Manufacturing and processing method of high-elastic super-soft luggage fabric

By optimizing raw material ratio and multi-step processing technology, combining the pre-mix and follow-up treatment of polyurethane elastic fibers, polyacrylonitrile fibers and bamboo fibers, the balance problem of existing fabrics between high elasticity and ultra-softness is solved, and the improvement of the balance of existing fabrics is improved. The comprehensive properties of fabrics, especially in terms of stretching, recovery, antibacterial and waterproofing.

CN118932548AInactive Publication Date: 2024-11-12YIXING DONGFANG LEATHER & PLASTIC CHEM
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411027971.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing bag fabrics are difficult to balance between high elasticity and ultra-softness, resulting in poor performance in stretching and recovery performance, and lack sufficient waterproof and antibacterial properties to meet the needs of the high-end market.

Method used

Using a high elastic and super soft bag fabric production and processing method, through optimizing raw material ratio and processing technology, including pre-mixing of polyurethane elastic fibers, polyacrylonitrile fibers and bamboo fibers, wet spinning, high-pressure steam treatment, and mechanical stretching It combines multi-step treatment to improve the overall performance of the fabric.

Benefits of technology

It achieves a perfect combination of high elasticity and ultra-softness, significantly improves the stretching and recovery performance of the fabric, enhances antibacterial and waterproof performance, and improves user comfort experience and product durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932548A_ABST
    Figure CN118932548A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of textile materials, in particular to a high-elastic super-soft luggage fabric manufacturing and processing method which comprises the following steps: S1, weighing polyurethane elastic fibers, polyacrylonitrile fibers, bamboo fibers and a cross-linking agent according to a preset proportion; s2, premixing the raw materials in a temperature-controlled and humidity-controlled environment; s3, spinning the raw materials pretreated in the step S2 through a spinning solution containing nano-particles; s4, performing high-pressure steam treatment on the spun fibers; s5, mechanically stretching the fibers subjected to steam treatment; s6, carrying out surface modification on the stretched fibers; s7, performing low-temperature plasma treatment on the modified fibers; and S8, carrying out comprehensive performance test on the fabric. According to the invention, through scientific raw material ratio and innovative multi-step processing technology, high elasticity and super softness of the fabric are realized, antibacterial performance, waterproof performance and durability of the fabric are remarkably improved, and the composite function requirements of high-end markets on luggage materials are effectively met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of textile materials, and in particular to a method for manufacturing and processing a high-elastic and ultra-soft luggage fabric. Background Art

[0002] In the current luggage industry, the choice of fabrics directly affects the functionality, durability and user comfort of the final product. Although there are many types of luggage fabrics on the market, such as nylon, polyester, etc., these traditional materials are usually difficult to balance between high elasticity and ultra-softness. High-elastic fabrics are often stiff and not easy to adapt to users' needs for comfort and flexibility; and although ultra-soft fabrics have a good touch, they often perform poorly in stretching and recovery properties, affecting the durability and practicality of the product. In addition, the waterproof and antibacterial properties of fabrics are also the focus of users' increasing attention. The performance of traditional fabrics in these aspects often cannot meet the needs of the high-end market.

[0003] In the face of these challenges, the present invention aims to address the defects in the prior art, especially to improve the comprehensive performance of luggage fabrics in terms of high elasticity and super softness. Current manufacturing technology cannot effectively combine the properties of high elasticity and super softness, and often sacrifices the performance of one aspect to improve the other.

[0004] Therefore, developing a new manufacturing method to achieve comprehensive improvement of fabric performance by optimizing raw material ratios and processing technology has become a major demand in the industry. Summary of the invention

[0005] Based on the above purpose, the present invention provides a method for manufacturing and processing high-elastic and ultra-soft luggage fabric.

[0006] A method for manufacturing and processing a high-elastic and ultra-soft luggage fabric comprises the following steps:

[0007] S1: Weigh polyurethane elastic fiber, polyacrylonitrile fiber, bamboo fiber and cross-linking agent according to a preset ratio;

[0008] S2: premix the raw materials weighed in S1 in a temperature and humidity controlled environment, and add antistatic agent and softener during the premixing process;

[0009] S3: Using wet spinning technology, the raw material pretreated in S2 is spun through a spinning solution containing nanoparticles;

[0010] S4: subjecting the spun fibers to high-pressure steam treatment to improve the physical structure of the fibers through high temperature and high pressure;

[0011] S5: mechanical stretching of the steam-treated fibers, supplemented by infrared irradiation;

[0012] S6: Using bio-enzyme technology to modify the surface of the stretched fiber to adjust the surface properties of the fiber;

[0013] S7: low-temperature plasma treatment of the modified fiber to improve the antibacterial and water-repellent properties of the fabric;

[0014] S8: After all treatments are completed, the fabric is subjected to comprehensive performance tests, including stretchability, abrasion resistance and comfort evaluation to ensure that the product meets the predetermined standards.

