Recyclable broad-spectrum antibacterial polylactic acid composite fiber and preparation method thereof
By introducing nanocupole oxide into polylactic acid fibers and using coordination bond cross-linking, polylactic acid composite fibers with broad-spectrum antibacterial and high mechanical properties were prepared, and reused through dichloromethane dissolution, textile materials were solved The shortcomings in antibacterial and recyclable improve the safety and sustainability of textiles.
Patent Information
- Application Number
- CN202411075753.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-07
AI Technical Summary
Existing textile materials such as PET and polylactic fibers are prone to breed bacteria and fungi during repeated use, and are difficult to recover, lacking broad-spectrum antibacterial properties and reusability.
By uniformly dispersing nanocut oxide in polylactic acid solution, mixing liquid is formed by coordinating bond cross-linking, and polylactic acid composite fibers with broad-spectrum antibacterial and high mechanical properties are prepared by extrusion granulation and melt spinning. , and use dichloromethane to dissolve and reuse.
The broad-spectrum antibacterial performance and mechanical properties of polylactic acid composite fiber are improved, and at the same time have good reusable performance, solving the challenges of textiles in terms of safety and reusableability.
Smart Images

Figure CN118932535A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite fibers, in particular to a recyclable broad-spectrum antibacterial polylactic acid composite fiber and a preparation method thereof. Background Art
[0002] At present, more than 90% of textiles are made of polyester fibers such as polyethylene terephthalate (PET). These materials do not have broad-spectrum antibacterial properties and are prone to breed bacteria and fungi during repeated use, posing a potential threat to consumer health. At the same time, these materials are difficult to recycle and often require complex process methods. The current market is in urgent need of developing a new type of fiber material that can not only meet the needs of the textile market, but also solve the problems of safety and reusability.
[0003] Polylactic acid fiber has excellent biocompatibility and mechanical properties, is friendly to human skin, and is an ideal textile raw material. However, although polylactic acid fiber has certain antibacterial ability due to its certain weak acidity, its broad-spectrum antibacterial performance is poor. For example, it is difficult to inhibit the activity of common pathogens such as Candida albicans and Staphylococcus aureus. In this regard, although the introduction of broad-spectrum antibacterial materials into polylactic acid fibers can improve their broad-spectrum antibacterial properties, the mechanical strength of the prepared broad-spectrum antibacterial polylactic acid composite fibers is reduced due to poor interfacial effects, which makes it difficult to meet the mechanical design requirements of textiles. In addition, poor interfacial effects also make the prepared antibacterial polylactic acid fibers difficult to recycle. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing recyclable broad-spectrum antibacterial polylactic acid composite fibers to solve the problems raised in the above-mentioned background technology.
[0005] To achieve the above objectives, the embodiments of the present invention provide the following technical solutions:
[0006] A method for preparing reusable broad-spectrum antibacterial polylactic acid composite fiber comprises the following steps:
[0007] Adding polylactic acid into dichloromethane to dissolve it, to obtain a polylactic acid solution;
[0008] The nano-cuprous oxide is uniformly dispersed in the polylactic acid solution through coordination bond cross-linking to form a mixed solution; the mass ratio of the nano-cuprous oxide to the polylactic acid is (0.001-0.009):1;
[0009] The mixed solution is evaporated, and then extruded into granules and melt-spun to obtain polylactic acid composite fibers.
[0010] Preferably, the mass ratio of the polylactic acid to dichloromethane is 1:(8-12).
[0011] Preferably, the mass ratio of the nano cuprous oxide to polylactic acid is 0.005:1.
[0012] Preferably, the step of uniformly dispersing the nano cuprous oxide in the polylactic acid solution through coordination bond cross-linking to form a mixed solution specifically includes:
[0013] The nano cuprous oxide and the polylactic acid solution are mixed and subjected to ultrasonic dispersion treatment to obtain a mixed solution.
[0014] Preferably, the ultrasonic dispersion treatment has an ultrasonic frequency of 20-40 kHz and a power of 50-100 W.
[0015] Preferably, the temperature of the volatilization treatment is 45-55°C.
[0016] Preferably, the extrusion granulation is carried out using a twin-screw extruder; the twin-screw temperature range of the twin-screw extruder is 170-200° C., and the screw speed is 110-130 r / min.
[0017] Preferably, the melt spinning process uses a spinneret with a diameter of 0.6-0.8 mm, a drawing speed of 250-350 r / min, and a spinning temperature of 180-200°C.
