Composite polyamide fiber and preparation method thereof
By using modified cuprous oxide, polydopamine and chitosan quaternary ammonium particles in nylon fibers, the problem of short-lasting antibacterial properties and yellowing resistance of nylon fibers is solved, and the durable antibacterial and light resistance of nylon fibers is achieved. Improves the stability and mechanical strength of the fibers.
Patent Information
- Application Number
- CN202411129116.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The antibacterial properties of nylon fibers are not lasting during use, and long-term exposure to light leads to yellowing and reduced mechanical strength.
Compound nylon fibers are prepared by extrusion and melt spinning using cuprous oxide, polydopamine and chitosan quaternary ammonium particles. Modified cuprous oxide is treated with silane coupling agent, and polydopamine and chitosan quaternary ammonium salts are passed through specific chemistry. The reaction is prepared to form composite fibers with good antibacterial and light resistance.
The long-lasting antibacterial properties and yellowing resistance of composite nylon fibers are achieved, the stability and mechanical strength of the fiber are improved, and the service life of the fiber is extended.
Smart Images

Figure BDA0004997321680000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite fibers, and in particular relates to a composite nylon fiber and a preparation method thereof. Background Art
[0002] As a commonly used fabric in the textile processing field, nylon has strong comprehensive advantages. It is not only skin-friendly and moisture-absorbent, but also has higher wear resistance than all other fibers. It is quick-drying and sun-resistant, and has a low price. It is more in line with people's basic needs for fabrics in today's society, and there are more and more functional improvements on nylon fibers.
[0003] At present, most antibacterial fabrics are obtained by applying antibacterial agents to the fabrics through post-finishing dipping or coating; however, as the use time increases, the antibacterial agents gradually peel off and the antibacterial effect is lost, resulting in the antibacterial performance not lasting. In addition, some nylon fibers are exposed to light for a long time, and the light and heat cause the nylon fibers to break and decompose, eventually leading to yellowing, and their mechanical strength is also reduced. Summary of the invention
[0004] The invention provides a composite nylon fiber and a preparation method thereof, which are used to solve the problem that the nylon fiber has poor antibacterial and yellowing resistance properties.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A composite nylon fiber, characterized in that it is obtained by extruding and melting a fiber masterbatch and spinning it, wherein the raw materials of the fiber masterbatch include cuprous oxide / polydopamine / chitosan quaternary ammonium salt particles and nylon 6 powder; the mass ratio of the cuprous oxide / polydopamine / chitosan quaternary ammonium salt particles to the nylon 6 powder is 1-3:97-99;
[0007] The raw materials of cuprous oxide / polydopamine / chitosan quaternary ammonium salt particles include modified cuprous oxide, polydopamine and chitosan quaternary ammonium salt particles; the mass ratio of cuprous oxide, polydopamine and chitosan quaternary ammonium salt in the cuprous oxide / polydopamine / chitosan quaternary ammonium salt particles is 0.5-2:1:1.
[0008] Furthermore, the modified cuprous oxide is cuprous oxide treated with silane coupling agent KH-550. Cuprous oxide and KH-550 are ultrasonically dissolved in a solution, heated and stirred, centrifuged and washed, and freeze-dried to obtain the modified cuprous oxide, and the mass ratio of KH-550 to cuprous oxide is 1-2.5:97-98.5.
[0009] Furthermore, the cuprous oxide is prepared by glucose reduction method. A certain amount of deionized water is prepared into an alkaline solution (pH=13) with NaOH, then heated, glucose is added and stirred, and then CuSO4·5H2O is added for reaction. Afterwards, the solution is filtered, washed, dried, cooled, and repeatedly ground to obtain cuprous oxide.
[0010] Furthermore, the average particle size of cuprous oxide is 800-1000 nm. If the particle size of cuprous oxide is too large (>1000 nm), it cannot be adapted to fiber processing, and the larger the cuprous oxide particles are, the worse the antibacterial performance is.
[0011] Furthermore, the particle size of the nylon 6 powder is 40-60 mesh, and the bulk density is 0.8 g / mL.
[0012] Furthermore, the polydopamine is prepared by the following steps: levodopa and deionized water are mixed in proportion, a NaOH solution is added to adjust the pH value to 8.5-8.8, potassium ferrate is added, the reaction solution is heated to 90-93°C under stirring, and the reaction is carried out at a constant temperature for 5.5-7h, and the reaction solution is centrifuged, washed, and dried to obtain polydopamine.
