Polyhedral oligomeric silsesquioxane-based electrostatic spinning fiber as well as preparation method and application thereof

By optimizing the mixing method and concentration of POSS and polymer, the problem of insufficient fiber performance in traditional electrospinning technology is solved, and a large number of fibers with excellent mechanical properties and heat resistance are prepared, expanding their application range.

CN118932528APending Publication Date: 2024-11-12HEZE UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411139641.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The fibers prepared by traditional electrospinning technology have shortcomings in strength, stability and functionalization, and the compatibility and proportion optimization of POSS with polymers are challenging issues.

Method used

By optimizing the usage ratio of POSS and the mixing method with polymer, electrospinning fibers with excellent properties are prepared, including adjusting the concentration of POSS and polymer, selecting suitable organic solvents and mixing methods, and electrospinning to obtain a surface Smooth, uniform diameter pure POSS and POSS-polymer composite fibers.

Benefits of technology

It significantly improves the strength, heat resistance and chemical stability of the fibers, expands the application scope of electrospinning technology, solves the problems of solubility and compatibility, realizes the preparation of high-quality fibers, and has broad application potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932528A_ABST
    Figure CN118932528A_ABST
Patent Text Reader

Abstract

The invention relates to a polyhedral oligomeric silsesquioxane (POSS)-based electrostatic spinning fiber as well as a preparation method and application thereof, and belongs to the field of high-performance functional materials. According to the preparation method, a pure POSS spinning solution and a POSS-polymer blended spinning solution are respectively prepared by selecting a proper solvent, and pure POSS fibers and POSS-polymer composite fibers which are smooth in surface and uniform in diameter are successfully prepared through electrostatic spinning. The POSS-based electrostatic spinning fiber provided by the invention not only has simple preparation method steps and easily controlled preparation conditions, but also has the characteristics of good heat resistance, excellent hydrophobicity and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of high-performance functional materials, and in particular to an electrospinning fiber based on polyhedral oligomeric silsesquioxane and a preparation method and application thereof, which is mainly used in the fields of filter materials, thermal insulation materials, electronic devices, etc. Background Art

[0002] Electrospinning technology has been widely used in various fields in recent years due to its advantages of simplicity, high efficiency and ability to produce nano-scale fibers. Its main applications include filtration materials, tissue engineering scaffolds, drug release systems and high-performance composite materials. However, the fibers prepared by traditional electrospinning technology still have certain limitations in certain properties, such as strength, stability and functionality, and innovative materials and processes are urgently needed to improve their performance. Polyhedral oligomeric silsesquioxane (POSS) is a class of organosilicon compounds with unique structure and excellent properties, and its application prospects in materials science are broad. POSS has a molecular framework similar to a cage structure, which not only gives the material extremely high thermal stability and chemical stability, but also can significantly improve the mechanical properties, anti-aging properties and optical properties of the material. Therefore, the application of POSS in electrospinning technology is expected to solve the shortcomings of traditional fiber materials in performance and open up new application areas. At present, the application research of POSS in electrospinning is still in the exploratory stage. In the prior art, electrospinning solution usually uses polymer solution, and the use of POSS alone or mixed with polymer can effectively improve the overall performance of electrospun fibers. Due to its high viscosity and strong chemical stability, pure POSS solution can form a stable fiber structure during the electrospinning process, thereby improving the strength and stability of the fiber. However, the electrospinning of pure POSS may face problems such as difficulty in fiber formation and uneven fiber diameter. On the other hand, blending POSS with other polymers can combine the advantages of both to prepare composite fibers with better performance. The combination of POSS and polymers can improve the mechanical properties and functional characteristics of fibers, while improving the processability and stability of fibers. However, the compatibility, ratio and optimization of electrospinning process conditions of POSS and polymers remain challenging research topics. Summary of the invention

[0003] Under this background, the present invention proposes a kind of electrostatic spinning fiber based on POSS and preparation method thereof, considers the use of two kinds of electrostatic spinning solutions of pure POSS and POSS-polymer. By optimizing the use ratio of POSS and the mixing mode with polymer, some problems in traditional electrostatic spinning technology can be effectively solved, and fiber with excellent performance is prepared. These novel fibers not only excel in mechanical properties, thermal stability and chemical tolerance, but also have a wide range of application potentials, including high-performance filter materials, medical dressings and composite materials, etc.

