Preparation method and application of ceramic nanofiber and silicon carbide fiber composite material

Through double-needle electrospinning technology and the design of cross-net structures, ceramic nanofiber and silicon carbide fiber composite materials with excellent high temperature resistance and mechanical properties were prepared, which solved the problem of insufficient material performance in the prior art and realized the use of Application in the field of electronic semiconductors.

CN118932549APending Publication Date: 2024-11-12JIAXING FREBANG NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410995706.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

It is difficult to prepare ceramic nanofiber and silicon carbide fiber composites with good high temperature resistance and mechanical properties in the prior art, and the preparation process is difficult to produce in large quantities.

Method used

The ceramic nanofiber and silicon carbide fiber composites were prepared by double-needle electrospinning technology. By adding (R)-A-lipoic acid terematramine and lignin-based resin to the precursor solution, the cross-net structure was formed. Improve viscoelasticity and mechanical strength and form composite materials through calcination steps.

Benefits of technology

It has achieved high temperature resistance and excellent mechanical properties of ceramic nanofibers and silicon carbide fiber composites, and is suitable for electronic semiconductor fields and has good market value.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of fibers, and provides a preparation method and application of a ceramic nanofiber and silicon carbide fiber composite material, and the preparation method comprises the following steps: S1, dissolving an aluminum source in an organic solvent, adding (R)-A-lipoic acid tromethamine salt, stirring for 30-80 min, then adding a stabilizer, and stirring for 40-100 min to obtain a precursor solution 1; s2, dissolving sodium metasilicate nonahydrate into absolute ethyl alcohol to obtain a silicon-containing solution, dropwise adding deionized water while stirring, then adding lignin-based resin, stirring for 2-4 hours, adding acetone, and mixing to obtain a precursor solution 2; s3, performing double-needle electrostatic spinning on the precursor solution 1 and the precursor solution 2 in equal volume to obtain a film-shaped composite material; and S4, calcining the film-shaped composite material to obtain the ceramic nanofiber and silicon carbide fiber composite material. The composite material disclosed by the invention has the characteristics of high temperature resistance and good mechanical property, is applied to the field of electronic semiconductors, and has better market value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of fiber technology, and specifically relates to a preparation method and application of a ceramic nanofiber and silicon carbide fiber composite material. Background Art

[0002] With the rapid development of modern industry, the demand for high-performance materials is growing, especially in the fields of aviation, aerospace, automobiles, electronics, etc. The demand for lightweight, high-strength, heat-resistant and corrosion-resistant materials is rising. For example, it can be used to manufacture aircraft thermal protection systems and rocket engine insulation materials; it can be used to manufacture lightweight components to improve fuel efficiency and performance; it can also be used as a high-performance electronic packaging material to improve the reliability and stability of electronic equipment.

[0003] Silicon carbide has excellent properties such as high critical breakdown voltage and high carrier saturation drift velocity, and has great development potential in high-frequency semiconductor devices. Silicon carbide fiber has heat resistance, oxidation resistance and chemical stability. However, silicon carbide fiber has poor resistance to ablation and particle erosion. Selecting specific ceramic materials and compounding them with silicon carbide fibers can give full play to their respective advantages and form a new composite material with better performance.

[0004] Chinese patent CN 114908474A discloses a technology for preparing ultra-high purity flexible ceramic fibers and films used in the field of electronics and semiconductors. By selecting and controlling the molecular structure, element composition, purity, liquid solidification method, molding technology and ceramicization process of metal organic prepolymers, flexible ceramic materials are prepared and produced, and the total content of trace polluting elements is controlled to be less than 10ppm, thereby preparing electronic and semiconductor-grade flexible ceramic materials with 5 9s, 6 9s or higher purity, and the prepared related ceramic materials can meet the requirements of application in the field of electronics and semiconductors. However, the technical process of its preparation is difficult, and the requirements for equipment are also high, making it difficult to popularize production in large quantities.

