Soybean fiber-cashmere blended yarn and preparation method thereof
Through the preparation method of blended yarns of soybean fiber and cashmere fiber, the problem of short and short cashmere fiber is solved, reducing costs and improving the yarn's consumption performance, which is suitable for lightweight and wide consumer needs.
Patent Information
- Application Number
- CN202411254939.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-09
AI Technical Summary
Cashmere fibers are thin, short in length and not as strong as wool, which hinders the development of lightweight cashmere products. In addition, pure cashmere products are costly and difficult to be accepted by consumers.
Using the blended yarn preparation method of soybean fiber and cashmere fiber, the blended yarn with a similar touch to pure cashmere through pretreatment and multi-carding process, reduce the use and production cost of cashmere, and combine the gloss of soybean fiber. and warm performance to improve the yarn's consumption performance.
It achieves a touch and performance similar to pure cashmere, reduces the use and production costs of cashmere, improves the consumption performance and uniformity of the yarn, and is suitable for a wide range of consumer needs.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present application relates to cashmere textile technology, and in particular to a soybean fiber-cashmere blended yarn and a preparation method thereof. Background Art
[0002] Cashmere is a rare and precious animal fiber in the world, a high-grade raw material for the textile industry. It is known as "fiber diamond" and "soft gold" because of its fineness, softness, lightness and scarcity. Cashmere products are thin, soft, smooth, lusterless, full of velvet, and excellent in warmth retention, and are deeply loved by consumers.
[0003] With the continuous development of the wool textile industry and the increasing quality requirements of consumers for wool and cashmere products, wool fabrics are developing towards high count and lightness in line with the international development trend. However, the defects of cashmere fibers such as thinness, short length and inferior strength to wool have hindered the development of lightness and thinness of cashmere products. In addition, although cashmere products are developing towards the civilian market, pure cashmere products are still difficult to be accepted by more consumers due to their high cost.
[0004] The development of blended fabrics of cashmere and other fibers is of great significance in reducing the use of cashmere, protecting the environment, reducing costs, better reflecting the advantages of cashmere products and improving the wearing properties of cashmere fabrics. Summary of the invention
[0005] The present application provides a soybean fiber-cashmere blended yarn and a preparation method thereof, in order to solve the above-mentioned technical problems.
[0006] In a first aspect, the present application provides a method for preparing soybean fiber-cashmere blended yarn, comprising:
[0007] The soybean fiber and the cashmere fiber are pretreated respectively;
[0008] The pretreated cashmere fiber and soybean fiber are weighed according to the corresponding proportions, and then manually fed into a cotton mixer and then fed into a cotton curtain for mixing to obtain a mixed fiber material, wherein the weight of the cashmere fiber accounts for 10-25% of the total weight of the mixed fiber;
[0009] In the process of making tops, the mixed fiber material is subjected to the following processes: cotton opening and cleaning → combing → first needle combing → second needle combing → third needle combing → wool type combing → fourth needle combing → fifth needle combing to obtain tops;
[0010] In the spinning process, the wool tops are subjected to the process of front spinning first needle combing → front spinning second needle combing → front spinning third needle combing → wool type roving → cotton type spun yarn → winding → doubling → doubling → steaming → finished cone yarn to produce soybean fiber-cashmere blended yarn.
[0011] The preparation method of soybean fiber-cashmere blended yarn provided in this application has the following beneficial effects:
[0012] 1) Because soybean fiber has a smooth, light and soft feel, and its properties are similar to those of cashmere fiber, blending soybean fiber and cashmere fiber can obtain yarn with a touch similar to that of pure cashmere, and soybean fiber is cheap and easy to obtain. Blending the two can effectively reduce the use of cashmere, as well as reduce production and consumption costs. Blending cashmere fiber and soybean fiber with cashmere can better reflect the advantages of cashmere products and improve the wearing performance of cashmere fabrics. In addition, soybean fiber also has excellent gloss, excellent warmth retention and good skin-friendliness. Blending the two can combine their respective excellent properties and improve the wearing performance.
[0013] 2) The method of the present application prepares wool tops through a multi-pass needle combing process, which can remove as many defective fibers as possible from the mixed fibers, thereby improving the quality of the prepared wool tops and improving the uniformity of the wool tops, laying a solid foundation for the preparation of qualified blended yarns.