[0004] The innovation of the present invention is that by optimizing POSS and its mixture with polymers, the application scope of electrospinning technology is expanded, and the performance and function of the fiber are improved, providing a new research direction and practical application solution for the field of materials science.

[0005] The present invention aims to provide a novel electrospinning fiber based on polyhedral oligomeric silsesquioxane and preparation method thereof, to improve the functionality and application range of electrospinning fiber. Specifically, the present invention firstly, POSS is dissolved in an organic solvent, the concentration of POSS in the solution is continuously adjusted, electrospinning is performed, and a spinning solution that can obtain a better POSS fiber morphology is selected for standby. Secondly, a polymer is dissolved in a suitable organic solvent, the concentration of the polymer in the solution is continuously adjusted, electrospinning is performed, and a spinning solution that can obtain a better polymer fiber morphology is selected for standby. Finally, a suitable mixing method is selected to mix the above two spinning solutions into a POSS-polymer blend solution, electrospinning is performed, and for the obtained POSS-polymer fiber morphology, the concentration of the blend solution POSS and the polymer is fine-tuned and corrected, and electrospinning is performed again to obtain a POSS-polymer composite fiber.

[0006] The preparation method based on POSS electrostatic spinning fiber provided by the present invention has simple steps, and the preparation conditions are easy to control, and not only can pure POSS electrostatic spinning fiber with smooth surface and uniform diameter be prepared, but also POSS-polymer composite fiber is prepared by optimizing the combination mode of POSS and polymer. The composite fiber solves the solubility and compatibility problems existing in the prior art, and exhibits performance characteristics such as higher strength, good heat resistance, superior chemical stability and hydrophobicity.

[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions: The invention provides a POSS-based electrospinning fiber, which comprises a pure POSS-organic solvent (I) spinning solution and a POSS-organic solvent (I) and a polymer-organic solvent (II) blended spinning solution, and pure POSS fiber and POSS-polymer composite fiber are prepared by electrospinning.

[0008] According to the above scheme, the concentration (w / v) of POSS in the mixed solution of POSS and organic solvent (I) is 0.1~3 g / mL, preferably 0.2~2 g / mL; the concentration (w / v) of the polymer in the mixed solution of polymer and organic solvent (II) is 0.05~1 g / mL, preferably 0.1~0.6 g / mL.

[0009] Further, the POSS is a polysilsesquioxane with long-chain organic groups around the molecule. Preferably, POSS refers to a polysilsesquioxane in which one or more of the following formulas A, B, C, D, E, F and G are mixed in any proportion, and the POSS refers to a polysilsesquioxane in which the peripheral organic groups in the molecular structure simultaneously contain phenyl and acryloyloxy, phenyl and epoxy, phenyl and isocyanate, phenyl and mercapto, phenyl and amino, phenyl and phosphaphenanthryl, phosphaphenanthryl and acryloyloxy, phosphaphenanthryl and epoxy, phosphaphenanthryl and isocyanate, phosphaphenanthryl and mercapto, phosphaphenanthryl and amino, or the POSS refers to a polysilsesquioxane in which the peripheral organic groups in the molecular structure only contain one of acryloyloxy, epoxy, isocyanate, mercapto, amino, and phosphaphenanthryl groups, and the molecule is composed of an internally stable Si-O-Si structure and organic groups around it, mainly including cage-shaped polysilsesquioxanes, random polysilsesquioxanes and ladder-shaped polysilsesquioxanes. The detailed structure of the preferred POSS is as follows: ; Where R is R 1 or R 2 , and R in substances A, B, C, D, E, F, and G cannot all be R 2 The phenyl group in R 1 , R 2 And the X structure is as follows: .