[0018] Another object of an embodiment of the present invention is to provide a polylactic acid composite fiber prepared by the above preparation method.
[0019] Preferably, the polylactic acid composite fiber is recovered by placing the polylactic acid composite fiber in dichloromethane to re-dissolve and recycle it.
[0020] The preparation method of the polylactic acid composite fiber provided in the embodiment of the present invention introduces nano cuprous oxide with broad-spectrum antibacterial properties as physical crystallization points into the polylactic acid molecular chain by utilizing the coordination bond cross-linking effect, thereby improving the mechanical properties of the polylactic acid composite fiber and giving the polylactic acid composite fiber good antibacterial properties. In addition, since the coordination bonds are easy to break and regenerate, the polylactic acid composite fiber prepared by the present invention also has good reusability, which is expected to enhance the application potential of the polylactic acid composite fiber and its products. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 is an outline diagram of the fiber obtained in Examples 1-5;
[0022] Figure 2 is a knitting forming diagram of Example 1;
[0023] Figure 3 It is a load-bearing diagram of a single filament of Example 1;
[0024] Figure 4 are surface and cross-sectional SEM images of Example 1;
[0025] Figure 5 are surface and cross-sectional SEM images of Examples 6-7;
[0026] Figure 6 It is the Mapping and EDS spectrum of Example 1;
[0027] Figure 7 It is the infrared spectrum of comparative example and Example 1;
[0028] Figure 8 It is the XRD curve diagram of comparative example and Example 1;
[0029] Fig. 9 It is the XPS general spectrum of comparative example and embodiment 1;
[0030] Fig.10 It is the fine spectra of C1s, O 1s, and Cu2p of the comparative example and Example 1;
[0031] Fig.11 is a stress-strain curve diagram of comparative examples and embodiments 1-5;
[0032] Fig.12 is a stress-strain curve diagram of Example 1 placed at different times;
[0033] Fig.13 It is the colony photos of Candida albicans, Escherichia coli and Staphylococcus aureus on the standard cotton fabric, the comparative example and Example 1;
[0034] Fig.14 It is a bar chart comparing the broad-spectrum antibacterial rates of the comparative example, Example 1 and the standard cotton fabric;
[0035] Fig.15 is a recovery schematic diagram of Example 10;
[0036] Fig.16 are surface and cross-sectional SEM images of Example 10;
[0037] Fig.17 These are colony photos of Candida albicans, Escherichia coli, and Staphylococcus aureus in Example 1 and Example 10. DETAILED DESCRIPTION
[0038] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0039] The embodiment of the present invention aims to provide a broad-spectrum antibacterial polylactic acid composite fiber with recyclable properties, which can not only meet the requirements of traditional textiles in terms of mechanical properties, but also significantly improve the broad-spectrum antibacterial properties of textiles and ensure that their recyclable properties are not affected. Through the technical solution provided by the embodiment of the present invention, it is expected to effectively promote the application of polylactic acid fibers in the high value-added textile market, while promoting environmentally friendly and sustainable textile production methods.
[0040] Specifically, in one embodiment of the present invention, a method for preparing a reusable broad-spectrum antibacterial polylactic acid composite fiber is provided, which comprises the following steps:
[0041] S1, adding polylactic acid into dichloromethane to dissolve it, to obtain a polylactic acid solution;
[0042] S2, uniformly dispersing the nano cuprous oxide in the polylactic acid solution through coordination bond cross-linking to form a mixed solution; the mass ratio of the nano cuprous oxide to the polylactic acid is (0.001-0.009):1;
[0043] S3. After the mixed solution is evaporated, it is extruded into granules and melt-spun to obtain polylactic acid composite fibers, which are recorded as Cu2O / PLA fibers.
[0044] In the Cu2O / PLA fiber prepared by the above preparation method, Cu2O and PLA molecular chains are cross-linked in the form of coordination bonds and dispersed in the PLA matrix. Cu2O, as a new physical crystallization point, makes the Cu2O / PLA fiber show excellent mechanical strength. Under the synergistic effect of the broad-spectrum antibacterial property of Cu2O and the natural weak acidity of PLA, the Cu2O / PLA fiber exhibits ultra-high broad-spectrum antibacterial performance. In addition, thanks to the easy breakage and regeneration of the coordination bonds, the Cu2O / PLA fiber exhibits excellent reusability. Therefore, the polylactic acid composite fiber prepared in the embodiment of the present invention has high mechanical strength, broad-spectrum antibacterial property and reusability.