[0005] Therefore, there is an urgent need to develop a ceramic nanofiber and silicon carbide fiber composite material that has the characteristics of high temperature resistance and excellent mechanical properties. Summary of the invention

[0006] In view of the existing technical problems, the purpose of the present invention is to provide a preparation and application of a ceramic nanofiber and silicon carbide fiber composite material. The composite material of the present invention has the characteristics of high temperature resistance and good mechanical properties, can be used in the field of electronic semiconductors, and has good market value.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0008] In one aspect, the present invention provides a method for preparing a composite material of ceramic nanofibers and silicon carbide fibers, comprising the following steps:

[0009] S1. dissolving an aluminum source in an organic solvent, adding (R)-A-lipoic acid tromethamine salt, stirring for 30-80 min, then adding a stabilizer, stirring for 40-100 min, and obtaining a precursor solution 1;

[0010] S2. Dissolve sodium metasilicate nonahydrate in anhydrous ethanol to obtain a silicon-containing solution, add deionized water dropwise while stirring, then add lignin-based resin, stir for 2-4 hours, add acetone and mix to obtain a precursor solution 2; wherein the mass ratio of sodium metasilicate nonahydrate to anhydrous ethanol is 1:(10-15);

[0011] S3. placing equal volumes of precursor solution 1 and precursor solution 2 in two syringes of a double-needle electrospinning machine, respectively, and performing double-needle electrospinning to obtain a film-like composite material;

[0012] S4. calcining the membrane-like composite material obtained in step S3 to obtain a composite material of ceramic nanofibers and silicon carbide fibers.

[0013] The reaction mechanism and effects of the present invention are as follows:

[0014] 1. In the precursor solution 1, (R)-A-lipoic acid tromethamine salt will chelate with free aluminum ions, thereby increasing the solubility of the aluminum source and preventing its precipitation, and the five-membered ring in the (R)-A-lipoic acid tromethamine salt molecule will open to form a linear molecular long chain, thereby improving the viscoelasticity of the solution; at the same time, the carboxyl group, hydroxyl group and amino group on the (R)-A-lipoic acid tromethamine salt may interact with the aluminum source through hydrogen bonds to form a complex three-dimensional network structure, effectively improving the viscoelasticity and stretchability of the precursor solution 1, so that the solution can resist fracture when subjected to external force; further, in order to improve the stability of the precursor solution, a stabilizer 1-butyl-3-methylimidazole tetrafluoroborate is added, and the cross-network structure is kept stable through intermolecular electrostatic interaction, and the (R)-A-lipoic acid tromethamine salt is coordinated to avoid the chain breakage phenomenon of the network molecular chain during rapid stretching; in addition, the addition of the aluminum source in the present invention will make the composite material have good electrical insulation, which is more suitable for the electronics industry.

[0015] 2. In the precursor solution 2, the introduction of lignin-based resin as a carbon source provides a way for bio-based resin to replace traditional resins. Mixing lignin-based resin with sodium metasilicate nonahydrate can improve the interfacial compatibility between them and form a uniform solution. First, the lignin-based resin can act as an adhesive, thereby enhancing the tensile strength and modulus of the fiber; second, the three-dimensional network structure of the lignin-based resin helps to enhance the mechanical strength, wear resistance and durability, and improve the overall performance of the composite material; third, the epoxidized lignin in the lignin-based resin contains epoxy groups, which can react with the silanol groups in the system to form a stable Si-OC cross-linked network, thereby improving the mechanical strength and thermal stability of the material, and helping to maintain the structural integrity of the fiber in the subsequent high-temperature treatment steps.

[0016] In some embodiments, the stabilizer in step S1 is 1-butyl-3-methylimidazolium tetrafluoroborate.

[0017] In some embodiments, the mass ratio of the aluminum source, (R)-A-lipoic acid tromethamine salt and the stabilizer in step S1 is 1:(0.5-1.5):(0.05-0.2).

[0018] Specifically, in step S1, the aluminum source is aluminum acetylacetonate and / or aluminum isopropoxide; the solvent is any one or more of ethanol, toluene and N,N-dimethylformamide; and the dosage ratio of the aluminum source to the solvent is 1 g: (2-8) ml.

[0019] In some embodiments, the mass ratio of the silicon-containing solution to the lignin-based resin in step S2 is 1:(4-6).

[0020] Specifically, the mass ratio of the deionized water to the silicon-containing solution in step S2 is (2-6):1.

[0021] In some embodiments, the method for preparing the lignin-based resin in step S2 comprises the following steps:

[0022] (1) adding lignin to a reactor, adjusting the pH value to 9-10, adding epichlorohydrin and tetrabutylammonium bromide, reacting at 55-70° C. for 2-3 hours, cooling to room temperature, adding tetrabutylammonium bromide and sodium hydroxide, reacting for 7-9 hours, and after the reaction, adding deionized water for precipitation, collecting the precipitate and drying it to obtain epoxidized lignin;

[0023] (2) dissolving the epoxidized lignin obtained in step (1) in polyethylene glycol, adding 2-toluene glycidyl ether and 2-methylpentanediamine, mixing and stirring, adding to a reaction kettle, and curing to obtain a lignin-based resin.