[0010] Furthermore, the polymer is a soluble or fusible high molecular material. Preferably, the polymer is a polymer selected from the group consisting of polymethyl methacrylate, polyurethane, polylactic acid, polycaprolactam, polyvinyl alcohol, polystyrene, polyethylene terephthalate, and polypropylene, mixed in any proportion.

[0011] Furthermore, the organic solvent (I) is an organic solvent selected from the group consisting of methanol, ethanol, dichloromethane, dichloroethane, acetone, tetrachloroethane, chlorobenzene, cyclohexanone, formic acid, tetrahydrofuran, dimethylformamide, dimethylacetamide, and propylene oxide, mixed in any proportion.

[0012] Furthermore, the organic solvent (II) is an organic solvent selected from the group consisting of methanol, ethanol, dichloromethane, dichloroethane, acetone, tetrachloroethane, chlorobenzene, cyclohexanone, formic acid, tetrahydrofuran, dimethylformamide, dimethylacetamide, and propylene oxide, mixed in any proportion.

[0013] A preparation method for electrospinning fiber materials based on polyhedral oligomeric silsesquioxane, the specific preparation steps are: Step 1: firstly place POSS in an organic solvent (Ⅰ), stir and mix until the mixture is uniform and transparent, and obtain a pure POSS-organic solvent (Ⅰ) spinning solution; Step 2: Use a syringe to absorb the prepared pure POSS-organic solvent (Ⅰ) spinning solution for electrospinning; Step 3: Continuously adjust the parameters of the electrospinning process until pure POSS electrospinning fibers with smooth surface and uniform diameter are obtained; Step 4: firstly placing the polymer in an organic solvent (II), stirring and mixing until the mixture is uniform and transparent, and obtaining a polymer-organic solvent (II) spinning solution; Step 5: Use a syringe to absorb the prepared polymer-organic solvent (II) spinning solution for electrospinning.

[0014] Step 6: Continuously adjust the parameters of the electrospinning process until a polymer fiber with a smooth surface and uniform diameter is obtained; Step 7: Prepare spinning solution with the concentration obtained in step 3 and step 6, stir and mix to form POSS-polymer blend solution, perform electrospinning, fine-tune and correct the concentration of POSS and polymer in the blend solution according to the morphology of the obtained POSS-polymer fiber, and perform electrospinning again until a POSS-polymer composite fiber with better morphology is obtained.

[0015] In step 1, step 4 and step 7, the stirring speed is 300-1000 rpm, the stirring temperature is 15-80° C., and the stirring time is 10-120 min; In step 1, step 4 and step 7, if the ideal spinning solution is not obtained after stirring and mixing, an ultrasonic instrument can be used to accelerate the dissolution, the ultrasonic temperature is 20 to 60° C., and the ultrasonic time is 10 to 120 min; In each of the above steps, the spinning solution before electrospinning needs to be vacuumed and bubbled, and the vacuum degree of the vacuuming reaches -0.01 to -0.09 MPa; In each of the above steps, when the electrospinning equipment is used for electrospinning, the propulsion speed of the syringe pump is 0.5-4 mL / h, the inner diameter of the spinning needle is a flat needle with an inner diameter of 0.1-2.5 mm, the high-voltage DC power supply is 6-22 kV, the distance between the spinning needle and the drum is 5-25 cm, and the drum speed is 100-800 rpm; In the above steps, when electrospinning is performed using an electrospinning device, the electrospinning fiber collection time is 1 to 6 hours, and the obtained white ultrafine fiber membrane with a certain thickness is dried at a drying temperature of 20 to 40° C. for a drying time of 4 to 24 hours.

[0016] Beneficial Effects 1) Improved functionality: By using POSS (polyhedral oligomeric silsesquioxane) as the main component of electrospun fibers, the strength, heat resistance and chemical stability of the fibers can be significantly improved. This fiber has excellent hydrophobicity, making it perform well in special application scenarios such as waterproofing and oil repellency.