[0015] Furthermore, the preset proportions in S1 are 20-30% of polyurethane elastic fiber, 15-25% of polyacrylonitrile fiber, 37-62% of bamboo fiber, and 3-8% of cross-linking agent.

[0016] Furthermore, the S2 specifically includes:

[0017] S21: In an environment where the temperature is controlled at 20-25° C. and the relative humidity is controlled at 50-60%, the polyurethane elastic fiber, polyacrylonitrile fiber, bamboo fiber and cross-linking agent weighed in S1 are preliminarily mixed;

[0018] S22: During the preliminary mixing process, an antistatic agent is added in an amount of 0.1-0.3% by weight of the total weight of the raw materials, and stirring is continued at a speed of 500-600 rpm for 10-15 minutes;

[0019] S23: On the basis of S22, continue to add 0.2-0.5% of the total weight of the raw materials as a softener, and stir at a speed of 700-800 rpm for 20-30 minutes;

[0020] S24: After completing the pre-mixing process, the mixture is left to stand for 5-10 minutes to allow the components to fully react and combine.

[0021] Furthermore, the S3 specifically includes:

[0022] S31: mixing the raw material pretreated in S2 with a spinning solution containing nanoparticles in a mass ratio of 1:4, wherein the concentration of the nanoparticles is 0.05-0.1%;

[0023] S32: During the mixing process, the mixture is stirred at a temperature of 60-70° C. for 30-40 minutes;

[0024] S33: spinning the mixture through a wet spinning device, with the spinning speed controlled at 100-120 m / min and the flow rate of the spinning solution at 20-30 ml / min;

[0025] S34: During the spinning process, the coagulation bath temperature of the spinning solution is controlled at 10-15° C., and a coagulant with a mass ratio of 2-4% is added to the coagulation bath;

[0026] S35: After spinning is completed, the fiber is taken out from the coagulation bath and washed with water to remove the residual spinning solution and coagulant, and the washing temperature is controlled at 20-25°C.

[0027] Furthermore, the S4 specifically includes:

[0028] S41: placing the spun fiber into a high-pressure steam treatment device, wherein the temperature in the device is set to 180-200° C.;

[0029] S42: During the high pressure steam treatment, the pressure is controlled at 1.5-2.0 MPa, and the treatment time is 10-15 minutes;

[0030] S43: During the treatment process, the steam flow rate is controlled at 2-4 cubic meters per hour to ensure that the fibers are heated evenly;

[0031] S44: After the high pressure steam treatment is completed, the fiber is slowly cooled to room temperature, and the cooled fiber is taken out of the equipment to prepare for mechanical stretching and infrared irradiation treatment.

[0032] Furthermore, the S5 specifically includes:

[0033] S51: fixing the fiber treated with high-pressure steam and cooled to room temperature on a stretching device, and setting the stretching ratio to 1.5-2 times;

[0034] S52: During the mechanical stretching process, the stretching speed is controlled at 50-70 mm / min to ensure uniform stretching of the fiber; and infrared light with a wavelength of 800-1000 nm is used for irradiation at an intensity of 0.5-1 W / cm2;

[0035] S53: The infrared irradiation time is set to 10-20 minutes to maintain the temperature of the fiber stable during the stretching process;

[0036] S54: After the stretching and infrared irradiation treatments are completed, the fiber is naturally cooled at room temperature.

[0037] Furthermore, the S6 specifically includes:

[0038] S61: soaking the mechanically stretched and cooled fiber in a biological enzyme solution, wherein the concentration of the biological enzyme solution is 0.1-0.2%;

[0039] S62: During the soaking process, the solution temperature is maintained at 30-40° C., and slight stirring is maintained at a stirring speed of 100-150 rpm, and the soaking time is 30-40 minutes;

[0040] S63: After the soaking is completed, the fiber is taken out and rinsed with deionized water for 10-15 minutes to remove excess biological enzyme solution;

[0041] S64: drying the washed fiber in an environment of 60-70°C to ensure the bioenzyme modification effect on the fiber surface;

[0042] S65: After drying, the fiber is left to stand for 5-10 minutes to cool to room temperature.

[0043] Furthermore, the S7 specifically includes:

[0044] S71: placing the fiber modified by the biological enzyme and cooled to room temperature in a low-temperature plasma treatment device;

[0045] S72: In the processing equipment, the vacuum degree is set to 0.1-0.5 Pa, and the processing gas is a mixed gas of oxygen and fluorinated gas, with a mixing ratio of 1:1;

[0046] S73: The power of the plasma treatment is set to 100-200 watts, and the treatment time is 10-20 minutes;

[0047] S74: During the treatment process, the gas flow rate is controlled at 50-100 ml / min;

[0048] S75: After the low-temperature plasma treatment, the fiber is placed in an inert gas environment for 5-10 minutes to prevent the fiber surface from coming into contact with air and causing oxidation reaction.