[0014] 3) The spinning process in the present application is highly operable and easy to implement.
[0015] 4) In the present application, soybean fiber and cashmere fiber are pretreated separately, which can effectively improve the textile performance of each fiber and increase the yield rate.
[0016] Optionally, the pretreatment of the soybean fiber comprises:
[0017] The soybean fiber is immersed in the antistatic liquid for 40 to 60 minutes, wherein the amount of the antistatic agent is 20 to 25 g / L, the bath ratio is 28 to 35:1, and the immersion temperature is 35 to 45°C;
[0018] Then, the soybean fiber impregnated with the antistatic liquid is dehydrated at a speed of 600 to 800 rpm for 5 to 10 minutes;
[0019] The dehydrated soybean fiber is pre-baked in an inert gas atmosphere at 80-90°C for 10-15 minutes, and then the baking temperature is increased to 150°C and baked for 1.5-2 minutes;
[0020] The baked soybean fiber is placed in a sealed warehouse in an environment with a relative humidity of 55-60% and a temperature of 25-30°C for 20-24 hours;
[0021] The soybean fiber stacked in the sealed warehouse is washed twice with clean water, and then the washed soybean fiber is dehydrated at a speed of 800-1000 rpm for 5-10 minutes to obtain the pretreated soybean fiber.
[0022] Optionally, the pretreatment of the cashmere fiber includes cashmere modification and cashmere modification post-treatment;
[0023] The cashmere modification comprises: adding cashmere fibers into an activation solution prepared by 3-5%wt of Triton, and controlling the bath ratio to be 1:3-5;
[0024] Adding a reducing solution prepared by ammonium persulfate-sodium sulfite to the activated solution, stirring, ultrasonicating for 15-30 seconds, then heating to 60-65° C., adding an aqueous solution of acrylonitrile monomer, adjusting the concentration of acrylonitrile monomer to 0.3-0.4 mol / L, the bath ratio to 130-150:1, keeping the temperature for reaction for 45-60 minutes, wherein the molar ratio of ammonium persulfate-sodium sulfite is 3:2, and the amount of ammonium persulfate-sodium sulfite added is 6-8%wt of the amount of acrylonitrile monomer added;
[0025] The cashmere fiber after the reaction is dehydrated at a speed of 800-1000 rpm for 5-10 minutes, immersed in 3 times the volume of clean water for ultrasonic 2-3 minutes, dehydrated at a speed of 800-1000 rpm for 5-10 minutes, and then washed with clean water for 3-4 times;
[0026] The washed cashmere fibers are drained of water and then dried at 80-100° C. to a constant weight to obtain modified cashmere fibers.
[0027] Optionally, the cashmere modification post-processing comprises:
[0028] The modified cashmere fiber is fed into a cashmere mixing machine, and the feeding speed is controlled at 1.7-2.4 kg / min, and 0.6-0.7% antistatic agent, 1.5-1.8% wool mixing oil and 25-30% water are added at the same time. After the cashmere is treated by the cashmere mixing machine, the cashmere is turned over once during the 24-hour stewing period, and the stewing temperature is 25±2°C and the relative humidity is 75-85%, so as to obtain pretreated cashmere fiber;
[0029] The model of the velvet kneading machine is L740 / 04.
[0030] Optionally, the cotton mixer is an A006B type cotton mixer;
[0031] The cotton opening and cleaning process is completed by using A036C cotton opener, A092A double cotton box cotton feeder and A076C lap forming machine in sequence;
[0032] Among them, the beater speed of the A036C cotton opener is 540rpm; the beater speed of the A076C lap forming machine is 640rpm.
[0033] Optionally, the combing process is performed using a CL / CASH worsted combing machine, and its operating parameters are as follows:
[0034] The feeding amount is 300g / min, the feeding cycle is 60-80s, the sliver output speed is 24-32m / min, the sliver output quality is 12±2g, and the spacing between the cylinder and the doffer is 0.12mm.