[0045] In a preferred embodiment of the present invention, the mass ratio of polylactic acid to dichloromethane is 1:(8-12), preferably 1:10.
[0046] In a preferred embodiment of the present invention, the mass ratio of nano cuprous oxide to polylactic acid is preferably 0.005:1.
[0047] In a preferred embodiment of the present invention, the step of uniformly dispersing nano cuprous oxide in a polylactic acid solution by coordination bond cross-linking to form a mixed solution, that is, the above step S2 specifically includes: mixing the nano cuprous oxide with the polylactic acid solution and performing ultrasonic dispersion treatment to obtain a mixed solution.
[0048] In a preferred embodiment of the present invention, the ultrasonic dispersion treatment has an ultrasonic frequency of 20-40 kHz and a power of 50-100 W; preferably, the ultrasonic frequency is 20 kHz and the power is 50 W.
[0049] In a preferred embodiment of the present invention, the temperature of the volatilization treatment is 45-55° C., preferably 50° C. In practical applications, the mixed solution can be placed in an oven at 45-55° C. for volatilization treatment to remove the dichloromethane solvent.
[0050] In a preferred embodiment of the present invention, the extrusion granulation is carried out by a twin-screw extruder; the twin-screw temperature zone of the twin-screw extruder is 170-200° C.; the screw speed is 110-130 r / min, preferably 120 r / min.
[0051] In a preferred embodiment of the present invention, the melt spinning process uses a spinneret with a diameter of 0.6-0.8 mm, a drawing speed of 250-350 r / min, and a spinning temperature of 180-200°C.
[0052] In the above-mentioned embodiment of the present invention, ultrasonic dispersion treatment is adopted to achieve uniform dispersion of nano cuprous oxide in the polylactic acid solution through coordination bond cross-linking, and nano cuprous oxide is introduced into the polylactic acid molecular chain as a physical crystallization point, thereby improving the mechanical properties of the polylactic acid composite fiber and giving the polylactic acid composite fiber good antibacterial properties. In addition, the polylactic acid composite fiber prepared by the dissolution, evaporation treatment, twin-screw extrusion granulation and melt spinning processes of the embodiment of the present invention is easy to recycle and reuse, eliminating the traditional polylactic acid recycling and reuse process such as degradation and repolymerization.
[0053] In another embodiment of the present invention, a method for recycling the polylactic acid composite fiber is provided, which comprises: placing the polylactic acid composite fiber in dichloromethane to re-dissolve and recycle it.
[0054] Specifically, the above-mentioned polylactic acid composite fiber recycling method comprises the following steps: mixing the above-mentioned used polylactic acid composite fiber with an appropriate amount of dichloromethane to convert the polylactic acid composite fiber into a new polylactic acid dispersion, and recycling the polylactic acid dispersion to obtain a new polylactic acid composite fiber. It should be noted that in the above-mentioned steps, the polylactic acid composite fiber can be quickly dissolved in dichloromethane by using ultrasonic dispersion technology.
[0055] The following examples are some specific implementation cases and application cases of the present invention in practical applications, but are not limited thereto. It should be noted that in the following examples, polylactic acid, nano cuprous oxide, dichloromethane, etc. are all conventional commercial products.
[0056] Example 1: This example provides a method for preparing a reusable broad-spectrum antibacterial polylactic acid composite fiber, which comprises the following steps:
[0057] S1. Add 10 g of polylactic acid into 100 g of dichloromethane for mixed dissolution to obtain a polylactic acid solution M1.
[0058] S2. Mix the polylactic acid solution M1 and 0.05 g of nano cuprous oxide, and perform ultrasonic dispersion treatment to obtain a mixed solution M2; wherein the ultrasonic frequency of the ultrasonic dispersion treatment is 20 kHz and the power is 50 W.
[0059] S3. The mixed liquid M2 is placed in a 50°C oven for evaporation to remove the dichloromethane solvent, and then extruded and granulated through a twin-screw extruder with a temperature range of 170°C to 200°C, and then melt-spun to obtain polylactic acid composite fibers, recorded as Cu2O / PLA-0.5%; wherein the screw speed of the twin-screw extruder is 120r / min; the melt spinning process is: using a spinneret with a diameter of 0.7mm, a drawing speed of 300r / min, and a spinning temperature of 190°C.
[0060] Example 2: This example provides a method for preparing a reusable broad-spectrum antibacterial polylactic acid composite fiber, which comprises the following steps:
[0061] S1. Add 10 g of polylactic acid into 100 g of dichloromethane for mixed dissolution to obtain a polylactic acid solution M1.
