Bio-based shape memory polylactic acid fiber material and preparation method thereof
By mixing bio-based polyether amide elastomers with modifiers and using polycarboxylic acid dispersants, the impact resistance and shape memory properties of polylactic acid fiber materials have been improved, solving the problems existing in the prior art and achieving high tensile properties and short shape memory recovery time.
Patent Information
- Application Number
- CN202411077335.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-12
AI Technical Summary
Existing technologies are insufficient to effectively improve the impact resistance, shape memory, and resilience of polylactic acid fiber materials, thus limiting their large-scale applications.
Bio-based shape memory polylactic acid fiber materials were prepared by mixing bio-based polyether amide elastomers with modifiers and using a specific ratio of polycarboxylic acid dispersants, thereby improving their tensile strength, elongation at break, impact resistance and shape memory properties.
It improves the tensile and impact resistance of polylactic acid fiber materials, shortens the shape memory recovery time, enhances the elastic recovery rate, and maintains good compatibility between bio-based elastomers and polylactic acid fiber materials.
Smart Images

Figure BDA0004982706200000021 
Figure BDA0004982706200000041 
Figure BDA0004982706200000042
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of modified preparation of polylactic acid fibers, and specifically relates to a bio-based shape memory polylactic acid fiber material and a preparation method thereof. Background Art
[0002] Polylactic acid fiber material is a biodegradable material derived from renewable resources. It has shape memory function and good transparency, chemical stability and biocompatibility. It plays an important role in the fields of medicine. However, due to the relatively poor impact resistance, shape memory and resilience of polylactic acid fiber material, its large-scale application is limited.
[0003] In the prior art, in order to improve the impact resistance, shape memory, resilience and other properties of polylactic acid fiber materials, polylactic acid fiber materials are blended with elastomers such as bio-based polyetheramide elastomers for toughening modification. Although the tensile strength, elongation at break, impact resistance and other mechanical properties of polylactic acid fiber materials are improved to a certain extent, the shape memory properties and resilience are still not significantly improved.
[0004] In order to further increase the tensile strength, elongation at break, impact resistance and other mechanical properties as well as shape memory properties and resilience of elastomers such as polylactic acid fiber materials and bio-based polyetheramide elastomers, dispersants such as polycarboxylate ammonium salt dispersants are often added to improve the impact resistance, resilience and shape memory properties of fiber materials made from bio-based elastomers and polylactic acid fiber materials, but the improvement is still not ideal.
[0005] In view of the problems existing in the prior art, how to improve the tensile strength, elongation at break, impact resistance and other mechanical properties of polylactic acid fiber materials as well as shape memory properties and resilience is a problem to be solved urgently in the present invention. Summary of the invention
[0006] The object of the present invention is to provide a bio-based shape memory polylactic acid fiber material and a preparation method to solve the problems raised in the above background technology.
[0007] To achieve the above object, the present invention provides the following technical solutions:
[0008] On the one hand, the present invention provides a bio-based shape memory polylactic acid fiber material, comprising polylactic acid fiber material, a bio-based elastomer and a dispersant; the raw materials for preparing the bio-based elastomer comprise a bio-based polyetheramide elastomer and a modifier; the raw materials for preparing the modifier include glycidyl methacrylate, vinyl pyrrolidone and an initiator.
[0009] As a further improvement, the mass ratio of the bio-based polyetheramide elastomer to the modifier is 1:(0.01-0.1).
[0010] As a further improvement, the mass ratio of glycidyl methacrylate, vinyl pyrrolidone and initiator is 1:(1-3):(0.1-0.5).
[0011] As a further improvement, the initiator is one or more of benzoyl peroxide, dicumyl peroxide and azobisisobutyronitrile.
[0012] The dispersant is a polycarboxylic acid dispersant having the following general formula:
[0013]
[0014] Wherein, p is selected from an integer of 1-3, q is selected from an integer of 1-4, and when p is 2 and q is 3, the obtained polycarboxylic acid dispersant has higher stability and dispersibility.
[0015] As a further improvement, the raw materials for preparing the polycarboxylic acid dispersant include methacrylic acid, allyl polyoxyethylene ether and a chain transfer agent.
[0016] As a further improvement, the chain transfer agent comprises one or more of potassium persulfate, ammonium persulfate, and glycolic acid.
[0017] As a further improvement, the specific preparation steps of the polycarboxylic acid dispersant are as follows: add 5-10g of allyl polyoxyethylene ether and 5-10mL of deionized water into a flask, stir for 3-5min, then drop 5-10g of methacrylic acid and 0.15-0.3g of thioglycolic acid into the flask respectively, stir at 100-150r / min, slowly heat to 80-100°C, react at 80-100°C for 2-3h, and then keep warm for 2-3h. After the reaction is completed, spin dry the reaction liquid, and then vacuum dry to obtain the polycarboxylic acid dispersant.