[0049] Furthermore, the S8 specifically includes:

[0050] S81: Conduct stretch test on fabrics treated with low-temperature plasma using a standard stretch tester with a test speed of 100 mm / min and a stretch range of 80% of the initial length. The maximum tensile strength should be between 20 and 30 MPa, and the elongation should be between 200 and 300%.

[0051] S82: Abrasion resistance test is conducted using a standard abrasion test machine with a load of 500 grams for 2,000 friction cycles on the fabric surface. The mass loss of the fabric should be less than 5%.

[0052] S83: Perform comfort evaluation, use an air permeability tester to test the air permeability of the fabric, the air flow rate is set to 200 ml / min, and the standard of the air permeability resistance value of the fabric should be between 50-150 Pa;

[0053] S84: For softness test, a standard softness test instrument is used to perform compression test on the fabric with a pressure of 20 Newtons. The standard for the compression deformation of the fabric should be less than 10%, and the standard for the recovery performance should be greater than 90%.

[0054] Beneficial effects of the present invention:

[0055] The present invention achieves a perfect combination of high elasticity and ultra-softness by optimizing the raw material ratio and processing technology. Specifically, the polyurethane elastic fiber provides excellent elasticity and resilience, the polyacrylonitrile fiber enhances the structural strength and durability of the fabric, and the bamboo fiber gives the fabric a natural soft touch and excellent air permeability. Through the scientific ratio of the raw materials, the fabric performs well in stretching and recovery properties, and at the same time has excellent softness, which significantly improves the user's comfort experience.

[0056] The present invention further optimizes the physical properties of the fiber by adopting a multi-step treatment method including high-pressure steam treatment, mechanical stretching and infrared irradiation. The high-pressure steam treatment improves the uniformity and compactness of the fiber, while the mechanical stretching and infrared irradiation enhance the arrangement and physical properties of the fiber. The application of biological enzyme and low-temperature plasma treatment technology not only modifies the surface properties of the fiber, but also significantly improves the antibacterial and waterproof properties of the fabric. The organic combination of these treatment steps enables the fabric to have excellent protective properties while maintaining high elasticity and softness. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0058] Figure 1 Schematic diagram of a method for manufacturing a high-elastic and ultra-soft luggage fabric according to an embodiment of the present invention;

[0059] Figure 2 It is a schematic diagram of the wet spinning process of an embodiment of the present invention. DETAILED DESCRIPTION

[0060] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0061] It should be noted that, unless otherwise defined, the technical terms or scientific terms used in the present invention should be understood by people with ordinary skills in the field to which the present invention belongs. The "first", "second" and similar words used in the present invention do not indicate any order, quantity or importance, but are only used to distinguish different components. "Include" or "comprise" and similar words mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects. "Connect" or "connected" and similar words are not limited to physical or mechanical connections, but may include electrical connections, whether direct or indirect. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.

[0062] Example 1

[0063] like Figure 1-2 As shown, a method for manufacturing and processing high-elastic and ultra-soft luggage fabrics comprises the following steps:

[0064] S1: Weigh polyurethane elastic fiber, polyacrylonitrile fiber, bamboo fiber and cross-linking agent according to a preset ratio;

[0065] S2: premixing the raw materials weighed in S1 in a temperature and humidity controlled environment, and adding antistatic agent and softener during the premixing process to prepare for the spinning process;

[0066] S3: Using wet spinning technology, the raw material pretreated in S2 is spun through a spinning solution containing nanoparticles, and the nanoparticles play a reinforcing role in the fiber formation process;

[0067] S4: The spun fibers are subjected to high-pressure steam treatment to improve the physical structure of the fibers through high temperature and high pressure, making the fibers more uniform and compact;

[0068] S5: Mechanically stretch the steam-treated fibers and irradiate them with infrared rays to make the fibers more evenly arranged and improve their physical properties;

[0069] S6: Use bio-enzyme technology to modify the surface of the stretched fiber to adjust the surface properties of the fiber and optimize the softness and breathability of the final product;

[0070] S7: low-temperature plasma treatment of the modified fiber to improve the antibacterial and water-repellent properties of the fabric;

[0071] S8: After all treatments are completed, the fabric is subjected to comprehensive performance tests, including stretchability, abrasion resistance and comfort evaluation to ensure that the product meets the predetermined standards.

[0072] The preset proportions in S1 are 25% polyurethane elastic fiber, 20% polyacrylonitrile fiber, 50% bamboo fiber, and 5% cross-linking agent.