[0017] 2) Simple preparation method: The present invention provides a simple preparation method with clear steps and easy operation. By adjusting the concentration and mixing method of POSS and polymer, high-quality fibers can be obtained under controlled conditions, greatly reducing process complexity and production costs.

[0018] 3) Optimized performance: Through the rational blending of pure POSS and POSS-polymer and the optimization of spinning process, the present invention can prepare pure POSS fibers and POSS-polymer composite fibers with excellent surface smoothness and diameter uniformity. These fibers show better performance in practical applications, such as higher mechanical strength and heat resistance.

[0019] 4) Solving technical problems: ① The present invention realizes the preparation of pure POSS fiber. ② The present invention solves the solubility and compatibility problems of POSS in traditional technology and realizes the effective combination of POSS and polymer. Thus, the performance bottleneck existing in the prior art is overcome and the comprehensive performance of the fiber is improved.

[0020] In summary, the present invention not only broadens the application scope of electrospun fibers, but also provides new ideas and methods for material research and development in related fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a digital photo of the phenyl-acryloxy POSS fiber membrane in Example 1 of the present invention.

[0022] Figure 2 This is a scanning electron microscope image of the phenyl-acryloxy POSS fiber in Example 1 of the present invention.

[0023] Figure 3This is a scanning electron microscope image of the primary phenyl-acryloxy POSS-polymethyl methacrylate composite fiber in Example 1 of the present invention.

[0024] Figure 4 This is a scanning electron microscope image of the phenyl-acryloxy POSS-polymethyl methacrylate composite fiber in Example 1 of the present invention.

[0025] Figure 5 This is a scanning electron microscope image of the phenyl-epoxy POSS fiber in Example 2 of the present invention.

[0026] Figure 6 This is a scanning electron microscope image of the phenyl-epoxy POSS-polyvinyl alcohol composite fiber in Example 2 of the present invention. DETAILED DESCRIPTION

[0027] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] Example 1 1) First, add 18 mL of dichloromethane into a mixing kettle, set the stirring speed to 400 rpm, and the stirring temperature to 25 °C. Then, slowly add 20 g of POSS containing both phenyl and acryloyloxy groups (hereinafter referred to as phenyl-acryloyloxy POSS, the detailed structure is shown in the formula below) into the mixing kettle, and stir for 20 min until a uniform and transparent phenyl-acryloyloxy POSS spinning solution is obtained. The spinning solution is vacuumed and then electrospinning is performed.

[0029] 2) A micro-injection pump is used to control the injection speed of the spinning solution, and aluminum foil is used as a collecting screen. The propulsion speed of the injection pump is 0.8 mL / h, the inner diameter of the spinning needle is 0.5 mm, the high-voltage DC power supply is 20 kV, the distance between the spinning needle and the drum is 20 cm, and the drum speed is 200 rpm. The spinning solution is sprayed into filaments under the action of the high-voltage electric field and attached to the collecting screen. After 2 hours, a fiber membrane of a certain thickness can be collected on the aluminum foil. The obtained fiber membrane is dried at a drying temperature of 30 ° C and a drying time of 4 hours. Figure 1 This is a digital photo of the phenyl-acryloxy POSS fiber membrane prepared in this example. Figure 2 The SEM image of the phenyl-acryloxy POSS fiber prepared in this example is Figure 1 and Figure 2The fiber morphology proves that the present invention can prepare pure phenyl-acryloxy POSS electrospun fibers with smooth surface and uniform thickness.

[0030] 3) First, add 100mL of tetrahydrofuran and N,N-dimethylformamide (1:1, v / v) mixed solvent into the mixing kettle, set the stirring speed to 500rpm, the stirring temperature to 30℃, and then slowly add 20g of polymethyl methacrylate with a weight average molecular weight of 70000g / mol into the mixing kettle, stirring for 50min, and obtain the primary spinning solution. The primary spinning solution is further subjected to ultrasonic treatment at a temperature of 25℃ and a time of 20min until a uniform and transparent polymethyl methacrylate spinning solution is obtained, and the spinning solution is vacuumed and then electrospinning is performed.