[0035] Optionally, the gilling process in the strip making process is completed by a VSN9+UV11 gilling machine, and the specific operating parameters are as follows:
[0036] The first needle comb, the number of feeding roots is 10, the total feeding amount is 105.50±2.50g / m, the drafting multiple is 5.15, the number of sliver roots is 1, and the sliver quality is 21.5±0.05g / m;
[0037] Two-pass needle comb, the number of feeding roots is 5, the total feeding amount is 115.00±2.50g / m, the drafting multiple is 5.40, the number of sliver roots is 1, the gauge is 30mm, and the sliver quality is 21.50±0.05g / m;
[0038] Three-pass needle combing, feeding number of 4 strands, total feeding amount of 86.50±2.50g / m, drafting multiple of 5.05, sliver number of 2 strands, gauge of 30mm, sliver quality of 7.80±0.05g / m;
[0039] Four-pass needle comb, feeding number of 6 strands, total feeding amount of 96.45±2.50g / m, drafting multiple of 5.00, sliver number of 1 strand, gauge of 30mm, sliver quality of 19.30±0.05g / m;
[0040] Five-way needle comb, the number of feed strands is 4, the total feed amount is 77.17±2.50g / m, the draft multiple is 5.20, the number of sliver strands is 1, the gauge is 30mm, and the sliver quality is 14.50±0.25g / m;
[0041] The wool combing is done by ALFA worsted combing machine, the specific parameters are as follows:
[0042] The number of strands fed is 10×2 strands, the total feed amount is 220±1g / m, the clamping times are 130±10 times / min, the front and rear stretching distance is 30mm, and the sliver quality is 20±0.5g.
[0043] Optionally, the needle combing process in the spinning process is completed by using a VSN9+UV11 needle combing machine, and the specific operating parameters are as follows:
[0044] The number of slivers fed into the front spinning comb is 6, the total amount of slivers fed is 42.92±1.50g / m, the drafting multiple is 5.30, the number of slivers produced is 2, the gauge is 30mm, and the sliver quality is 8.10±0.05g / m;
[0045] The front spinning two-pass needle comb has 16 feeding roots, a total feeding amount of 32.56±1.50g / m, a drafting multiple of 5.50, 4 sliver roots, a gauge of 30mm, and a sliver quality of 5.90±0.05g / m;
[0046] The front spinning has three needle combs, the number of feeding roots is 16, the total feeding amount is 23.70±1.50g / m, the drafting multiple is 6.80, the number of sliver roots is 4, the gauge is 30mm, and the sliver quality is 3.14±0.05g / m;
[0047] In the yarn steaming process, the temperature is 80-85°C and the time is 25-30 minutes.
[0048] Optionally, the cashmere fiber has a length of 38±2 mm and an average fineness of 15 μm;
[0049] The length of soybean fiber is 42±2 mm and the average fineness is 14.78 μm.
[0050] In a second aspect, the present application provides a soybean fiber-cashmere blended yarn, which is produced by the method described in any one of the first aspects above.
[0051] The soybean fiber-cashmere blended yarn provided in the present application can combine the advantages of soybean fiber and cashmere fiber, thereby improving the wearing performance of the prepared yarn. Moreover, since the yarn of the present application is made by mixing cashmere and soybean fiber, the amount of cashmere used can be reduced, thus having the characteristic of reducing costs. DETAILED DESCRIPTION
[0052] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application is clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work also fall within the scope of protection of the present application.
[0053] In a first aspect, the present application provides a method for preparing soybean fiber-cashmere blended yarn, comprising:
[0054] The soybean fiber and the cashmere fiber are pretreated respectively;
[0055] The pretreated cashmere fiber and soybean fiber are weighed according to the corresponding proportions, and then manually fed into a cotton mixer and then fed into a cotton curtain for mixing to obtain a mixed fiber material, wherein the weight of the cashmere fiber accounts for 10-25% of the total weight of the mixed fiber;
[0056] In the process of making tops, the mixed fiber material is subjected to the following processes: cotton opening and cleaning → combing → first needle combing → second needle combing → third needle combing → wool type combing → fourth needle combing → fifth needle combing to obtain tops;
[0057] In the spinning process, the wool tops are subjected to the process of front spinning first needle combing → front spinning second needle combing → front spinning third needle combing → wool type roving → cotton type spun yarn → winding → doubling → doubling → steaming → finished cone yarn to produce soybean fiber-cashmere blended yarn.