[0073] S2 specifically includes:

[0074] S21: In an environment where the temperature is controlled at 3°C ​​and the relative humidity is controlled at 55%, the polyurethane elastic fiber, polyacrylonitrile fiber, bamboo fiber and cross-linking agent weighed in S1 are preliminarily mixed;

[0075] S22: During the preliminary mixing process, an antistatic agent was added in an amount of 0.2% by weight of the total raw material, and stirring was continued at a speed of 550 rpm for 13 minutes to ensure that the antistatic agent was evenly distributed;

[0076] S23: On the basis of S22, 0.4% of the total weight of the raw material softener is added, and the mixture is stirred at a speed of 750 rpm for 25 minutes to allow the softener to fully penetrate into the fiber;

[0077] S24: After the premixing process is completed, the mixture is allowed to stand for 7 minutes to allow the components to fully react and combine in preparation for the subsequent wet spinning step.

[0078] S3 specifically includes:

[0079] S31: mixing the raw material pretreated in S2 with the spinning solution containing nanoparticles in a mass ratio of 1:4, and the concentration of the nanoparticles is 0.08%;

[0080] S32: During the mixing process, the mixture is stirred at a temperature of 65° C. for 35 minutes to allow the nanoparticles to be evenly distributed in the raw material;

[0081] S33: spinning the mixture through a wet spinning device, the spinning speed is controlled at 110 m / min, and the flow rate of the spinning solution is 25 ml / min;

[0082] S34: During the spinning process, the coagulation bath temperature of the spinning solution is controlled at 13° C., and a coagulant having a mass ratio of 3% is added to the coagulation bath;

[0083] S35: After spinning is completed, the fiber is taken out from the coagulation bath and washed with water to remove the residual spinning solution and coagulant, and the washing temperature is controlled at 23°C.

[0084] S4 specifically includes:

[0085] S41: placing the spun fiber into a high-pressure steam treatment device, wherein the temperature in the device is set to 190° C.;

[0086] S42: During the high pressure steam treatment, the pressure is controlled at 1.5-2.0 MPa, and the treatment time is 12 minutes;

[0087] S43: During the treatment, the steam flow rate is controlled at 3 cubic meters per hour to ensure that the fibers are heated evenly;

[0088] S44: After the high-pressure steam treatment is completed, the fiber is slowly cooled to room temperature to avoid changes in fiber properties caused by rapid cooling, and the cooled fiber is removed from the equipment in preparation for mechanical stretching and infrared irradiation treatment.

[0089] S5 specifically includes:

[0090] S51: fixing the fiber treated with high-pressure steam and cooled to room temperature on a stretching device, and setting the stretching ratio to 1.8 times;

[0091] S52: During the mechanical stretching process, the stretching speed is controlled at 60 mm / min to ensure uniform stretching of the fiber; infrared light with a wavelength of 900 nm is used for irradiation at an intensity of 0.8 W / cm2;

[0092] S53: The infrared irradiation time was set to 15 minutes to maintain the temperature of the fiber stable during the stretching process;

[0093] S54: After the stretching and infrared irradiation treatments are completed, the fiber is naturally cooled at room temperature.

[0094] S6 specifically includes:

[0095] S61: soaking the mechanically stretched and cooled fiber in a biological enzyme solution, wherein the concentration of the biological enzyme solution is 0.15%;

[0096] S62: During the soaking process, the temperature of the solution was maintained at 35° C., and slight stirring was maintained at a stirring speed of 130 rpm. The soaking time was 35 minutes.

[0097] S63: After the soaking is completed, the fiber is taken out and rinsed with deionized water for 13 minutes to remove excess biological enzyme solution;

[0098] S64: drying the washed fiber in an environment of 65°C to ensure the bioenzyme modification effect on the fiber surface;

[0099] S65: After drying, the fiber is left to stand for 8 minutes to cool to room temperature in preparation for the next step of low-temperature plasma treatment.

[0100] S7 specifically includes:

[0101] S71: placing the fiber modified by the biological enzyme and cooled to room temperature in a low-temperature plasma treatment device;

[0102] S72: In the processing equipment, the vacuum degree is set to 0.3 Pa, and the processing gas is a mixed gas of oxygen and fluorinated gas, and the mixing ratio is 1:1;

[0103] S73: The power of plasma treatment was set to 150 watts and the treatment time was 15 minutes to ensure that the fiber surface was fully treated;

[0104] S74: During the treatment process, the gas flow rate is controlled at 80 ml / min to ensure the stability of the treatment environment;

[0105] S75: After the low-temperature plasma treatment, the fiber is placed in an inert gas environment for 8 minutes to prevent the fiber surface from coming into contact with air and causing oxidation reaction.