[0062] S2. Mix the polylactic acid solution M1 and 0.01 g of nano cuprous oxide, and perform ultrasonic dispersion treatment to obtain a mixed solution M2; wherein the ultrasonic dispersion treatment is performed at an ultrasonic frequency of 20 kHz and a power of 50 W.
[0063] S3. The mixed liquid M2 is placed in a 50°C oven for evaporation to remove the dichloromethane solvent, and then extruded and granulated through a twin-screw extruder with a temperature range of 170°C to 200°C, and then melt-spun to obtain polylactic acid composite fibers, recorded as Cu2O / PLA-0.1%; wherein the screw speed of the twin-screw extruder is 120r / min; the melt spinning process is: using a spinneret with a diameter of 0.7mm, a drawing speed of 300r / min, and a spinning temperature of 190°C.
[0064] Example 3: This example provides a method for preparing a reusable broad-spectrum antibacterial polylactic acid composite fiber, which comprises the following steps:
[0065] S1. Add 10 g of polylactic acid into 100 g of dichloromethane for mixed dissolution to obtain a polylactic acid solution M1.
[0066] S2. Mix the polylactic acid solution M1 and 0.03 g of nano cuprous oxide, and perform ultrasonic dispersion treatment to obtain a mixed solution M2; wherein the ultrasonic dispersion treatment is performed at an ultrasonic frequency of 20 kHz and a power of 50 W.
[0067] S3. The mixed liquid M2 is placed in a 50°C oven for evaporation to remove the dichloromethane solvent, and then extruded and granulated through a twin-screw extruder with a temperature range of 170°C to 200°C, and then melt-spun to obtain polylactic acid composite fibers, recorded as Cu2O / PLA-0.3%; wherein the screw speed of the twin-screw extruder is 120r / min; the melt spinning process is: using a spinneret with a diameter of 0.7mm, a drawing speed of 300r / min, and a spinning temperature of 190°C.
[0068] Example 4: This example provides a method for preparing a reusable broad-spectrum antibacterial polylactic acid composite fiber, which comprises the following steps:
[0069] S1. Add 10 g of polylactic acid into 100 g of dichloromethane for mixed dissolution to obtain a polylactic acid solution M1.
[0070] S2. Mix the polylactic acid solution M1 and 0.07 g of nano cuprous oxide, and perform ultrasonic dispersion treatment to obtain a mixed solution M2; wherein the ultrasonic dispersion treatment is performed at an ultrasonic frequency of 20 kHz and a power of 50 W.
[0071] S3. The mixed liquid M2 is placed in a 50°C oven for evaporation to remove the dichloromethane solvent, and then extruded and granulated through a twin-screw extruder with a temperature range of 170°C to 200°C, and then melt-spun to obtain polylactic acid composite fibers, recorded as Cu2O / PLA-0.7%; wherein the screw speed of the twin-screw extruder is 120r / min; the melt spinning process is: using a spinneret with a diameter of 0.7mm, a drawing speed of 300r / min, and a spinning temperature of 190°C.
[0072] Example 5: This example provides a method for preparing a reusable broad-spectrum antibacterial polylactic acid composite fiber, which comprises the following steps:
[0073] S1. Add 10 g of polylactic acid into 100 g of dichloromethane for mixed dissolution to obtain a polylactic acid solution M1.
[0074] S2. Mix the polylactic acid solution M1 and 0.09 g of nano cuprous oxide, and perform ultrasonic dispersion treatment to obtain a mixed solution M2; wherein the ultrasonic dispersion treatment is performed at an ultrasonic frequency of 20 kHz and a power of 50 W.
[0075] S3. The mixed liquid M2 is placed in a 50°C oven for evaporation to remove the dichloromethane solvent, and then extruded and granulated through a twin-screw extruder with a temperature range of 170°C to 200°C, and then melt-spun to obtain polylactic acid composite fibers, recorded as Cu2O / PLA-0.9%; wherein the screw speed of the twin-screw extruder is 120r / min; the melt spinning process is: using a spinneret with a diameter of 0.7mm, a drawing speed of 300r / min, and a spinning temperature of 190°C.
[0076] Example 6: This example provides a method for preparing a reusable broad-spectrum antibacterial polylactic acid composite fiber, which comprises the following steps:
[0077] S1. Add 10 g of polylactic acid into 100 g of dichloromethane for mixed dissolution to obtain a polylactic acid solution M1.