[0018] The specific preparation steps of the bio-based elastomer are as follows: premix 20-100g of the bio-based polyetheramide elastomer at 170-200°C and a rotation speed of 50-100r / min for 2-3min to make it completely melted, and then add 0.1-10g of the modifier and continue blending for 5-10min.
[0019] On the other hand, the present invention also provides a method for preparing a bio-based shape memory polylactic acid fiber material. The specific preparation steps of the bio-based shape memory polylactic acid fiber material are as follows: the prepared dispersant, bio-based elastomer and polylactic acid fiber material are melt-blended at 170-200°C and a rotation speed of 50-100r / min for 5-10min to obtain a bio-based shape memory polylactic acid fiber material, and the mass ratio of the bio-based elastomer to the polylactic acid fiber material is 1:(3-9).
[0020] Compared with the prior art, the beneficial effects of the present invention are as follows: the bio-based shape memory polylactic acid fiber material provided by the present invention has good tensile properties and impact resistance, and a short shape memory recovery time and a high elastic recovery rate. Even if the amount of modifier added is small, the bio-based elastomer and the polylactic acid fiber material still have good compatibility, so that the bio-based shape memory polylactic acid fiber material prepared by the present invention is toughened while maintaining a high shape memory recovery. DETAILED DESCRIPTION
[0021] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0022] In the following examples, the compound monomers and related reagents used can be purchased from the market. Among them, the polylactic acid fiber material was purchased from Yisheng New Materials (Suzhou) Co., Ltd.; the bio-based polyether fiber amide elastomer was purchased from Shanghai Mingyang Plastic Co., Ltd., with a brand number of 5533; polyethylene glycol monomethyl ether and allyl polyoxyethylene ether were purchased from Hai'an Petrochemical Plant, Jiangsu Province; SN-5027 was purchased from Guangzhou Yachuang Innovation Materials Co., Ltd.
[0023] Preparation of polycarboxylic acid dispersant A: Add 5 g of allyl polyoxyethylene ether and 10 mL of deionized water to a flask, stir for 5 min, then drop 5 g of methacrylic acid and 0.24 g of thioglycolic acid into the flask, stir at 130 r / min, slowly heat to 90°C, react at 90°C for 2 h, and then keep warm for 2 h. After the reaction is completed, spin dry the reaction solution, and then vacuum dry to obtain polycarboxylic acid dispersant A, the structural formula of which is
[0024]
[0025] Preparation of bio-based elastomer: Weigh each component according to Table 1, premix the bio-based polyetheramide elastomer at 200° C. and a rotation speed of 100 r / min for 3 minutes to completely melt it, and then add the modifier and continue blending for 10 minutes to obtain the bio-based elastomer.
[0026] The components and contents used to prepare the bio-based elastomer are shown in Table 1:
[0027] Table 1
[0028]
[0029]
[0030] The preparation methods of the bio-based shape memory polylactic acid fiber materials of Examples 1-7 all include the following steps:
[0031] The polylactic acid fiber material, the bio-based elastomer and the dispersant were melt-blended at a temperature of 170° C. and a rotation speed of 100 r / min for 10 minutes to obtain the bio-based shape memory polylactic acid fiber material.
[0032] The preparation method of the bio-based shape memory polylactic acid fiber material of Comparative Example 1 specifically includes the following steps: melt-blending the polylactic acid fiber material and the bio-based elastomer A at a temperature of 170°C and a rotation speed of 100 r / min for 10 minutes to obtain the bio-based shape memory polylactic acid fiber material.
[0033] The preparation method of the bio-based shape memory polylactic acid fiber material of Comparative Example 2 specifically includes the following steps: melt-blending the polylactic acid fiber material, polycarboxylic acid dispersant A, and bio-based polyetheramide elastomer at a temperature of 170°C and a rotation speed of 100r / min for 10 minutes to obtain a bio-based shape memory polylactic acid fiber material.
[0034] The preparation method of the bio-based shape memory polylactic acid fiber material of Comparative Example 3 specifically includes the following steps: melt-blending the polylactic acid fiber material, dispersant, and bio-based polyetheramide elastomer at a temperature of 170°C and a rotation speed of 100r / min for 10 minutes to obtain a bio-based shape memory polylactic acid fiber material.
[0035] Example 1 provides a bio-based shape memory polylactic acid fiber material, comprising 70 g of polylactic acid fiber material, 20 g of bio-based elastomer A, and 10 g of polycarboxylic acid dispersant A.