[0024] In some embodiments, the mass ratio of lignin to epichlorohydrin in step (1) is 1:(8-12).

[0025] In some embodiments, the mass ratio of the epoxidized lignin to 2-toluene glycidyl ether in step (2) is 1:(15-18).

[0026] In some embodiments, the propulsion speed of the double-needle electrospinning in step S3 is 0.2-0.6 mL / h.

[0027] In some embodiments, the specific steps of step S4 are as follows: drying the film-like composite material obtained in step S3, taking it out and cooling it to room temperature, putting it into a sintering furnace, introducing argon containing H2, heating it to 400-550°C at a rate of 150-200°C / h, and keeping it warm for 2-3h; heating it to 850-1000°C at a rate of 100-140°C / h, and keeping it warm for 1.5-2.5h; then introducing pure argon, heating it to 1200-1500°C at a rate of 50-80°C / h, keeping it warm for 0.5-2h, and cooling it to obtain a ceramic nanofiber and silicon carbide fiber composite material.

[0028] Another aspect of the present invention provides an application of a ceramic nanofiber and silicon carbide fiber composite material obtained by the preparation method, which is used in the field of electronic semiconductors.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] 1. The ceramic nanofiber and silicon carbide fiber composite material of the present invention has the characteristics of high temperature resistance and good mechanical properties, and is used in the field of electronic semiconductors and has good market value.

[0031] 2. The present invention effectively improves the viscoelasticity and stretchability of the precursor solution 1 by introducing (R)-A-lipoic acid tromethamine salt; further, 1-butyl-3-methylimidazolium tetrafluoroborate is added to stabilize the cross-network structure, and cooperates with (R)-A-lipoic acid tromethamine salt to avoid chain breakage of the network molecular chain during rapid stretching.

[0032] 3. In the present invention, the introduction of lignin-based resin in the preparation of precursor solution 2 not only helps to improve the processing and performance of the material and improve the overall performance of the composite material, but also the epoxidized lignin in the lignin-based resin contains epoxy groups that can react with the silanol groups in the system to form a stable Si-OC cross-linked network, thereby improving the mechanical strength and thermal stability of the material. DETAILED DESCRIPTION

[0033] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, rather than to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.

[0034] The composite materials were prepared according to the ratios of the raw materials and the preparation methods specified in the following examples and comparative examples.

[0035] In order to facilitate those skilled in the art to implement the present invention, some raw material manufacturers of the embodiments and comparative examples are described as follows:

[0036] Lignin: purchased from Jiaxiang County Dahai Chemical Co., Ltd.

[0037] Polyethylene glycol 200: purchased from Shandong Haochen New Materials Technology Co., Ltd.;

[0038] Other raw materials are not specially specified and can be purchased from the market.

[0039] Preparation Example 1

[0040] The preparation method of lignin-based resin A comprises the following steps:

[0041] (1) 10 g of lignin was added to a reactor, the pH value was adjusted to 9.5 with sodium hydroxide solution, 100 g of epichlorohydrin and 1 g of tetrabutylammonium bromide were added, the reaction was carried out at 60° C. for 3 h, the reaction was cooled to room temperature, 0.5 g of tetrabutylammonium bromide and 1 g of sodium hydroxide were added, the reaction was carried out for 7-9 h, and after the reaction was completed, 200 ml of deionized water was added for precipitation, the precipitate was collected, and it was dried at 85° C. for 6 h to obtain epoxidized lignin;

[0042] (2) 7.2 g of epoxidized lignin obtained in step (1) was dissolved in 25 g of polyethylene glycol 200, 120 g of 2-toluene glycidyl ether and 35 g of 2-methylpentanediamine were added, the mixture was mixed and stirred, and then added to a reaction kettle and cured to obtain a lignin-based resin.

[0043] Preparation Example 2

[0044] The preparation method of lignin-based resin B is the same as that of Preparation Example 1, except that 70 g of epichlorohydrin is added in step (1).

[0045] Preparation Example 3

[0046] The preparation method of lignin-based resin C is the same as that of Preparation Example 1, except that 140 g of epichlorohydrin is added in step (1).