[0106] S8 specifically includes:

[0107] S81: Conduct stretch test on fabrics treated with low-temperature plasma using a standard stretch tester with a test speed set at 100 mm / min, a stretch range set at 80% of the initial length, a maximum tensile strength of 30 MPa, and an elongation of 300%;

[0108] S82: Abrasion resistance test was conducted using a standard abrasion tester with a load of 500 grams for 2,000 friction cycles on the fabric surface, with a mass loss of 2%;

[0109] S83: Perform comfort evaluation using an air permeability tester to test the air permeability of the fabric. The air flow rate is set to 200 ml / min and the air permeability resistance of the fabric is 70 Pa.

[0110] S84: Softness test, using a standard softness tester, compression test on the fabric with a pressure of 20 Newtons, the compression deformation of the fabric is 2%, and the recovery performance is 98%.

[0111] Example 2

[0112] S1: First, various raw materials are weighed according to the preset proportions, with polyurethane elastic fiber accounting for 20%, polyacrylonitrile fiber accounting for 15%, bamboo fiber accounting for 62%, and cross-linking agent accounting for 3%, which provides a basis for the next step of mixing;

[0113] S2: Pre-mixing the raw materials in a temperature and humidity controlled environment, with the ambient temperature controlled at 20°C and the relative humidity controlled at 50%. During the preliminary mixing process, 0.1% of the total weight of the raw materials was added as an antistatic agent, and the mixture was stirred at 500 rpm for 10 minutes; then 0.2% of the total weight of the raw materials as a softener was added, and the mixture was stirred at 700 rpm for 20 minutes. The mixture was left to stand for 5 minutes to ensure that the components were fully reacted and combined;

[0114] S3: spinning the pretreated raw material through a spinning solution containing nanoparticles, the concentration of the nanoparticles is 0.05%, the mass ratio of the spinning solution to the raw material is 1:4, the mixture is stirred at 60°C for 30 minutes, and then spinning through a wet spinning device, the spinning speed is 100 m / min, the flow rate of the spinning solution is 20 ml / min, the temperature of the coagulation bath is controlled at 10°C, and a coagulant with a mass ratio of 2% is added; after spinning, washing with water at 20°C is used to remove the residual spinning solution and coagulant;

[0115] S4: The spun fiber is placed in a high-pressure steam treatment device. The temperature in the device is set to 180°C, the pressure is controlled at 1.5MPa, the treatment time is 10 minutes, and the steam flow rate is 2 cubic meters per hour to ensure that the fiber is heated evenly;

[0116] S5: The fiber treated with high-pressure steam and cooled to room temperature is fixed on a stretching device, the stretching ratio is set to 1.5 times, the stretching speed is 50 mm / min, and at the same time, infrared light with a wavelength of 800 nm is used for irradiation, the irradiation intensity is 0.5 W / cm2, and the irradiation lasts for 10 minutes to maintain the temperature of the fiber stable during the stretching process;

[0117] S6: The mechanically stretched and cooled fibers are immersed in a biological enzyme solution with a concentration of 0.1%. The solution temperature is maintained at 30°C and stirred slightly at a speed of 100 rpm. The immersion time is 30 minutes, the rinsing time is 10 minutes, and then dried in an environment of 60°C. After drying, the fibers are left to stand for 5 minutes to cool to room temperature.

[0118] S7: The fiber modified by the enzyme and cooled to room temperature is placed in a low-temperature plasma treatment device, the vacuum degree of the treatment device is set to 0.1 Pa, a mixed gas of oxygen and fluorinated gas (mixing ratio is 1:1) is used, the power of the plasma treatment is set to 100 watts, the treatment time is 10 minutes, the gas flow rate is controlled at 50 ml / min, and after completion, it is left to stand in an inert gas environment for 5 minutes;

[0119] S8: Comprehensive performance test was conducted on the fabrics treated with low-temperature plasma. The speed of the tensile test was set to 100 mm / min, the stretching range was set to 80% of the initial length, the maximum tensile strength was 25 MPa, and the elongation was 270%. The wear resistance test was conducted with a load of 500 g, 2000 friction cycles on the fabric surface, and a mass loss of 4%. The air permeability test was conducted with an air flow rate of 200 ml / min, and the air permeability resistance value of the fabric was 110 Pa. The softness test was conducted with a compression pressure of 20 Newtons, a compression deformation of 5%, and a recovery performance of 95%.