[0036] Example 2 provides a bio-based shape memory polylactic acid fiber material, comprising 70 g of polylactic acid fiber material, 20 g of bio-based elastomer B, and 10 g of polycarboxylic acid dispersant A.
[0037] Example 3 provides a bio-based shape memory polylactic acid fiber material, comprising 70 g of polylactic acid fiber material, 20 g of bio-based elastomer C, and 10 g of polycarboxylic acid dispersant A.
[0038] Example 4 provides a bio-based shape memory polylactic acid fiber material, comprising 70 g of polylactic acid fiber material, 20 g of bio-based elastomer D, and 10 g of polycarboxylic acid dispersant A.
[0039] Example 5 provides a bio-based shape memory polylactic acid fiber material, comprising 70 g of polylactic acid fiber material, 20 g of bio-based elastomer E, and 10 g of polycarboxylic acid dispersant A.
[0040] Example 6 provides a bio-based shape memory polylactic acid fiber material, comprising 70 g of polylactic acid fiber material, 20 g of bio-based elastomer A, and 10 g of dispersant, wherein the dispersant is SN-5027.
[0041] Example 7 provides a bio-based shape memory polylactic acid fiber material, comprising 70 g of polylactic acid fiber material, 20 g of bio-based elastomer C, and 10 g of dispersant, wherein the dispersant is SN-5027.
[0042] Comparative Example 1 provides a bio-based shape memory polylactic acid fiber material, comprising 70 g of polylactic acid fiber material and 20 g of bio-based elastomer A.
[0043] Comparative Example 2 provides a bio-based shape memory polylactic acid fiber material, comprising 70 g of polylactic acid fiber material, 20 g of bio-based polyetheramide elastomer and 10 g of polycarboxylic acid dispersant A.
[0044] Comparative Example 3: A bio-based shape memory polylactic acid fiber material is provided, comprising 70 g of polylactic acid fiber material, 20 g of bio-based polyetheramide elastomer, and 10 g of dispersant, wherein the dispersant is SN-5027.
[0045] The test method is as follows:
[0046] Tensile performance test: The size of the tensile test specimen is 63.5mm×12.7mm×3.2mm. According to ASTM D-638 standard, the test was performed 5 times at a tensile rate of 20mm / min, and the average value was taken;
[0047] Impact performance test: The impact test specimen size is 50.0mm×6.0mm×1.0mm. According to ASTM D-256 standard, the impact performance is tested at room temperature, and the test is repeated 5 times to obtain the average value.
[0048] Elastic recovery rate test: Instron 5500 fully digital electronic universal testing machine was used for testing.
[0049] Shape memory recovery time test: This test uses the time of shape recovery to characterize shape memory performance. The test sample is a spline specimen cut by a laser cutting machine, with a size of 60mm×10mm×5mm. The test spline is placed in 80℃ hot water for 10 minutes, then the spline is bent into a U shape with a diameter of 10mm, the spline is shaped, and then cooled to room temperature. The shaped spline is placed in hot water and the time is recorded. When the shape of the spline returns to a fixed form and the shape does not change within 5 minutes, the time recording is stopped.
[0050] The test results are shown in Table 1, as follows:
[0051] Table 1
[0052]
[0053]
[0054] From the comparison of Examples 1-3, it can be seen that when the mass ratio of the bio-based polyetheramide elastomer to the modifier and the mass ratio of glycidyl methacrylate, vinyl pyrrolidone and diisopropyl benzene peroxide in the modifier are within an appropriate range, the tensile properties and impact resistance are good, the shape memory recovery time is short, and the elastic recovery rate is high. When the mass ratio of the bio-based polyetheramide elastomer to the modifier is 1:0.05 and the ratio of glycidyl methacrylate, vinyl pyrrolidone and diisopropyl benzene peroxide in the modifier is 1:1:0.5, this type of bio-based shape memory polylactic acid fiber material has higher tensile properties and impact resistance, and at the same time, the shape memory recovery time is shorter and the elastic recovery rate is higher.
[0055] By comparing Examples 1-3 and 4-5, it can be seen that when the mass ratio of the bio-based polyetheramide elastomer to the modifier is in an appropriate range, the obtained bio-based shape memory polylactic acid fiber material has good tensile properties and impact resistance, a short shape memory recovery time, and a high elastic recovery rate, which improves the toughness of the polylactic acid fiber material while ensuring the shape memory properties of this type of fiber material.