[0047] Preparation Example 4

[0048] The preparation method of lignin-based resin D is the same as that of Preparation Example 1, except that 86.4 g of 2-toluene glycidyl ether is added in step (2).

[0049] Preparation Example 5

[0050] The preparation method of lignin-based resin E is the same as that of Preparation Example 1, except that 144 g of 2-toluene glycidyl ether is added in step (2).

[0051] Example 1

[0052] A method for preparing a composite material of ceramic nanofibers and silicon carbide fibers comprises the following steps:

[0053] S1. 20 g of aluminum acetylacetonate was dissolved in 100 ml of N, N-dimethylformamide, 20 g of (R)-A-lipoic acid tromethamine salt was added, and the mixture was stirred for 50 min, followed by addition of 2 g of 1-butyl-3-methylimidazolium tetrafluoroborate, and the mixture was stirred for 60 min to obtain a precursor solution 1;

[0054] S2. 10 g of sodium metasilicate nonahydrate was dissolved in 120 g of anhydrous ethanol to obtain a silicon-containing solution, 560 g of deionized water was added dropwise while stirring, and then 700 g of lignin-based resin A was added, stirred for 3 h, and 70 g of acetone was added to obtain a precursor solution 2;

[0055] S3. Place equal volumes of precursor solution 1 and precursor solution 2 in two syringes of a double-needle electrospinning machine, respectively, at a propulsion speed of 0.4 mL / h, an electric field voltage of 28 KV, and a needle distance of 15 cm from a receiving plate to perform double-needle electrospinning to obtain a membrane composite material;

[0056] S4. The film-like composite material obtained in step S3 is placed in an oven and dried at 80°C for 2h, taken out and cooled to room temperature, placed in a sintering furnace, introduced with hydrogen-containing argon (the volume ratio of hydrogen / argon is 1 / 8), heated to 500°C at a rate of 180°C / h, and kept warm for 2.5h; heated to 900°C at a rate of 120°C / h, and kept warm for 2h; then introduced with pure argon, heated to 1300°C at a rate of 65°C / h, and kept warm for 1h, and cooled to room temperature to obtain a ceramic nanofiber and silicon carbide fiber composite material.

[0057] Example 2

[0058] A method for preparing a composite material of ceramic nanofibers and silicon carbide fibers comprises the following steps:

[0059] S1. 20 g of aluminum acetylacetonate was dissolved in 80 ml of N,N-dimethylformamide, 10 g of (R)-A-lipoic acid tromethamine salt was added, and the mixture was stirred for 30 min, followed by addition of 1 g of 1-butyl-3-methylimidazolium tetrafluoroborate, and the mixture was stirred for 40 min to obtain a precursor solution 1;

[0060] S2. 10 g of sodium metasilicate nonahydrate was dissolved in 100 g of anhydrous ethanol to obtain a silicon-containing solution, 240 g of deionized water was added dropwise while stirring, and then 480 g of lignin-based resin A was added, stirred for 2 h, and 70 g of acetone was added to obtain a precursor solution 2;

[0061] S3. Place equal volumes of precursor solution 1 and precursor solution 2 in two syringes of a double-needle electrospinning machine, respectively, at a propulsion speed of 0.2 mL / h, an electric field voltage of 25 KV, and a needle distance of 15 cm from a receiving plate to perform double-needle electrospinning to obtain a membrane composite material;

[0062] S4. The film-like composite material obtained in step S3 is placed in an oven and dried at 80°C for 2h, taken out and cooled to room temperature, placed in a sintering furnace, introduced with hydrogen-containing argon (the volume ratio of hydrogen / argon is 1 / 8), heated to 400°C at a rate of 150°C / h, and kept warm for 2h; heated to 850°C at a rate of 100°C / h, and kept warm for 1.5h; then introduced with pure argon, heated to 1200°C at a rate of 50°C / h, and kept warm for 0.5h, and cooled to room temperature to obtain a ceramic nanofiber and silicon carbide fiber composite material.