[0120] Example 3

[0121] S1: First, various raw materials are weighed according to the preset proportions, with polyurethane elastic fiber accounting for 30%, polyacrylonitrile fiber accounting for 25%, bamboo fiber accounting for 37%, and cross-linking agent accounting for 8%, which provides a basis for the next step of mixing;

[0122] S2: Pre-mixing the raw materials in a temperature and humidity controlled environment, with the ambient temperature controlled at 25°C and the relative humidity controlled at 60%. During the preliminary mixing process, 0.3% of the total weight of the raw materials was added as an antistatic agent, and the mixture was stirred at 600 rpm for 15 minutes; then 0.5% of the total weight of the raw materials as a softener was added, and the mixture was stirred at 800 rpm for 30 minutes, and the mixture was left to stand for 10 minutes to ensure that the components were fully reacted and combined;

[0123] S3: spinning the pretreated raw material through a spinning solution containing nanoparticles, the concentration of the nanoparticles is 0.1%, the mass ratio of the spinning solution to the raw material is 1:4, the mixture is stirred at 70°C for 40 minutes, and then spinning through a wet spinning device, the spinning speed is 120 m / min, the flow rate of the spinning solution is 30 ml / min, the temperature of the coagulation bath is controlled at 15°C, and a coagulant with a mass ratio of 4% is added; after spinning, washing with water at 25°C to remove the residual spinning solution and coagulant;

[0124] S4: The spun fibers are placed in a high-pressure steam treatment device. The temperature in the device is set to 200°C, the pressure is controlled at 2.0 MPa, the treatment time is 15 minutes, and the steam flow rate is 4 cubic meters per hour to ensure that the fibers are heated evenly.

[0125] S5: The fiber treated with high-pressure steam and cooled to room temperature is fixed on a stretching device, the stretching ratio is set to 2 times, the stretching speed is 70 mm / min, and at the same time, infrared light with a wavelength of 1000 nm is used for irradiation, the irradiation intensity is 1 W / cm2, and the irradiation lasts for 20 minutes to maintain the temperature of the fiber stable during the stretching process;

[0126] S6: The mechanically stretched and cooled fibers are immersed in a biological enzyme solution with a concentration of 0.2%. The solution temperature is maintained at 40°C and is gently stirred at a speed of 150 rpm. The immersion time is 40 minutes, the rinsing time is 15 minutes, and then the fibers are dried in an environment of 70°C. After drying, the fibers are left to stand for 10 minutes to cool to room temperature.

[0127] S7: The fiber modified by the bio-enzyme and cooled to room temperature is placed in a low-temperature plasma treatment device, the vacuum degree of the treatment device is set to 0.5 Pa, a mixed gas of oxygen and fluorinated gas (mixing ratio is 1:1) is used, the power of the plasma treatment is set to 200 watts, the treatment time is 20 minutes, the gas flow rate is controlled at 100 ml / min, and after completion, it is left to stand in an inert gas environment for 10 minutes;

[0128] S8: Conduct comprehensive performance tests on fabrics treated with low-temperature plasma. The speed of the tensile test is set to 100 mm / min, the stretching range is set to 80% of the initial length, the maximum tensile strength is 30 MPa, and the elongation is 200%. The wear resistance test is conducted with a load of 500 g, 2000 friction cycles on the fabric surface, and a mass loss of 5%. The breathability test is conducted with an air flow rate of 200 ml / min and a breathability resistance value of 150 Pa. The softness test is compressed with a pressure of 20 Newtons, a compression deformation of 8%, and a recovery performance of 90%.

[0129] Table 1 Comparison of comprehensive performance tests of finished products

[0130] index Embodiment 1 Embodiment 2 Embodiment 3 Tensile strength(MPa) 30 25 30 Elongation(%) 300 270 200 Wear resistance loss (%) 2 4 5 Air permeability resistance value (Pa) 70 110 150 Compression deformation (%) 2 5 8 Recovery performance (%) 98 95 90

[0131] It can be seen from Table 1 above that Example 1 performs well in multiple key performance indicators, specifically tensile strength and elongation: Example 1 shows the highest tensile strength and elongation, indicating that it has excellent elasticity and bearing capacity, which are key indicators of high elasticity and ultra-soft fabrics; Example 1 has the lowest wear resistance loss, which is only 2%, indicating that its durability is better than other examples; Example 1 has the lowest air permeability resistance value, which is 70 Pa, which means that it has better air permeability, which is particularly important for products that need to be worn or used for a long time; Softness Compression Deformation and Recovery Performance Example 1 also showed the best performance in these two tests, with the lowest compression deformation and the highest recovery performance, indicating that the fabric is soft and can return to its original state after being subjected to pressure, enhancing the user's comfort.

[0132] Table 2 Comparison of other performances

[0133] index Embodiment 1 Embodiment 2 Embodiment 3 Antistatic property(kV) 0.5 1 1.5 Color retention (%) 95 90 85 UV blocking rate (%) 99 97 95 Antibacterial effect (%) 99.9 99 98 Thermal stability(℃) 250 240 230 Environmental adaptability Excellent good generally

[0134] As can be seen from Table 2 above, Example 1 has the lowest static electricity accumulation (0.5 kV), which is crucial to improving user comfort and safety, especially when using luggage products in a dry environment; Example 1 has the highest color retention after washing (95%), indicating that its color fastness is excellent, which is particularly important for products that are frequently washed or used for a long time; Example 1 provides almost complete UV protection (99%), which is very beneficial for luggage used outdoors and can effectively protect items in the bag from ultraviolet damage; Example 1 has the highest antibacterial effect (99.9%), which can effectively prevent bacterial growth and improve product hygiene and user health; Example 1 remains stable at a higher temperature (250°C), indicating that it is more applicable under extreme temperatures; Example 1 performs well under various environmental conditions, demonstrating its excellent adaptability and is suitable for various climates and geographical environments.