[0013] The mass ratio of levodopa to deionized water is 0.2-0.24:100;
[0014] The mass ratio of potassium ferrate to levodopa is 0.8-1.2:3.
[0015] Furthermore, the chitosan quaternary ammonium salt is prepared by the following steps: chitosan, NaOH and isopropanol are added to a round-bottom flask in sequence, and after constant temperature stirring for 4 hours, 60% of epoxypropyl trimethyl ammonium chloride is slowly added dropwise, and the temperature is raised to 70° C. and the reaction is continued for 7 hours. After the reaction is completed, it is cooled to room temperature, the pH is adjusted to 7 with 10% dilute hydrochloric acid, centrifuged, and the obtained product is washed 3 times with an acetone-ethanol mixed solution, and vacuum dried to obtain chitosan quaternary ammonium salt.
[0016] Furthermore, the mass ratio of chitosan / epoxypropyltrimethylammonium chloride is 1:4.
[0017] Furthermore, the volume ratio of the acetone-ethanol mixed solution is 4:1.
[0018] Furthermore, nylon powder is prepared by the following steps: adding nylon 6 chips with a viscosity of 3.4 into a grinding machine, adjusting the blade clearance to 1.5 mm, using cooling water at 9° C., and grinding at 3800 rpm to obtain nylon 6 powder.
[0019] A method for preparing a composite nylon fiber comprises the following steps:
[0020] 1) adding modified cuprous oxide and polydopamine to deionized water, stirring at 80° C. for 4-5 hours, adding chitosan quaternary ammonium salt, and continuing stirring at 80° C. for 7-8 hours to obtain cuprous oxide / polydopamine / chitosan quaternary ammonium salt particles;
[0021] 2) adding cuprous oxide / polydopamine / chitosan quaternary ammonium salt particles and nylon 6 powder into a high-speed mixer for mixing, adding the mixed particles into a twin-screw extruder for extrusion melting, spinning, and obtaining fibers.
[0022] Furthermore, cuprous oxide / polydopamine / chitosan quaternary ammonium salt particles and nylon 6 powder are mixed and added into a twin-screw extruder for extrusion melting and spinning, and the screw temperatures T1-T8 are set to 220°C, 235°C, 245°C, 255°C, 260°C, 260°C, 245°C, and 235°C.
[0023] Beneficial effects of the present invention:
[0024] (1) KH-550 modified cuprous oxide used in the present invention: the coating layer formed after modification can improve the disadvantage of easy agglomeration of cuprous oxide particles, has uniform particle size, good spinnability, good antibacterial properties and lower toxicity.
[0025] (2) The chitosan quaternary ammonium salt used in the present invention is a high-grade chitosan derivative obtained by chemical modification, and its antibacterial property is superior to chitosan and other chitosan derivatives, and it has good film-forming property through intramolecular and intermolecular hydrogen bonding.
[0026] (3) The polydopamine used in the present invention has active groups such as catechol and amino groups, and has excellent ability to absorb ultraviolet rays, thereby improving the light resistance of the fiber and reducing the yellowing of the fiber. It produces a coordination reaction with modified cuprous oxide, and its negative charge can more easily combine with the positively charged chitosan quaternary ammonium salt, thereby enhancing the overall stability of the material.
[0027] (4) The composite nylon fiber synthesized by the present invention has good antibacterial properties and yellowing resistance. The positively charged chitosan quaternary ammonium salt and the negatively charged polydopamine are more likely to combine, and the film-forming properties of the chitosan quaternary ammonium salt effectively reduce the loss of breaking strength of the composite nylon fiber. DETAILED DESCRIPTION
[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Example 1
[0030] This embodiment provides a composite nylon fiber, which is prepared by the following steps:
[0031] 1) Preparation of modified cuprous oxide
[0032] Cuprous oxide was prepared by glucose reduction method. 1500mL of deionized water was measured and placed in a beaker and stirred. NaOH was used to prepare an alkaline solution (pH=13) and then heated. 10g of glucose was added and magnetically stirred until fully dissolved. After the temperature was constant, 5g of CuSO4·5H2O was added. After the reaction was completed, the product was filtered, washed with water, and dried in a vacuum drying oven at 80°C for 12h to obtain blocky cuprous oxide. After cooling to room temperature, it was ground and then surface treated with KH-550. 9.85g of cuprous oxide was weighed and added to a mixture of 50mL of ethanol and 50mL of deionized water, and 0.15g of KH-550 was added. The solution was dispersed in an ultrasonic disperser for 1h, and then heated to 80°C and stirred for 4h. After the reaction was completed, the product was centrifuged at 12000rpm and then washed with ethanol 3 times, freeze-dried, and modified cuprous oxide was obtained.