[0063] Example 3

[0064] A method for preparing a composite material of ceramic nanofibers and silicon carbide fibers comprises the following steps:

[0065] S1. 20 g of aluminum acetylacetonate was dissolved in 140 ml of N, N-dimethylformamide, 30 g of (R)-A-thioctic acid tromethamine salt was added, and the mixture was stirred for 80 min, followed by addition of 4 g of 1-butyl-3-methylimidazolium tetrafluoroborate, and the mixture was stirred for 100 min to obtain a precursor solution 1;

[0066] S2. 10 g of sodium metasilicate nonahydrate was dissolved in 150 g of anhydrous ethanol to obtain a silicon-containing solution, 1000 g of deionized water was added dropwise while stirring, and then 1000 g of lignin-based resin A was added, stirred for 4 h, and 70 g of acetone was added to obtain a precursor solution 2;

[0067] S3. Place equal volumes of precursor solution 1 and precursor solution 2 in two syringes of a double-needle electrospinning machine, respectively, at a propulsion speed of 0.6 mL / h, an electric field voltage of 30 KV, and a needle distance of 15 cm from a receiving plate to perform double-needle electrospinning to obtain a membrane composite material;

[0068] S4. The film-like composite material obtained in step S3 is placed in an oven and dried at 80°C for 2h, taken out and cooled to room temperature, placed in a sintering furnace, introduced with hydrogen-containing argon (the volume ratio of hydrogen / argon is 1 / 8), and heated to 550°C at a rate of 200°C / h, and kept warm for 3h; heated to 1000°C at a rate of 140°C / h, and kept warm for 2.5h; then introduced with pure argon, heated to 1500°C at a rate of 80°C / h, and kept warm for 2h, and cooled to room temperature to obtain a ceramic nanofiber and silicon carbide fiber composite material.

[0069] Example 4

[0070] A method for preparing a ceramic nanofiber and silicon carbide fiber composite material is the same as that in Example 1, except that an equal amount of lignin-based resin B is used to replace lignin-based resin A.

[0071] Example 5

[0072] A method for preparing a ceramic nanofiber and silicon carbide fiber composite material is the same as that in Example 1, except that an equal amount of lignin-based resin C is used to replace lignin-based resin A.

[0073] Example 6

[0074] A method for preparing a ceramic nanofiber and silicon carbide fiber composite material is the same as that in Example 1, except that an equal amount of lignin-based resin D is used to replace lignin-based resin A.

[0075] Example 7

[0076] A method for preparing a ceramic nanofiber and silicon carbide fiber composite material is the same as that in Example 1, except that an equal amount of lignin-based resin E is used to replace lignin-based resin A.

[0077] Example 8

[0078] A method for preparing a ceramic nanofiber and silicon carbide fiber composite material is the same as that in Example 1, except that an equal amount of methylimidazole is used to replace 1-butyl-3-methylimidazole tetrafluoroborate.

[0079] Example 9

[0080] A method for preparing a ceramic nanofiber and silicon carbide fiber composite material is the same as that in Example 1, except that the amount of (R)-A-lipoic acid tromethamine salt added is 8.8 g.

[0081] Example 10

[0082] A method for preparing a ceramic nanofiber and silicon carbide fiber composite material is the same as that in Example 1, except that the amount of 1-butyl-3-methylimidazole tetrafluoroborate added is 6.1 g.

[0083] Embodiment 11

[0084] The preparation method of a ceramic nanofiber and silicon carbide fiber composite material is the same as that of Example 1, except that the amount of lignin-based resin A added is 350 g.

[0085] Example 12

[0086] A method for preparing a ceramic nanofiber and silicon carbide fiber composite material is the same as that in Example 1, except that step S4 is: placing the film-like composite material obtained in step S3 in an oven at 80°C for 2 hours, taking it out and cooling it to room temperature, placing it in a sintering furnace, introducing argon gas containing H2, heating it to 900°C at a rate of 180°C / h, and keeping it warm for 5 hours; then introducing pure argon gas, heating it to 1600°C at a rate of 120°C / h, keeping it warm for 1 hour, and cooling it to obtain a ceramic nanofiber and silicon carbide fiber composite material.

[0087] Comparative Example 1

[0088] A method for preparing a ceramic nanofiber and silicon carbide fiber composite material is the same as that in Example 1, except that step S1: dissolving 20 g of aluminum acetylacetonate in 80 ml of N,N-dimethylformamide, adding 1 g of 1-butyl-3-methylimidazole tetrafluoroborate, and stirring for 40 min to obtain a precursor solution 1.

[0089] Comparative Example 2

[0090] A method for preparing a ceramic nanofiber and silicon carbide fiber composite material is the same as Example 1, except that step S2: dissolving 10 g of sodium metasilicate nonahydrate in 120 g of anhydrous ethanol, adding 560 g of deionized water dropwise while stirring, then adding 700 g of sucrose, and stirring for 3 hours to obtain a precursor solution 2.