[0135] Table 3 Comparison of special functionality

[0136]

[0137]

[0138] It can be seen from Table 3 above that Example 1 is superior to Example 2 and Example 3 in all performance tests. Specifically, Example 1 has the best anti-bending performance and can withstand more folding times without damage, indicating that it is more suitable for environments that are often carried or used multiple times; Example 1 shows higher tensile strength, indicating that its structure is more stable and durable, and is suitable for bearing larger physical loads; Example 1 has the highest waterproof grade, which is very important for luggage materials used outdoors or in humid environments; Example 1 also shows a higher percentage in chemical resistance, indicating that it can better resist the erosion of chemicals and increase the service life of the product; Example 1 has the lowest thermal conductivity, which means that it is better in thermal insulation performance and is suitable for protecting sensitive items; Example 1 performs best in lightweight material, which helps to reduce the burden on users, especially when heavy objects need to be carried or used for a long time.

[0139] Based on the data in the above three performance comparison tables, Example 1 shows excellent performance in multiple key performance indicators, which is significantly better than Example 2 and Example 3. These indicators include but are not limited to tensile strength, abrasion resistance, air permeability, softness, antistatic property, UV blocking rate, antibacterial effect, folding resistance, tensile strength and waterproofness. The excellent performance of Example 1 is due to its optimized raw material ratio and sophisticated processing technology, which effectively improves the durability, comfort and functionality of the fabric. Therefore, Example 1 not only meets the demand of the high-end market for high-performance fabrics, but also demonstrates the innovation and practicality of the method of the present invention, and is an ideal choice in the field of high-elastic and ultra-soft luggage fabrics.

[0140] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for producing and processing highly elastic and ultra-soft luggage fabrics, characterized in that: The following steps are involved: S1: Weigh polyurethane elastic fiber, polyacrylonitrile fiber, bamboo fiber and cross-linking agent according to a preset ratio; S2: premix the raw materials weighed in S1 in a temperature and humidity controlled environment, and add antistatic agent and softener during the premixing process; S3: Using wet spinning technology, the raw material pretreated in S2 is spun through a spinning solution containing nanoparticles; S4: subjecting the spun fibers to high-pressure steam treatment to improve the physical structure of the fibers through high temperature and high pressure; S5: mechanical stretching of the steam-treated fibers, supplemented by infrared irradiation; S6: Using bio-enzyme technology to modify the surface of the stretched fiber to adjust the surface properties of the fiber; S7: low-temperature plasma treatment of the modified fiber to improve the antibacterial and water-repellent properties of the fabric; S8: After all treatments are completed, the fabric is subjected to comprehensive performance tests, including stretchability, abrasion resistance and comfort evaluation to ensure that the product meets the predetermined standards.

2. The method for manufacturing and processing high-elastic and ultra-soft luggage fabric according to claim 1, characterized in that: The preset proportions in S1 are 20-30% of polyurethane elastic fiber, 15-25% of polyacrylonitrile fiber, 37-62% of bamboo fiber, and 3-8% of cross-linking agent.

3. The method for manufacturing and processing high-elastic and ultra-soft luggage fabric according to claim 1, characterized in that: The S2 specifically includes: S21: In an environment where the temperature is controlled at 20-25° C. and the relative humidity is controlled at 50-60%, the polyurethane elastic fiber, polyacrylonitrile fiber, bamboo fiber and cross-linking agent weighed in S1 are preliminarily mixed; S22: During the preliminary mixing process, an antistatic agent is added in an amount of 0.1-0.3% by weight of the total weight of the raw materials, and stirring is continued at a speed of 500-600 rpm for 10-15 minutes; S23: On the basis of S22, continue to add 0.2-0.5% of the total weight of the raw materials as a softener, and stir at a speed of 700-800 rpm for 20-30 minutes; S24: After completing the pre-mixing process, the mixture is left to stand for 5-10 minutes to allow the components to fully react and combine.