[0033] 2) Preparation of polydopamine
[0034] 0.24 g of levodopa was mixed evenly with 100 mL of deionized water, and then a 40% by mass NaOH solution was added to adjust the pH value to 8.5-8.8, and then 0.08 g of potassium ferrate was added. The reaction solution was heated to 90° C. with stirring, and reacted at a constant temperature for 6 hours to obtain a reaction solution. The reaction solution was then centrifuged at 12000 rpm and washed 3 times with deionized water to obtain a solid product. After the solid product was dried, polydopamine was obtained.
[0035] 3) Preparation of chitosan quaternary ammonium salt
[0036] 5g chitosan, 50mL of 40% NaOH and 80mL of isopropanol were added to a round-bottom flask in sequence, stirred at 50°C for 4h, and then 35mL of 60% epoxypropyltrimethylammonium chloride was slowly added dropwise, and the temperature was raised to 70°C to continue the reaction for 7h. After the reaction, the reaction solution was cooled to room temperature, the pH was adjusted to 7 with 10% dilute hydrochloric acid, and centrifuged at 12000rpm. The obtained product was washed 3 times with an acetone-ethanol mixed solution (V / V=4:1), and vacuum dried at 50°C for 24h to obtain chitosan quaternary ammonium salt.
[0037] 4) Preparation of cuprous oxide / polydopamine / chitosan quaternary ammonium salt particles
[0038] Cuprous oxide particles with an average particle size of 800 nm were selected, 2 g of modified cuprous oxide and 1 g of polydopamine were added to deionized water, and after stirring at 80° C. for 4 h, 1 g of chitosan quaternary ammonium salt was added, and stirring was continued for 8 h to obtain cuprous oxide / polydopamine / chitosan quaternary ammonium salt particles.
[0039] 5) Preparation of nylon 6 powder
[0040] Nylon 6 chips with a viscosity of 3.4 were added to the grinding machine, the blade clearance was adjusted to 1.5 mm, and cooling water at 9° C. was used. The grinding process was carried out at 3800 rpm to produce nylon 6 powder with a particle size of 40-60 meshes. The bulk density of the nylon 6 powder was 0.8 g / mL.
[0041] 6) Spinning
[0042] The nylon 6 powder is dried at 80°C for 12 hours in a vacuum drying oven and then cooled to room temperature; the cuprous oxide / polydopamine / chitosan quaternary ammonium salt particles are added into a high-speed mixer with a content of 2% and mixed with nylon 6; the mixture is extruded and melted at 260°C, and after metering, spinning is performed to obtain fibers.
[0043] Example 2
[0044] Compared with Example 1, the difference between this example and Example 1 is that "2 g of modified cuprous oxide" is changed to "1 g of modified cuprous oxide";
[0045] The remaining raw materials and preparation process remain the same as in Example 1.
[0046] Example 3
[0047] Compared with Example 1, the difference between this example and Example 1 is that "2 g of modified cuprous oxide" is changed to "0.5 g of modified cuprous oxide";
[0048] The remaining raw materials and preparation process remain the same as in Example 1.
[0049] Example 4
[0050] The present embodiment is different from the embodiment 1 in that the content of cuprous oxide / polydopamine / chitosan quaternary ammonium salt particles is adjusted to 3%.
[0051] The remaining raw materials and preparation process remain the same as in Example 1.
[0052] Example 5
[0053] The present embodiment is different from the embodiment 1 in that the mass ratio of KH-550 and cuprous oxide is adjusted to 2.5:97.5, specifically, "0.25 g KH-550 and 9.75 g cuprous oxide are added".
[0054] The remaining raw materials and preparation process remain the same as in Example 1.
[0055] Example 6
[0056] Compared with Example 1, the present embodiment differs in that the reaction time in the preparation method is changed, "modified cuprous oxide and polydopamine are added to deionized water, stirred at 80° C. for 5 hours, chitosan quaternary ammonium salt is added, and stirring is continued for 7 hours to obtain cuprous oxide / polydopamine / chitosan quaternary ammonium salt particles".
[0057] The remaining raw materials and preparation process remain the same as in Example 1.
[0058] Comparative Example 1
[0059] The difference between this comparative example and Example 1 is that "chitosan quaternary ammonium salt" is not added; the other raw materials and preparation process remain the same as those in Example 1.