[0058] 1) Because soybean fiber has a smooth, light and soft feel, and its properties are similar to those of cashmere fiber, blending soybean fiber and cashmere fiber can obtain yarn with a touch similar to that of pure cashmere, and soybean fiber is cheap and easy to obtain. Blending the two can effectively reduce the use of cashmere, as well as reduce production and consumption costs. Blending cashmere fiber and soybean fiber with cashmere can better reflect the advantages of cashmere products and improve the wearing performance of cashmere fabrics. In addition, soybean fiber also has excellent gloss, excellent warmth retention and good skin-friendliness. Blending the two can combine their respective excellent properties and improve the wearing performance.
[0059] 2) The method of the present application prepares wool tops through a multi-pass needle combing process, which can remove as many defective fibers as possible from the mixed fibers, thereby improving the quality of the prepared wool tops and improving the uniformity of the wool tops, laying a solid foundation for the preparation of qualified blended yarns.
[0060] 3) The spinning process in the present application is highly operable and easy to implement.
[0061] 4) In the present application, soybean fiber and cashmere fiber are pretreated separately, which can effectively improve the textile performance of each fiber and increase the yield rate.
[0062] Optionally, the pretreatment of the soybean fiber comprises:
[0063] The soybean fiber is immersed in the antistatic liquid for 40 to 60 minutes, wherein the amount of the antistatic agent is 20 to 25 g / L, the bath ratio is 28 to 35:1, and the immersion temperature is 35 to 45°C;
[0064] Then, the soybean fiber impregnated with the antistatic liquid is dehydrated at a speed of 600 to 800 rpm for 5 to 10 minutes;
[0065] The dehydrated soybean fiber is pre-baked in an inert gas atmosphere at 80-90°C for 10-15 minutes, and then the baking temperature is increased to 150°C and baked for 1.5-2 minutes;
[0066] The baked soybean fiber is placed in a sealed warehouse in an environment with a relative humidity of 55-60% and a temperature of 25-30°C for 20-24 hours;
[0067] The soybean fiber stacked in the sealed warehouse is washed twice with clean water, and then the washed soybean fiber is dehydrated at a speed of 800-1000 rpm for 5-10 minutes to obtain the pretreated soybean fiber.
[0068] In the present application, the soybean fiber is prepared by copolymerization of soybean protein and polyvinyl alcohol monomer, so there are a large number of hydroxyl groups on the surface of the soybean fiber, so that the antistatic agent can better adhere to the fiber surface during the above-mentioned treatment process. The antistatic agent is selected from antistatic agent FX-AS301, antistatic agent SN, or antistatic agent AEA prepared by adding N,N-dimethylacetamide to triethanolamine adipate and sodium chloroacetate mixed in an equal molar ratio, reacting at 80°C for 8 hours, and evaporating to dryness.
[0069] In the present application, during the above soybean fiber pretreatment process, the antistatic agent can be solidified on the soybean fiber surface to enhance its adhesion performance. The antistatic agent AEA can combine with the hydroxyl groups on the soybean fiber surface to form covalent bonds during the above treatment process, further improving its adhesion.
[0070] Optionally, the pretreatment of the cashmere fiber includes cashmere modification and cashmere modification post-treatment;
[0071] The cashmere modification comprises: adding cashmere fibers into an activation solution prepared by 3-5%wt of Triton, and controlling the bath ratio to be 1:3-5;
[0072] Adding a reducing solution prepared by ammonium persulfate-sodium sulfite to the activated solution, stirring, ultrasonicating for 15-30 seconds, then heating to 60-65° C., adding an aqueous solution of acrylonitrile monomer, adjusting the concentration of acrylonitrile monomer to 0.3-0.4 mol / L, the bath ratio to 130-150:1, keeping the temperature for reaction for 45-60 minutes, wherein the molar ratio of ammonium persulfate-sodium sulfite is 3:2, and the amount of ammonium persulfate-sodium sulfite added is 6-8%wt of the amount of acrylonitrile monomer added;
[0073] The cashmere fiber after the reaction is dehydrated at a speed of 800-1000 rpm for 5-10 minutes, immersed in 3 times the volume of clean water for ultrasonic 2-3 minutes, dehydrated at a speed of 800-1000 rpm for 5-10 minutes, and then washed with clean water for 3-4 times;
[0074] The washed cashmere fibers are drained of water and then dried at 80-100° C. to a constant weight to obtain modified cashmere fibers.
