a single external electrode on the fiber surface cannot cover the fiber surface, the uniform light emission of the electroluminescent fiber surface cannot be achieved. If the silver nanowire external electrodes are not coated, the uniform and high-brightness light emission of the fiber cannot be achieved, and the prepared electroluminescent fiber will have no practical application value.

[0089] The method of the present invention broadens the color of the electroluminescent fiber by introducing fluorescent dyes of different colors, and has high application value in the field of smart clothing and pattern decoration. The photo of the embroidered luminous LOGO on the jacket made of the fiber of the present invention is shown in Figure 8 The preparation process is simple, the conditions are mild, the cost is low, and it is suitable for industrial production.

[0090] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.

[0091] The above is a detailed introduction to a multicolor electroluminescent fiber and an electrospinning preparation method thereof provided by the present invention. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, several improvements and modifications can be made to the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing multicolor electroluminescent fibers by electrospinning, characterized in that The method comprises the following steps: (1) Preparation of the light-emitting layer by electrospinning: an electroluminescent material, a solvent and a polymer as a binder are mixed and stirred to obtain a light-emitting spinning solution, and the electroluminescent material is loaded onto the surface of the conductive fiber by electrospinning to obtain a conductive fiber with a light-emitting layer; The electroluminescent material is selected from one or more of zinc sulfide-doped luminescent powders ZnS:Mn, ZnS:Cl, ZnS:Cu, ZnS:Sm, ZnS:Tm, ZnS:Cu,Cl and ZnS:Mn,Cu,Cl, and the mass ratio of the electroluminescent material to the polymer is (1-5):1; (2) Preparation of color conversion layer by dyeing: The conductive fiber with the luminescent layer is dipped into a fluorescent dye solution to dye the fiber surface, and then dried to form a color conversion layer; (3) Dip-coating to prepare the dielectric layer: The conductive fiber dyed with fluorescent dye is immersed in the PDMS dilution solution, then slowly pulled out at a uniform speed, and dried to obtain a uniformly loaded dielectric layer; The PDMS diluent is a mixture of PDMS and n-hexane in a mass ratio of 1: (1-5); (4) constructing an external electrode: loading the external electrode on the surface of the dielectric layer by winding or coating to obtain an electroluminescent fiber; (5) Insulation packaging: A transparent insulating polymer is coated on the outside of the electroluminescent fiber, and after drying, a multi-color electroluminescent fiber with a transparent packaging layer as the outermost layer is obtained.

2. The preparation method according to claim 1, characterized in that: In step (1), The conductive fiber includes one or more of metal conductive fiber, metal particle plated chemical fiber, carbon fiber, ion gel fiber, and conductive polymer composite fiber; The particle size of the electroluminescent material is 10 to 50 μm; The solvent is a mixture of N,N-dimethylformamide and acetone in a mass ratio of (1-2):1; The polymer is selected from one of styrene-butadiene-styrene, polyurethane, and polyvinylidene fluoride-hexafluoropropylene.

3. The preparation method according to claim 1, characterized in that: In step (1), the steps of preparing the luminescent spinning solution are: firstly preparing the polymer into a polymer solution with a solid content of 10% to 20%, then adding the electroluminescent material, and mixing them evenly to obtain the luminescent spinning solution.

4. The preparation method according to claim 1, characterized in that: In step (1), the process parameters of electrospinning are: flow rate 0.3-1.5 mL / hr, rotation speed 140-260 rpm, and moving speed 0.5-2.5 mm / s.

5. The preparation method according to claim 1, characterized in that: In step (2), the fluorescent dye is one or more of cyanine dyes, rhodamine dyes, fluorescein dyes, coumarins and their derivatives, benzanthrone dyes, nelcarboxylic acid derivatives, anthraquinone derivatives, and naphthoquinone derivatives.

6. The preparation method according to claim 1, characterized in that: In step (2), the drying conditions are: temperature 60-100° C., time 5-10 min; in step (3), the drying conditions are: temperature 80-120° C., time 15-30 min.

7. The preparation method according to claim 1, characterized in that: In step (4), the external electrode includes metal wire or metal particles, the metal wire includes silver wire, copper wire, silver-plated copper wire, steel wire, titanium wire or tungsten wire, and the metal particles include conductive silver paste, silver nanowire, copper nanowire or silver nanowire.

8. The preparation method according to claim 1, characterized in that: When the outer electrode is prepared by winding method, the pitch is 0.2 to 0.8 mm; When the coating method is used to load the external electrode, the surface of the dielectric layer needs to be plasma treated to improve the hydrophilicity. The plasma treatment power is 100-150W, the treatment time is 1-5min, and then the conductive solution is dipped for 5-30s and 2-5 times. After dipping, it is dried in an oven at a temperature of 60-150°C.

9. The preparation method according to claim 1, characterized in that: In step (5), the insulating polymer is one or more of epoxy resin, acrylate resin, polyurethane resin, polytetrafluoroethylene resin, polyvinylidene fluoride resin or silicone resin; the drying conditions are: temperature 80-150° C., time 20-40 min.

10. A multicolor electroluminescent fiber prepared by the preparation method according to claim 1, characterized in that: The multicolor electroluminescent fiber comprises conductive fiber, luminescent layer, color conversion layer, dielectric layer and packaging layer from inside to outside. The outer surface of the dielectric layer is wound or coated with an external electrode, which is a metal wire or metal particle.

Citation Information

Patent Citations

  • Electroluminescent color-changing fiber as well as preparation method and application thereof

    CN114892392A

  • Multi-color flexible wearable electroluminescent device and preparation method thereof

    CN116997225A

  • Textile fabric structure from an arrangement of a large number of conductive threads or threads having conductive properties, and method for their production

    DE10333583A1

  • Method for determining a location and electronic device supporting the same

    KR1020230048839A

Cited By

  • Preparation method of electroluminescent fiber and auxiliary communication electroluminescent device prepared from electroluminescent fiber

    CN120273052A

  • High-performance luminescent fiber driven by safe voltage and preparation method of high-performance luminescent fiber

    CN120465167A