[0031] 4) The propulsion speed of the injection pump is 2.5mL / h, the inner diameter of the spinning needle is 1.26mm, the high-voltage DC power supply is 15kV, the distance between the spinning needle and the drum is 15cm, and the drum speed is 500rpm. The spinning solution is sprayed into filaments under the action of the high-voltage electric field and attached to the collecting screen. After 4 hours, a fiber membrane of a certain thickness can be collected on the aluminum foil. The obtained fiber membrane is dried at a drying temperature of 25°C and a drying time of 10 hours, and finally a polymethyl methacrylate fiber with a good morphology is obtained.

[0032] 5) Take equal mass (20g) of spinning solutions of the concentrations obtained in 1) and 3) respectively, stir and mix to form a uniform and transparent phenyl-acryloyloxy POSS-polymethyl methacrylate blend solution, the stirring speed is 400rpm, the stirring temperature is 30℃, the stirring time is 20min, and the primary spinning solution is obtained. The obtained primary spinning solution is then subjected to ultrasonic treatment, the ultrasonic temperature is 25℃, and the ultrasonic time is 10min. After vacuum treatment, electrospinning is carried out, the propulsion speed of the injection pump is 1.5mL / h, the inner diameter of the spinning needle is 1.07mm, the high-voltage DC power supply is 15kV, the distance between the spinning needle and the drum is 15cm, and the drum speed is 500rpm. The spinning solution is sprayed into filaments under the action of the high-voltage electric field and attached to the collecting screen. After 2 hours, a fiber membrane of a certain thickness can be collected on the aluminum foil. Figure 3 This is a SEM photo of the primary phenyl-acryloxy POSS-polymethyl methacrylate composite fiber prepared in this example. In view of the morphology of the obtained composite fiber, 4 g of phenyl-acryloxy POSS was added to the spinning solution of the concentration obtained in 1) and 3) of equal mass (20 g), mixed, ultrasonicated, and vacuumed, and then electrospun again until a phenyl-acryloxy POSS-polymethyl methacrylate composite fiber with a good morphology was obtained. Figure 4 The SEM photo of the composite fiber prepared in this example is Figure 4The fiber morphology proves that the present invention can prepare phenyl-acryloxy POSS-polymethyl methacrylate composite fibers with smooth surface and uniform thickness.

[0033] Example 2 1) First, add 40 mL of dichloromethane into the mixing kettle, set the stirring speed to 400 rpm, and the stirring temperature to 30 °C. Then, slowly add 20 g of POSS containing both phenyl and epoxy groups (hereinafter referred to as phenyl-epoxy POSS, the detailed structure is shown in the formula below) into the mixing kettle, and stir for 30 min until a uniform and transparent phenyl-epoxy POSS spinning solution is obtained. After the spinning solution is vacuumed, electrospinning is performed.

[0034] ; 2) A micro-injection pump is used to control the injection speed of the spinning solution, and aluminum foil is used as a collecting screen. The propulsion speed of the injection pump is 1 mL / h, the inner diameter of the spinning needle is 0.5 mm, the high-voltage DC power supply is 20 kV, the distance between the spinning needle and the drum is 20 cm, and the drum speed is 200 rpm. The spinning solution is sprayed into filaments under the action of the high-voltage electric field and attached to the collecting screen. After 2.5 hours, a fiber membrane of a certain thickness can be collected on the aluminum foil. The obtained fiber membrane is dried at a drying temperature of 30 ° C and a drying time of 5 hours. Figure 5 The SEM image of the phenyl-epoxy POSS fiber prepared in this example is Figure 5 The fiber morphology proves that the present invention can produce pure phenyl-epoxy POSS electrospun fibers with smooth surface and uniform thickness.