[0091] Effect evaluation:

[0092] The composite materials prepared in the above-mentioned Examples 1-12 and Comparative Examples 1-2 were tested and analyzed, and the specific results are shown in Table 1.

[0093] Performance Test:

[0094] (1) Elastic modulus: according to national standard ASTM D 3039;

[0095] (2) Thermal conductivity: The thermal conductivity of the material is measured at 1200°C using a thermal conductivity instrument.

[0096] Thermal conductivity describes the amount of heat that passes through a unit temperature difference per unit area per unit time. Materials with lower thermal conductivity usually have better thermal insulation properties and can more effectively prevent heat transfer in high temperature environments. Low thermal conductivity means that under the same temperature gradient, the composite material transfers less heat per unit time, which helps protect the composite material or the surrounding environment from high temperatures. The thermal conductivity can indirectly reflect the high temperature resistance of the composite material.

[0097] Table 1

[0098] Serial number Elastic modulus(GPa) Thermal conductivity (W / mK) Example 1 315 0.0238 Example 2 309 0.0285 Example 3 314 0.0245 Example 4 285 0.0387 Example 5 298 0.0354 Example 6 274 0.0406 Example 7 262 0.0299 Example 8 249 0.0482 Example 9 257 0.0295 Example 10 273 0.0398 Embodiment 11 243 0.0555 Example 12 237 0.0625 Comparative Example 1 230 0.0567 Comparative Example 2 221 0.0699

[0099] From the results in Table 1, it can be seen that the ceramic nanofiber and silicon carbide fiber composite materials prepared in Examples 1-3 have lower thermal conductivity, high temperature resistance and better mechanical properties, and have better market value.

[0100] Compared with Example 1, in the preparation of lignin-based resin, the mass ratio of lignin to epichlorohydrin is changed, so that the phenolic hydroxyl groups in the lignin are not fully converted into epoxides, which may lead to incomplete curing of the resin and affect the final mechanical properties and temperature resistance.

[0101] Compared with Example 1, when preparing the lignin-based resin, the mass ratio of lignin to epichlorohydrin is changed, which will lead to excessive epoxidation of lignin, which may lead to an increase in the viscosity of the resin, thereby affecting the fluidity and processing properties of the resin, and further affecting the final elastic modulus.

[0102] Compared with Example 1, Example 6 changes the mass ratio of epoxidized lignin and 2-toluene glycidyl ether, which will prevent the epoxy groups in the epoxidized lignin from fully reacting, resulting in incomplete curing of the resin, which will make the cross-linking density of the resin insufficient and affect the final mechanical properties and temperature resistance.

[0103] Compared with Example 1, Example 7 changes the mass ratio of epoxidized lignin and 2-toluene glycidyl ether, which will result in excessive epoxy groups in the resin, which may cause the resin to produce a higher cross-linking density during the curing process, thereby making the resin too hard and brittle, affecting its mechanical properties.

[0104] Compared with Example 1, Example 8 changes the type of stabilizer, and the stabilizing effect is weakened at high temperatures, which makes the material formed by the precursor solution 1 less resistant to fracture when subjected to external force, thereby affecting the temperature resistance.

[0105] Compared with Example 1, Examples 9-10 changed the molar ratios of the aluminum source, (R)-A-lipoic acid tromethamine salt, and the stabilizer. Example 9 weakened the hydrogen bond interaction between the carboxyl group, hydroxyl group, and amino group and the aluminum source, reduced the stretchability, and thus the ability to resist fracture when subjected to external force deteriorated; Example 10 deteriorated the intermolecular electrostatic interaction and the cross-network structure, and chain breakage was prone to occur during rapid stretching, thereby affecting the temperature resistance.

[0106] Compared with Example 1, Example 11 changes the mass ratio of the composite material to the lignin-based resin, and the cross-linking structure becomes worse, which affects the elastic modulus and temperature resistance of the composite material.

[0107] Compared with Example 1, Example 12 changes the sintering temperature and the heating rate, so that the formed composite material has poor structural stability, affecting the final mechanical properties and temperature resistance.

[0108] Compared with Example 1, in Comparative Example 1, (R)-A-lipoic acid tromethamine salt was not added when preparing the precursor solution 1, so the fracture resistance and viscoelasticity were deteriorated when subjected to external force, which further affected the temperature resistance.