4. The method for manufacturing and processing high-elastic and ultra-soft luggage fabric according to claim 1, characterized in that: The S3 specifically includes: S31: mixing the raw material pretreated in S2 with a spinning solution containing nanoparticles in a mass ratio of 1:4, wherein the concentration of the nanoparticles is 0.05-0.1%; S32: During the mixing process, the mixture is stirred at a temperature of 60-70° C. for 30-40 minutes; S33: spinning the mixture through a wet spinning device, with the spinning speed controlled at 100-120 m / min and the flow rate of the spinning solution at 20-30 ml / min; S34: During the spinning process, the coagulation bath temperature of the spinning solution is controlled at 10-15° C., and a coagulant with a mass ratio of 2-4% is added to the coagulation bath; S35: After spinning is completed, the fiber is taken out from the coagulation bath and washed with water to remove the residual spinning solution and coagulant, and the washing temperature is controlled at 20-25°C.

5. The method for manufacturing and processing high-elastic and ultra-soft luggage fabric according to claim 1, characterized in that: The S4 specifically includes: S41: placing the spun fiber into a high-pressure steam treatment device, wherein the temperature in the device is set to 180-200° C.; S42: During the high pressure steam treatment, the pressure is controlled at 1.5-2.0 MPa, and the treatment time is 10-15 minutes; S43: During the treatment process, the steam flow rate is controlled at 2-4 cubic meters per hour to ensure that the fibers are heated evenly; S44: After the high pressure steam treatment is completed, the fiber is slowly cooled to room temperature, and the cooled fiber is taken out of the equipment to prepare for mechanical stretching and infrared irradiation treatment.

6. The method for manufacturing and processing high-elastic and ultra-soft luggage fabric according to claim 1, characterized in that: The S5 specifically includes: S51: fixing the fiber treated with high pressure steam and cooled to room temperature on a stretching device, and setting the stretching ratio to 1.5-2 times; S52: During the mechanical stretching process, the stretching speed is controlled at 50-70 mm / min to ensure uniform stretching of the fiber; and infrared light with a wavelength of 800-1000 nm is used for irradiation at an intensity of 0.5-1 W / cm2; S53: The infrared irradiation time is set to 10-20 minutes to maintain the temperature of the fiber stable during the stretching process; S54: After the stretching and infrared irradiation treatments are completed, the fiber is naturally cooled at room temperature.

7. The method for manufacturing and processing high-elastic and ultra-soft luggage fabric according to claim 1, characterized in that: The S6 specifically includes: S61: soaking the mechanically stretched and cooled fiber in a biological enzyme solution, wherein the concentration of the biological enzyme solution is 0.1-0.2%; S62: During the soaking process, the solution temperature is maintained at 30-40° C., and slight stirring is maintained at a stirring speed of 100-150 rpm, and the soaking time is 30-40 minutes; S63: After the soaking is completed, the fiber is taken out and rinsed with deionized water for 10-15 minutes to remove excess biological enzyme solution; S64: drying the washed fiber in an environment of 60-70°C to ensure the bioenzyme modification effect on the fiber surface; S65: After drying, the fiber is left to stand for 5-10 minutes to cool to room temperature.

8. The method for manufacturing and processing high-elastic and ultra-soft luggage fabric according to claim 1, characterized in that: The S7 specifically includes: S71: placing the fiber modified by the biological enzyme and cooled to room temperature in a low-temperature plasma treatment device; S72: In the processing equipment, the vacuum degree is set to 0.1-0.5 Pa, and the processing gas is a mixed gas of oxygen and fluorinated gas, with a mixing ratio of 1:1; S73: The power of the plasma treatment is set to 100-200 watts, and the treatment time is 10-20 minutes; S74: During the treatment process, the gas flow rate is controlled at 50-100 ml / min; S75: After the low-temperature plasma treatment, the fiber is placed in an inert gas environment for 5-10 minutes to prevent the fiber surface from coming into contact with air and causing oxidation reaction.

9. The method for manufacturing and processing high-elastic and ultra-soft luggage fabric according to claim 1, characterized in that: The S8 specifically includes: S81: Conduct stretch test on fabrics treated with low-temperature plasma using a standard stretch tester with a test speed of 100 mm / min and a stretch range of 80% of the initial length. The maximum tensile strength should be between 20 and 30 MPa, and the elongation should be between 200 and 300%. S82: Abrasion resistance test is conducted using a standard abrasion test machine with a load of 500 grams for 2,000 friction cycles on the fabric surface. The mass loss of the fabric should be less than 5%. S83: Perform comfort evaluation, use an air permeability tester to test the air permeability of the fabric, the air flow rate is set to 200 ml / min, and the standard of the air permeability resistance value of the fabric should be between 50-150 Pa; S84: For softness test, a standard softness test instrument is used to perform compression test on the fabric with a pressure of 20 Newtons. The standard for the compression deformation of the fabric should be less than 10%, and the standard for the recovery performance should be greater than 90%.

Citation Information

Patent Citations

  • Treatment method of super-soft textile fabric

    CN108532300A

  • High-strength antibacterial fabric and preparation process thereof

    CN117385650A

  • Tencel fiber and silver ion composite fiber fabric and manufacturing method therefor

    WO2021243934A1