[0078] S2. Mix the polylactic acid solution M1 and 0.1 g of nano cuprous oxide, and perform ultrasonic dispersion treatment to obtain a mixed solution M2; wherein the ultrasonic dispersion treatment is performed at an ultrasonic frequency of 20 kHz and a power of 50 W.
[0079] S3. The mixed liquid M2 is placed in a 50°C oven for evaporation to remove the dichloromethane solvent, and then extruded and granulated through a twin-screw extruder with a temperature range of 170°C to 200°C, and then melt-spun to obtain polylactic acid composite fibers, recorded as Cu2O / PLA-1%; wherein the screw speed of the twin-screw extruder is 120r / min; the melt spinning process is: using a spinneret with a diameter of 0.7mm, a drawing speed of 300r / min, and a spinning temperature of 190°C.
[0080] Example 7: This example provides a method for preparing a reusable broad-spectrum antibacterial polylactic acid composite fiber, which comprises the following steps:
[0081] S1. Add 10 g of polylactic acid into 100 g of dichloromethane for mixed dissolution to obtain a polylactic acid solution M1.
[0082] S2. Mix the polylactic acid solution M1 and 0.3 g of nano cuprous oxide, and perform ultrasonic dispersion treatment to obtain a mixed solution M2; wherein the ultrasonic dispersion treatment is performed at an ultrasonic frequency of 20 kHz and a power of 50 W.
[0083] S3. The mixed liquid M2 is placed in a 50°C oven for evaporation to remove the dichloromethane solvent, and then extruded and granulated through a twin-screw extruder with a temperature range of 170°C to 200°C, and then melt-spun to obtain polylactic acid composite fibers, recorded as Cu2O / PLA-3%; wherein the screw speed of the twin-screw extruder is 120r / min; the melt spinning process is: using a spinneret with a diameter of 0.7mm, a drawing speed of 300r / min, and a spinning temperature of 190°C.
[0084] Example 8: This example provides a method for preparing a reusable broad-spectrum antibacterial polylactic acid composite fiber, which comprises the following steps:
[0085] S1. Add 10 g of polylactic acid into 80 g of dichloromethane for mixing and dissolving to obtain a polylactic acid solution M1.
[0086] S2. Mix the polylactic acid solution M1 and 0.05 g of nano cuprous oxide, and perform ultrasonic dispersion treatment to obtain a mixed solution M2; wherein the ultrasonic dispersion treatment is performed at an ultrasonic frequency of 30 kHz and a power of 75 W.
[0087] S3. The mixed solution M2 is placed in a 45°C oven for evaporation to remove the dichloromethane solvent, and then extruded and granulated through a twin-screw extruder with a temperature range of 170°C to 200°C, and then melt-spun to obtain polylactic acid composite fibers, denoted as Cu2O / PLA-3%; wherein the screw speed of the twin-screw extruder is 110r / min; the melt-spinning process is: using a spinneret with a diameter of 0.6mm, a drawing speed of 250r / min, and a spinning temperature of 180°C.
[0088] Example 9: This example provides a method for preparing a reusable broad-spectrum antibacterial polylactic acid composite fiber, which comprises the following steps:
[0089] S1. Add 10 g of polylactic acid into 120 g of dichloromethane for mixed dissolution to obtain a polylactic acid solution M1.
[0090] S2. Mix the polylactic acid solution M1 and 0.05 g of nano cuprous oxide, and perform ultrasonic dispersion treatment to obtain a mixed solution M2; wherein the ultrasonic frequency of the ultrasonic dispersion treatment is 40 kHz and the power is 100 W.
[0091] S3. The mixed liquid M2 is placed in a 55°C oven for evaporation to remove the dichloromethane solvent, and then extruded and granulated through a twin-screw extruder with a temperature range of 170°C to 200°C, and then melt-spun to obtain polylactic acid composite fibers, recorded as Cu2O / PLA-3%; wherein the screw speed of the twin-screw extruder is 130r / min; the melt spinning process is: using a spinneret with a diameter of 0.8mm, a drawing speed of 350r / min, and a spinning temperature of 200°C.
[0092] Example 10: This example provides a method for recycling and preparing reusable broad-spectrum antibacterial polylactic acid composite fibers, which comprises the following steps:
[0093] S1. Cut 10 g of the polylactic acid composite fiber obtained in the above Example 1 into pieces, and then add them into 100 g of dichloromethane for mixing and dissolving to obtain a polylactic acid solution M1.
[0094] S2. Perform ultrasonic dispersion treatment on the polylactic acid solution M1 to obtain polylactic acid dispersion M2; wherein the ultrasonic dispersion treatment is performed at an ultrasonic frequency of 20 kHz and a power of 50 W.