[0035] 3) First, add 100 mL of methanol solvent into the mixing kettle, set the stirring speed to 600 rpm and the stirring temperature to 40°C, then slowly add 10 g of polyvinyl alcohol with a weight average molecular weight of 88,000 g / mol into the mixing kettle, and stir for 100 min to obtain a primary spinning solution. The primary spinning solution is further subjected to ultrasonic treatment at a temperature of 25°C and a time of 30 min until a uniform and transparent polyvinyl alcohol spinning solution is obtained, and the spinning solution is vacuumed and then subjected to electrospinning.

[0036] 4) The propulsion speed of the injection pump is 1mL / h, the inner diameter of the spinning needle is 1.26mm, the high-voltage DC power supply is 15kV, the distance between the spinning needle and the drum is 15cm, and the drum speed is 400rpm. The spinning solution is sprayed into filaments under the action of the high-voltage electric field and attached to the collecting screen. After 4 hours, a fiber membrane of a certain thickness can be collected on the aluminum foil. The obtained fiber membrane is dried at a drying temperature of 25°C and a drying time of 10 hours, and finally a polyvinyl alcohol fiber with a good morphology is obtained.

[0037] 5) Take 30g and 10g of the spinning solution of the concentration obtained in 1) and 3) respectively, stir and mix to form a uniform and transparent phenyl-epoxy POSS-polyvinyl alcohol blend solution, the stirring speed is 400rpm, the stirring temperature is 30℃, the stirring time is 40min, and the primary spinning solution is obtained. The obtained primary spinning solution is then subjected to ultrasonic treatment, the ultrasonic temperature is 25℃, and the ultrasonic time is 15min. After vacuum treatment, electrospinning is carried out, the propulsion speed of the injection pump is 1.5mL / h, the inner diameter of the spinning needle is 1.07mm, the high-voltage DC power supply is 15kV, the distance between the spinning needle and the drum is 15cm, and the drum speed is 500rpm. The spinning solution is sprayed into filaments under the action of the high-voltage electric field and attached to the collecting screen. After 2 hours, a fiber membrane of a certain thickness can be collected on the aluminum foil. Figure 6 The SEM photo of the composite fiber prepared in this example is Figure 6 The fiber morphology proves that the present invention can produce phenyl-epoxy POSS-polyvinyl alcohol composite fibers with smooth surface and uniform thickness.

[0038] Example 3 1) First, 50 mL of dichloromethane was added into the mixing kettle, and the stirring speed was set to 400 rpm and the stirring temperature was set to 25 °C. Then, 20 g of POSS containing both phosphaphenanthryl and acryloyloxy groups (referred to as phosphaphenanthryl-acryloyloxy POSS, with detailed structure as shown in the formula below) was slowly added into the mixing kettle. The stirring time was 20 min until a uniform and transparent phosphaphenanthryl-acryloyloxy POSS spinning solution was obtained. The spinning solution was vacuumed and then electrospinning was performed.

[0039] ; A micro-injection pump is used to control the injection speed of the spinning solution, and aluminum foil is used as a collecting screen. The propulsion speed of the injection pump is 0.8 mL / h, the inner diameter of the spinning needle is 0.67 mm, the high-voltage DC power supply is 20 kV, the distance between the spinning needle and the drum is 20 cm, and the drum speed is 200 rpm. The spinning solution is sprayed into filaments under the action of a high-voltage electric field and attached to the collecting screen. After 2 hours, a fiber membrane of a certain thickness can be collected on the aluminum foil. The obtained fiber membrane is dried at a drying temperature of 30 ° C and a drying time of 3 hours.

[0040] 3) First, add 100mL of N,N-dimethylformamide into the mixing kettle, set the stirring speed to 500rpm and the stirring temperature to 30℃, then slowly add 20g of polymethyl methacrylate with a weight average molecular weight of 70000g / mol into the mixing kettle, and stir for 50min to obtain the primary spinning solution. The primary spinning solution is further subjected to ultrasonic treatment at a temperature of 25℃ and a time of 20min until a uniform and transparent polymethyl methacrylate spinning solution is obtained, and the spinning solution is vacuumed and then electrospinning is performed.