[0109] Compared with Example 1, in Comparative Example 2, sucrose was added during the preparation of precursor solution 2, which weakened the cross-linking effect and affected the final mechanical properties and temperature resistance.

[0110] The above is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present application. Although the present application is disclosed as above in the preferred embodiment, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases. However, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution.

Claims

1. A method for preparing a composite material of ceramic nanofibers and silicon carbide fibers, characterized in that: The following steps are included: S1. dissolving an aluminum source in an organic solvent, adding (R)-A-lipoic acid tromethamine salt, stirring for 30-80 min, then adding a stabilizer, stirring for 40-100 min, and obtaining a precursor solution 1; S2. Dissolve sodium metasilicate nonahydrate in anhydrous ethanol to obtain a silicon-containing solution, add deionized water dropwise while stirring, then add lignin-based resin, stir for 2-4 hours, add acetone and mix to obtain a precursor solution 2; wherein the mass ratio of sodium metasilicate nonahydrate to anhydrous ethanol is 1:(10-15); S3. placing equal volumes of precursor solution 1 and precursor solution 2 in two syringes of a double-needle electrospinning machine, respectively, and performing double-needle electrospinning to obtain a film-like composite material; S4. calcining the membrane-like composite material obtained in step S3 to obtain a composite material of ceramic nanofibers and silicon carbide fibers.

2. The method for preparing the composite material of ceramic nanofiber and silicon carbide fiber according to claim 1, characterized in that: The stabilizer in step S1 is 1-butyl-3-methylimidazolium tetrafluoroborate.

3. The method for preparing the composite material of ceramic nanofiber and silicon carbide fiber according to claim 1, characterized in that: The mass ratio of the aluminum source, (R)-A-lipoic acid tromethamine salt and the stabilizer in step S1 is 1:(0.5-1.5):(0.05-0.2).

4. The method for preparing the composite material of ceramic nanofiber and silicon carbide fiber according to claim 1, characterized in that: The mass ratio of the silicon-containing solution to the lignin-based resin in step S2 is 1:(4-6).

5. The method for preparing the composite material of ceramic nanofiber and silicon carbide fiber according to claim 1, characterized in that: The method for preparing the lignin-based resin in step S2 comprises the following steps: (1) adding lignin to a reactor, adjusting the pH value to 9-10, adding epichlorohydrin and tetrabutylammonium bromide, reacting at 55-70° C. for 2-3 hours, cooling to room temperature, adding tetrabutylammonium bromide and sodium hydroxide, reacting for 7-9 hours, and after the reaction, adding deionized water for precipitation, collecting the precipitate and drying it to obtain epoxidized lignin; (2) dissolving the epoxidized lignin obtained in step (1) in polyethylene glycol, adding 2-toluene glycidyl ether and 2-methylpentanediamine, mixing and stirring, adding to a reaction kettle, and curing to obtain a lignin-based resin.

6. The method for preparing the composite material of ceramic nanofiber and silicon carbide fiber according to claim 5, characterized in that: The mass ratio of lignin to epichlorohydrin in step (1) is 1:(8-12).

7. The method for preparing the composite material of ceramic nanofiber and silicon carbide fiber according to claim 5, characterized in that: The mass ratio of the epoxidized lignin to 2-toluene glycidyl ether in step (2) is 1:(15-18).

8. The method for preparing a composite material of ceramic nanofibers and silicon carbide fibers according to claim 1, characterized in that: The propulsion speed of the double-needle electrospinning in step S3 is 0.2-0.6 mL / h.

9. The method for preparing a composite material of ceramic nanofibers and silicon carbide fibers according to claim 1, characterized in that: The specific steps of step S4 are as follows: drying the film-like composite material obtained in step S3, taking it out and cooling it to room temperature, putting it into a sintering furnace, introducing argon gas containing H2, heating it to 400-550°C at a rate of 150-200°C / h, and keeping it warm for 2-3h; heating it to 850-1000°C at a rate of 100-140°C / h, and keeping it warm for 1.5-2.5h; then introducing pure argon gas, heating it to 1200-1500°C at a rate of 50-80°C / h, keeping it warm for 0.5-2h, and cooling it to obtain a ceramic nanofiber and silicon carbide fiber composite material.

10. An application of a composite material of ceramic nanofibers and silicon carbide fibers obtained by the preparation method according to any one of claims 1 to 9, characterized in that: Used in the field of electronic semiconductors.