[0095] S3. The polylactic acid dispersion M2 is placed in a 50°C oven for evaporation to remove the dichloromethane solvent, and then extruded and granulated through a twin-screw extruder with a temperature range of 170°C to 200°C, and then melt-spun to obtain recycled polylactic acid composite fibers, denoted as Cu2O / PLA-R; wherein the screw speed of the twin-screw extruder is 120r / min; the melt-spinning process is: using a spinneret with a diameter of 0.7mm, a drawing speed of 300r / min, and a spinning temperature of 190°C.
[0096] Comparative Example: This comparative example provides a method for preparing pure polylactic acid fiber, which comprises the following steps:
[0097] S1. Add 10 g of polylactic acid into 100 g of dichloromethane for mixed dissolution to obtain a polylactic acid solution M1.
[0098] S2. Perform ultrasonic dispersion treatment on the polylactic acid solution M1 to obtain polylactic acid dispersion M2; wherein the ultrasonic dispersion treatment is performed at an ultrasonic frequency of 20 kHz and a power of 50 W.
[0099] S3. The polylactic acid dispersion M2 is placed in a 50°C oven for volatilization to remove the dichloromethane solvent, and then extruded and granulated through a twin-screw extruder with a temperature range of 170°C to 200°C, and then melt-spun to obtain pure polylactic acid fiber, denoted as Neat PLA; wherein the screw speed of the twin-screw extruder is 120r / min; the melt-spinning process is: using a spinneret with a diameter of 0.7mm, a drawing speed of 300r / min, and a spinning temperature of 190°C.
[0100] Performance test: 1. The Cu2O / PLA fibers prepared in the above examples 1-5 were respectively wound on a winding drum, such as Figure 1 As shown (from left to right: Cu2O / PLA-0.1%, Cu2O / PLA-0.3%, Cu2O / PLA-0.5%, Cu2O / PLA-0.7%, Cu2O / PLA-0.9%), it shows that the polylactic acid composite fiber material provided by the present invention can be prepared continuously.
[0101] 2. The Cu2O / PLA fibers prepared in the embodiment of the present invention are woven into a shape to obtain Figure 2 , which shows that Cu2O / PLA fiber has good weaving performance.
[0102] 3. Hang a 20g weight on the Cu2O / PLA-0.5% fiber of Example 1. Figure 3 As shown, it can be seen from the figure that the fiber will not break, which indicates its excellent mechanical strength.
[0103] 4. The surface and cross section of the Cu2O / PLA-0.5% prepared in Example 1 were placed under an ion sputtering apparatus for 30 seconds to obtain Figure 4 From the SEM images, it can be seen that Cu2O / PLA-0.5% has a smooth surface and cross-section, and there is no particle aggregation.
[0104] 5. The surfaces and cross sections of Cu2O / PLA-1% and Cu2O / PLA-3% prepared in Examples 6-7 were placed under an ion sputtering apparatus for 30 seconds to obtain Figure 5 From the SEM image, it can be seen that when too much cuprous oxide is introduced, the surface will become rough and there will be obvious aggregation of particles. Too much cuprous oxide will agglomerate in the polylactic acid matrix, affecting its morphology and performance.
[0105] 6. The Cu2O / PLA-0.5% cross section prepared in Example 1 was characterized in the energy dispersive x-ray spectroscopy (EDS) surface scanning mode to obtain Figure 6 As can be seen from the figure, there are three elements, C, O, and Cu, in the cross-sectional structure of Cu2O / PLA-0.5%, with contents of 70.83%, 28.81%, and 0.36%, respectively. Figure 6 It can also be seen that on the cross section of the fiber, Cu2O is evenly dispersed in the cross section of the Cu2O / PLA fiber.
[0106] 7. The Neat PLA prepared in the comparative example and the Cu2O / PLA prepared in the example were placed in a Fourier transform infrared spectrometer to obtain infrared spectra of the above materials, as shown in FIG. Figure 7 As shown. Figure 7 It can be seen that 1750cm -1 The C=O vibration peak at 40° is slightly blue-shifted, indicating that the cuprous ions in cuprous oxide form coordination bonds with the carbonyl groups in polylactic acid. Thanks to the coordination effect, cuprous oxide can be well dispersed in polylactic acid, laying a molecular structural foundation for the good mechanical properties of the Cu2O / PLA fiber in the example.