[0041] 4) The propulsion speed of the injection pump is 2.5mL / h, the inner diameter of the spinning needle is 1.26mm, the high-voltage DC power supply is 15kV, the distance between the spinning needle and the drum is 15cm, and the drum speed is 500rpm. The spinning solution is sprayed into filaments under the action of the high-voltage electric field and attached to the collecting screen. After 4 hours, a fiber membrane of a certain thickness can be collected on the aluminum foil. The obtained fiber membrane is dried at a drying temperature of 25°C and a drying time of 10 hours, and finally a polymethyl methacrylate fiber with a good morphology is obtained.

[0042] 5) Take 10g and 30g of the spinning solution of the concentration obtained in 1) and 3) respectively, stir and mix to form a uniform and transparent phosphaphenanthryl-acryloyloxy POSS-polymethyl methacrylate blend solution, the stirring speed is 400rpm, the stirring temperature is 30℃, the stirring time is 20min, and the spinning solution is obtained. The obtained spinning solution is then subjected to ultrasonic treatment, the ultrasonic temperature is 25℃, and the ultrasonic time is 10min. After vacuum treatment, electrospinning is carried out, the propulsion speed of the injection pump is 1.5mL / h, the inner diameter of the spinning needle is 1.07mm, the high-voltage DC power supply is 15kV, the distance between the spinning needle and the drum is 15cm, and the drum speed is 500rpm. The spinning solution is sprayed into filaments under the action of the high-voltage electric field and attached to the collecting screen. After 2 hours, a composite fiber membrane of a certain thickness can be collected on the aluminum foil.

[0043] The test results of thermal stability (nitrogen atmosphere) and water contact angle of fiber materials in various embodiments are shown in the following table: It can be seen from the analysis results of Examples 1 to 3 that the pure POSS fibers and POSS-polymer composite fibers prepared in the present invention not only have a stable morphology with a smooth surface and uniform diameter, but also exhibit excellent heat resistance, good hydrophobicity and chemical stability.

[0044] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A POSS electrospinning fiber material, characterized in that: The method comprises a pure POSS-organic solvent (Ⅰ) spinning solution and a POSS-organic solvent (Ⅰ) and polymer-organic solvent (Ⅱ) blended spinning solution, and pure POS fiber and POSS-polymer composite fiber are prepared by electrospinning respectively.

2. A POSS electrospinning fiber material according to claim 1, characterized in that: The concentration (w / v) of POSS in the mixed solution of POSS and organic solvent (I) is 0.1-3 g / mL, preferably 0.2-2 g / mL; the concentration (w / v) of the polymer in the mixed solution of the polymer and organic solvent (II) is 0.05-1 g / mL, preferably 0.1-0.6 g / mL.

3. The material according to claim 1 or 2, characterized in that: The POSS is a molecule with a fixed structural skeleton composed of an internally stable Si-O-Si structure and surrounding organic groups, and contains a certain amount of long-chain organic groups around the molecule.

4. The material according to claim 3, characterized in that: The POSS mainly includes cage-shaped polysilsesquioxane, random polysilsesquioxane and ladder-shaped polysilsesquioxane; in its molecular structure, the peripheral organic groups simultaneously contain phenyl and acryloxy, phenyl and epoxy, phenyl and isocyanate, phenyl and mercapto, phenyl and amino, phenyl and phosphaphenanthryl, phosphaphenanthryl and acryloxy, phosphaphenanthryl and epoxy, phosphaphenanthryl and isocyanate, phosphaphenanthryl and mercapto, phosphaphenanthryl and amino polysilsesquioxane, or the POSS refers to a polysilsesquioxane in which the peripheral organic groups in the molecular structure only contain one of acryloxy, epoxy, isocyanate, mercapto, amino, and phosphaphenanthryl groups. The detailed structure of the POSS is as follows: ; Wherein, R is R1 or R2, and R in substances A, B, C, D, E, F and G cannot all be phenyl in R2, and the structures of R1, R2 and X are as follows: 。 5. The material according to claim 1 or 2, characterized in that: The polymer is a soluble or fusible high molecular material, including: a polymer selected from polymethyl methacrylate, polyurethane, polylactic acid, polycaprolactam, polyvinyl alcohol, polystyrene, polyethylene terephthalate, and polypropylene mixed in any proportion.