[0056] From the comparison between Example 1 and Example 6-7, it can be seen that when the dispersant is not used with the structural formula When a polycarboxylic acid dispersant is used, even if the mass ratio of the modifier to the bio-based polyetheramide elastomer is within an appropriate range, the tensile properties, impact resistance, shape memory recovery time, elastic recovery rate and shape memory performance are all affected, and the lower the amount of modifier, the worse the effect. Even if the amount of modifier is increased, the effects of tensile properties, impact resistance, shape memory recovery time, elastic recovery rate and other aspects are improved, but they are still not ideal.
[0057] Comparison between Example 1 and Comparative Examples 1-3 shows that the modified bio-based polyetheramide elastomer and When a structural polycarboxylic acid dispersant is used in combination and the mass ratio of the modifier to the bio-based polyetheramide elastomer is within an appropriate range, this type of bio-based shape memory polylactic acid fiber material can have higher shape memory performance while improving toughness.
[0058] In summary, the bio-based shape memory polylactic acid fiber material provided by the present invention has good tensile properties and impact resistance, and has a short shape memory recovery time and a high elastic recovery rate. Moreover, when the polycarboxylic acid dispersant provided by the present invention is used, even if the amount of the modifier added is small, the bio-based elastomer and the polylactic acid fiber material still have good compatibility, so that the bio-based shape memory polylactic acid fiber material prepared by the present invention is toughened while maintaining a high shape memory recovery.
[0059] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A bio-based shape memory polylactic acid fiber material, characterized in that: The bio-based shape memory polylactic acid fiber material comprises the following components: polylactic acid fiber material, a bio-based elastomer and a dispersant; the raw materials for preparing the bio-based elastomer comprise a bio-based polyetheramide elastomer and a modifier, wherein the raw materials for preparing the modifier comprise glycidyl methacrylate, vinyl pyrrolidone and an initiator.
2. The bio-based shape memory polylactic acid fiber material according to claim 1, characterized in that: The mass ratio of the bio-based polyetheramide elastomer to the modifier is 1:(0.01-0.1).
3. The bio-based shape memory polylactic acid fiber material according to claim 1, characterized in that: The initiator is one or more of benzoyl peroxide, dicumyl peroxide and azobisisobutyronitrile.
4. The bio-based shape memory polylactic acid fiber material according to claim 1, characterized in that: The mass ratio of the glycidyl methacrylate, vinyl pyrrolidone and initiator is 1:(1-3):(0.1-0.5).
5. The bio-based shape memory polylactic acid fiber material according to claim 1, characterized in that: The preparation steps of the bio-based elastomer are as follows: premix 20-100g of bio-based polyetheramide elastomer at a temperature of 170-200°C and a rotation speed of 50-100r / min for 2-3min to make it completely melted, and then add 0.1-10g of modifier and continue blending for 5-10min.
6. The bio-based shape memory polylactic acid fiber material according to claim 1, characterized in that: The dispersant is a polycarboxylic acid dispersant having the following general structural formula: Wherein, p is selected from an integer of 1-3, and q is selected from an integer of 1-4.
7. The bio-based shape memory polylactic acid fiber material according to claim 1, characterized in that: The raw materials for preparing the polycarboxylic acid dispersant include methacrylic acid, allyl polyoxyethylene ether and a chain transfer agent.
8. The bio-based shape memory polylactic acid fiber material according to claim 7, characterized in that: The chain transfer agent comprises one or more of potassium persulfate, ammonium persulfate, and glycolic acid.
9. The bio-based shape memory polylactic acid fiber material according to claim 6, characterized in that: The preparation steps of the polycarboxylic acid dispersant are as follows: add 5-10g of allyl polyoxyethylene ether and 5-10mL of deionized water into a flask, stir for 3-5min, then drop 5-10g of methacrylic acid and 0.15-0.3g of a chain transfer agent into the flask respectively, stir at 100-150r / min, slowly heat to 80-100°C, react at 80-100°C for 2-3h, and then keep warm for 2-3h. After the reaction is completed, spin dry the reaction solution, and then vacuum dry to obtain the polycarboxylic acid dispersant.
10. The method for preparing the bio-based shape memory polylactic acid fiber material according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: melt-blending a bio-based elastomer, a dispersant and a polylactic acid fiber material at a temperature of 170-200° C. and a rotation speed of 50-100 r / min for 5-10 minutes to obtain a bio-based shape memory polylactic acid fiber material, wherein the mass ratio of the bio-based elastomer to the polylactic acid fiber material is 1:(3-9).
Citation Information
Cited By
Polybutylene succinate composite material as well as preparation method and application thereof
CN120682614A
Preparation method and application of dynamically crosslinked PLA / PBS material