[0107] 8. The Neat PLA prepared in the comparative example and the Cu2O / PLA-0.5% prepared in Example 1 were placed in an X-ray diffractometer to obtain the XRD curves of the above materials, as shown in FIG. Figure 8 As shown. Figure 8 It can be seen that the diffraction peaks of Neat PLA at 16.7° and 19.1° correspond to the
[200] and
[203] crystal planes, respectively. Cu2O / PLA-0.5% fiber also has diffraction peaks at 16.7° and 19.1°, indicating that a small amount of cuprous oxide will not change the crystal structure of polylactic acid.
[0108] 9. X-ray photoelectron spectroscopy was used to characterize the chemical element environment changes of Neat PLA prepared in the comparative example and Cu2O / PLA-0.5% prepared in Example 1, and the XPS total spectrum was obtained, as shown in FIG. Fig. 9 As shown. Fig. 9 It can be seen that Neat PLA has typical C1s and O1s binding energy signal peaks at 283.48eV and 531.17eV. Compared with Neat PLA, Cu2O / PLA fiber has two new peaks at 933.46eV and 952.29eV, which belong to the binding energy signal peaks of Cu 2p2 / 3 and Cu2p1 / 3 respectively. This shows that Cu2O was successfully introduced into PLA.
[0109] 10. According to the same method as above, the fine spectra of C1s, O 1s, and Cu 2p of Neat PLA prepared in the comparative example and Cu2O / PLA-0.5% prepared in Example 1 were obtained, as shown in FIG. Fig.10 As shown. Fig.10It can be seen that the position of the C 1s signal peak on the Cu2O / PLA fiber has not changed, indicating that the C atom does not directly interact with the Cu atom. In the O 1s signal peak, a new peak appears at 531.0eV, corresponding to the Cu:O coordination bond. This indicates that there is an interaction between the O atom and the Cu atom. In addition, the binding energy of the C=O bond shifts from 533.8eV to 533.4eV, which is considered to be the formation of a coordination bond between Cu and O atoms in the carbon-oxygen double bond, and the migration of the electron cloud. It can be seen from the Cu 2p fine spectrum that due to the effect of the Cu:O coordination bond, the Cu 2p binding energy of the Cu2O / PLA fiber has also shifted. At the same time, there is no shock peak of divalent copper in the spectrum, which indicates that Cu2O exists stably in the PLA matrix and no oxidation occurs during the preparation process.
[0110] 11. The Neat PLA prepared in the comparative example and the Cu2O / PLA (Cu2O / PLA-0.1%, Cu2O / PLA-0.3%, Cu2O / PLA-0.5%, Cu2O / PLA-0.7%, Cu2O / PLA-0.9%) prepared in Examples 1-5 were cut into 60 mm lengths, connected to a universal material testing machine, and the tensile rate was controlled to 5 mm / min. Stress-strain experiments were performed to obtain stress-strain curves and comparison diagrams of various mechanical properties, as shown in FIG. Fig.11 shown. Fig.11 It shows that after adding Cu2O, the prepared Cu2O / PLA has good mechanical properties.
[0111] 12. The Cu2O / PLA-0.5% prepared in Example 1 was placed at room temperature and pressure for 6 months, and its mechanical properties were tested in the same manner as above. Fig.12 .from Fig.12 It can be seen that after 6 months of storage, the elongation at break decreased, but the tensile strength decreased slowly. This shows that under normal conditions, the prepared Cu2O / PLA fiber has a long stability and can be used and stored for a long time.
[0112] 13. According to GB / T 20944.3-2008 textile broad-spectrum antibacterial performance evaluation standard, the broad-spectrum antibacterial performance of standard cotton fabric, Cu2O / PLA fiber prepared in Example 1 and comparative example Neat PLA fiber against Candida albicans, Escherichia coli and Staphylococcus aureus was studied by oscillation method. The colony photos are shown in Fig.13 As shown. It can be seen that there are almost no colonies in the culture dish where the Cu2O / PLA fiber is located, and there are still many colonies in the culture dish where the Neat PLA is located. The results show that the Cu2O / PLA fiber has ultra-high broad-spectrum antibacterial properties.
[0113] 14. According to GB / T 20944.3-2008, the broad-spectrum antibacterial rates of Cu2O / PLA-0.5% prepared in Example 1, the comparative example Neat PLA and the standard cotton fabric were tested and calculated to obtain a broad-spectrum antibacterial rate comparison bar graph, as shown in FIG. Fig.14 shown. Fig.14 It shows that the Cu2O / PLA-0.5% prepared in Example 1 has an ultra-high broad-spectrum antibacterial rate of more than 99%, far exceeding the standard cotton fabric and the comparative example Neat PLA.