[0060] Comparative Example 2
[0061] The difference between this comparative example and Example 1 is that "polydopamine" is not added; the other raw materials and preparation process remain the same as those in Example 1.
[0062] Performance tests were performed on Examples 1 to 6 and Comparative Examples 1 to 2. The breaking strength of the composite nylon fiber samples was tested according to the test method specified in FZ / T52002-2012; the yellowing performance of the composite nylon fiber samples was tested according to the test method specified in GB / T8427-2019 "Textiles - Color Fastness Tests - Color Fastness to Artificial Light: Xenon Arc"; and the resistance to Gram-negative bacteria (Escherichia coli) and Gram-positive bacteria (Staphylococcus aureus) was tested according to the FZ / T73023-2006 standard. The test results are shown in Table 1:
[0063] Table 1
[0064]
[0065] As can be seen from Table 1, by adopting the above technical scheme, the composite nylon fiber sample prepared in Example 1 has a strength of 3.58CN / dtex, a yellowing resistance grade of L6, an antibacterial rate of Escherichia coli of 92.47%, and an antibacterial rate of Staphylococcus aureus of 97.85%. The antibacterial ability of the composite nylon fiber prepared in Example 2 and Example 3 is significantly reduced; the fiber strength prepared in Example 4 is too low, indicating that the content of cuprous oxide / polydopamine / chitosan quaternary ammonium salt particles is too high, which will make the fiber difficult to form; compared with Example 1, the breaking strength of Example 5 is significantly reduced, because as the mass fraction of KH-550 increases, self-polymerization occurs between KH-550, resulting in a decrease in its mechanical strength.
[0066] Compared with Example 1, the fracture strength of Comparative Example 1 and Comparative Example 2 is reduced; and compared with Comparative Example 1 and Comparative Example 2, the fracture strength is higher after adding chitosan quaternary ammonium salt, which may be because the film-forming properties of chitosan quaternary ammonium salt lead to higher mechanical strength. In particular, compared with Example 1, the yellowing resistance grade of Comparative Example 2 is only significantly reduced to L4, indicating that the addition of polydopamine has obvious yellowing resistance properties.
[0067] In summary, the composite nylon fiber sample prepared in Example 1 has good yellowing resistance and strong antibacterial properties.
[0068] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0069] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A composite nylon fiber, characterized in that: The fiber masterbatch is prepared by extrusion melting and spinning. The raw materials of the fiber masterbatch include cuprous oxide / polydopamine / chitosan quaternary ammonium salt particles and nylon 6 powder. The mass ratio of cuprous oxide / polydopamine / chitosan quaternary ammonium salt particles to nylon 6 powder is 1-3:97-99. The raw materials of cuprous oxide / polydopamine / chitosan quaternary ammonium salt particles include modified cuprous oxide, polydopamine and chitosan quaternary ammonium salt particles; the mass ratio of cuprous oxide, polydopamine and chitosan quaternary ammonium salt in the cuprous oxide / polydopamine / chitosan quaternary ammonium salt particles is 0.5-2:1:
1.
2. A composite nylon fiber according to claim 1, characterized in that: The modified cuprous oxide is cuprous oxide treated with silane coupling agent KH-550, and the mass ratio of the silane coupling agent KH-550 to the cuprous oxide is 1-2.5:97-98.
5.
3. A composite nylon fiber according to claim 2, characterized in that: The average particle size of cuprous oxide is 800-1000 nm.
4. The composite nylon fiber according to claim 1, characterized in that: The particle size of the nylon 6 powder is 40-60 meshes, and the bulk density is 0.8 g / mL.
5. A composite nylon fiber according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: 1) adding modified cuprous oxide and polydopamine to deionized water, stirring at 80° C. for 4-5 hours, adding chitosan quaternary ammonium salt, and continuing to stir for 7-8 hours to obtain cuprous oxide / polydopamine / chitosan quaternary ammonium salt particles; 2) adding cuprous oxide / polydopamine / chitosan quaternary ammonium salt particles and nylon powder into a high-speed mixer for mixing, and then adding the mixed particles into a twin-screw extruder for extrusion melting and spinning to obtain fibers.
6. The composite nylon fiber according to claim 5, characterized in that: The screw temperatures T1 to T8 during the extrusion melting and spinning process were set to 220°C, 235°C, 245°C, 255°C, 260°C, 260°C, 245°C, and 235°C.
Citation Information
Cited By
Corrosion-resistant chinlon 66 industrial yarn and preparation method thereof
CN120138832A
A corrosion-resistant nylon 66 industrial yarn and its preparation method
CN120138832B