6. The material according to claim 1 or 2, characterized in that: The organic solvent (I) is one or more of methanol, ethanol, dichloromethane, dichloroethane, acetone, tetrachloroethane, chlorobenzene, cyclohexanone, formic acid, tetrahydrofuran, dimethylformamide, dimethylacetamide, and propylene oxide, mixed in any proportion.

7. The material according to claim 1 or 2, characterized in that: The organic solvent (II) is an organic solvent selected from the group consisting of methanol, ethanol, dichloromethane, dichloroethane, acetone, tetrachloroethane, chlorobenzene, cyclohexanone, formic acid, tetrahydrofuran, dimethylformamide, dimethylacetamide, and propylene oxide, mixed in any proportion.

8. A method for preparing the material according to claim 1 or 2, characterized in that: The specific preparation steps are: Step 1: firstly place POSS in an organic solvent (Ⅰ), stir and mix until the mixture is uniform and transparent, and obtain a pure POSS-organic solvent (Ⅰ) spinning solution; Step 2: Use a syringe to absorb the prepared pure POSS-organic solvent (Ⅰ) spinning solution for electrospinning; Step 3: Continuously adjust the parameters of the electrospinning process until pure POSS electrospinning fibers with smooth surface and uniform diameter are obtained; Step 4: firstly placing the polymer in an organic solvent (II), stirring and mixing until the mixture is uniform and transparent, and obtaining a polymer-organic solvent (II) spinning solution; Step 5: Use a syringe to absorb the prepared polymer-organic solvent (II) spinning solution for electrospinning; Step 6: Continuously adjust the parameters of the electrospinning process until a polymer fiber with a smooth surface and uniform diameter is obtained; Step 7: Prepare spinning solution with the concentration obtained in step 3 and step 6, stir and mix to form POSS-polymer blend solution, perform electrospinning, fine-tune and correct the concentration of POSS and polymer in the blend solution according to the morphology of the obtained POSS-polymer fiber, and perform electrospinning again until a POSS-polymer composite fiber with better morphology is obtained.

9. The method according to claim 8, characterized in that: In step 1, step 4 and step 7, the stirring speed is 300-1000 rpm, the stirring temperature is 15-80° C., and the stirring time is 10-120 min; In step 1, step 4 and step 7, if the ideal spinning solution is not obtained after stirring and mixing, an ultrasonic instrument is used to accelerate the dissolution, the ultrasonic temperature is 20 to 60° C., and the ultrasonic time is 10 to 120 min.

10. The method according to claim 8, characterized in that: The spinning solution before electrospinning is subjected to vacuum bubbling treatment, wherein the vacuum degree of the vacuum bubbling treatment reaches -0.01 to -0.09 MPa; When electrospinning is performed using an electrospinning device, the propulsion speed of the syringe pump is 0.5 to 4 mL / h, the inner diameter of the spinning needle is a flat needle with an inner diameter of 0.1 to 2.5 mm, the high-voltage DC power supply is 6 to 22 kV, the distance between the spinning needle and the drum is 5 to 25 cm, and the drum speed is 100 to 800 rpm; When electrospinning is performed using an electrospinning device, the electrospinning fiber collection time is 1 to 6 hours, and the obtained white ultrafine fiber membrane is dried at a drying temperature of 20 to 40° C. for a drying time of 4 to 24 hours.

Citation Information

Cited By

  • High-conductivity carbon nanotube modified polyurethane fiber membrane and preparation method thereof

    CN119571540A