[0114] 15. Recycling of Cu2O / PLA fibers Fig.15 As shown. Cu2O / PLA-R fibers can be recovered through dissolution and re-spinning.
[0115] 16. The surface and cross section of the Cu2O / PLA-R fiber recovered in Example 10 were placed under an ion sputtering instrument for 30 seconds to obtain a SEM image, as shown in FIG. Fig.16 As shown. Fig.16 It can be seen that the fibers still maintain a smooth surface and cross-section after respinning, and the nanoparticles do not agglomerate in the polylactic acid matrix.
[0116] 17. According to GB / T 20944.3-2008 textile broad-spectrum antibacterial performance evaluation standard, the broad-spectrum antibacterial performance of the Cu2O / PLA-R fiber recovered from Example 10 against Candida albicans (C.albicans), Escherichia coli (E.coli) and Staphylococcus aureus (S.aureus) was studied by oscillation method. Fig.17 It can be seen that there are almost no colonies in the culture dish of the solvent-recovered and re-spun fibers, which indicates that the recycled fibers still have ultra-high broad-spectrum antibacterial properties.
[0117] In summary, the Cu2O / PLA fiber prepared in the embodiment of the present invention has excellent broad-spectrum antibacterial properties, high mechanical strength and recyclability, and has high practical value in the field of polylactic acid fibers.
[0118] Based on the above-mentioned ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above-mentioned description. The technical scope of the present invention is not limited to the contents of the specification.
Claims
1. A method for preparing recyclable broad-spectrum antibacterial polylactic acid composite fiber, characterized in that: The following steps are involved: Adding polylactic acid into dichloromethane to dissolve it, to obtain a polylactic acid solution; The nano-cuprous oxide is uniformly dispersed in the polylactic acid solution through coordination bond cross-linking to form a mixed solution; the mass ratio of the nano-cuprous oxide to the polylactic acid is (0.001-0.009):1; The mixed solution is evaporated, and then extruded into granules and melt-spun to obtain polylactic acid composite fibers.
2. The method for preparing polylactic acid composite fiber according to claim 1, characterized in that: The mass ratio of the polylactic acid to dichloromethane is 1:(8-12).
3. The method for preparing polylactic acid composite fiber according to claim 1, characterized in that: The mass ratio of the nano cuprous oxide to the polylactic acid is 0.005:
1.
4. The method for preparing polylactic acid composite fiber according to claim 1, characterized in that: The step of uniformly dispersing nano cuprous oxide in a polylactic acid solution through coordination bond cross-linking to form a mixed solution specifically comprises: The nano cuprous oxide and the polylactic acid solution are mixed and subjected to ultrasonic dispersion treatment to obtain a mixed solution.
5. The method for preparing polylactic acid composite fiber according to claim 4, characterized in that: The ultrasonic frequency of the ultrasonic dispersion treatment is 20-40kHz and the power is 50-100W.
6. The method for preparing polylactic acid composite fiber according to claim 1, characterized in that: The temperature of the evaporation treatment is 45-55°C.
7. The method for preparing polylactic acid composite fiber according to claim 1, characterized in that: The extrusion granulation is carried out by a twin-screw extruder; the twin-screw temperature zone of the twin-screw extruder is 170-200° C., and the screw speed is 110-130 r / min.
8. The method for preparing polylactic acid composite fiber according to claim 1, characterized in that: The melt spinning process uses a spinneret with a diameter of 0.6-0.8 mm, a drawing speed of 250-350 r / min, and a spinning temperature of 180-200°C.
9. A polylactic acid composite fiber prepared by the preparation method according to any one of claims 1 to 8.
10. The polylactic acid composite fiber according to claim 9, characterized in that: The polylactic acid composite fiber recovery method comprises: placing the polylactic acid composite fiber in dichloromethane to re-dissolve and recycle it.
Citation Information
Patent Citations
Manufacturing method of colored antibacterial corn fiber filaments
CN109629039A
Antibacterial and antiviral mask containing cuprous oxide
CN113291002A
Polylactic acid / nanocellulose whisker / graphene oxide ternary composite material
CN116120723A
Graphene oxide loaded cuprous oxide antibacterial fiber as well as preparation method and application thereof
CN116427051A
Spinning method of nano-particle-containing fibrous membrane
CN117867674A
Cited By
Antibacterial cool polylactic acid fiber fabric as well as preparation method and application thereof
CN120606578A