[0075] In the present application, because the microstructure of the cashmere surface is a scaly structure, long-term friction will cause the cashmere fibers to become knotted and pilling, affecting the appearance of the fabric. The surface of the cashmere fibers is modified to form a protective film layer on the surface of the cashmere, filling the grooves of the scales on the surface of the cashmere to make the surface of the cashmere smoother, reducing the pilling phenomenon of the cashmere after friction caused by the scaly structure, and the strength of the modified cashmere fibers is also improved. In addition, due to the control of the amount of the modifier used in the present application, the influence of the modifier on the sensory perception of the cashmere itself can be reduced while the cashmere is modified.
[0076] In this application, a hydrolysis operation is also performed before drying the cashmere fiber:
[0077] The washed cashmere fiber is immersed in 2 to 3 times the volume of acid water (the pH of the acid water is adjusted to 2.5 to 3 with chloroacetic acid), and then sodium iodide is added thereto, the amount of sodium iodide added is 1 to 1.5% of the mass of the cashmere fiber, and heated to 55 to 60°C for hydrolysis for 25 to 30 minutes;
[0078] After the hydrolysis is completed, the cashmere fiber is dehydrated, washed with clean water until neutral, dehydrated, and placed in an environment of 25±2°C and a relative humidity of 65-75% for 3 hours before drying.
[0079] In the present application, the cashmere is hydrolyzed to hydrolyze the cyanide groups modified on the surface of the cashmere fiber into carboxyl groups. This hydrophilic group can effectively improve the antistatic properties of the cashmere fiber. In addition, since the cashmere fiber and the soybean fiber are first mixed and then made into strips and spun, the carboxyl groups on the surface of the cashmere can form hydrogen bonds with the hydroxyl groups on the surface of the soybean fiber (in the present application, the soybean fiber is made by copolymerizing soybean protein and polyvinyl alcohol monomer) during the yarn steaming process, which can better shape the blended yarn. The blended yarn that is shaped after the yarn steaming has better antistatic and anti-pilling properties after being woven into a fabric.
[0080] Optionally, the cashmere modification post-processing comprises:
[0081] The modified cashmere fiber is fed into a cashmere mixing machine, and the feeding speed is controlled at 1.7-2.4 kg / min, and 0.6-0.7% antistatic agent, 1.5-1.8% wool mixing oil and 25-30% water are added at the same time. After the cashmere is treated by the cashmere mixing machine, the cashmere is stewed for 24 hours, during which the warehouse is turned over once, and the stewing temperature is 25±2°C and the humidity is 75-85%, so as to obtain pretreated cashmere fiber;
[0082] The model of the velvet kneading machine is L740 / 04.
[0083] In the present application, the antistatic agent used in the post-treatment of cashmere modification is the antistatic agent FX-AS301, and the wool oil is FX-905. The post-treatment of cashmere modification allows the wool oil to better penetrate into the cashmere fiber, thereby improving the spinnability of the wool.
[0084] Optionally, the cotton mixer is an A006B type cotton mixer;
[0085] The cotton opening and cleaning process is completed by using A036C cotton opener, A092A double cotton box cotton feeder and A076C lap forming machine in sequence;
[0086] Among them, the beater speed of the A036C cotton opener is 540rpm; the beater speed of the A076C lap forming machine is 640rpm.
[0087] In this application, the cotton opening and cleaning process adopts the process principle of "loosening more and beating less" to reduce damage to the fibers.
[0088] Optionally, the combing process is performed using a CL / CASH worsted combing machine, and its operating parameters are as follows:
[0089] The feeding amount is 300g / min, the feeding cycle is 60-80s, the sliver output speed is 24-32m / min, the sliver output quality is 12±2g, and the spacing between the cylinder and the doffer is 0.12mm.
[0090] In this application, the combing process must reduce fiber damage, reduce the entanglement and rubbing between fibers, and achieve smooth fiber transfer. The dust removal knife adopts a high knife process to reduce the length of the first impurity removal zone. The dust removal knife height is 4mm and the dust removal knife angle is 85°.
[0091] Optionally, the gilling process in the strip making process is completed by a VSN9+UV11 gilling machine, and the specific operating parameters are as follows:
[0092] The first needle comb, the number of feeding roots is 10, the total feeding amount is 105.50±2.50g / m, the drafting multiple is 5.15, the number of sliver roots is 1, and the sliver quality is 21.5±0.05g / m;
[0093] Two-pass needle comb, the number of feeding roots is 5, the total feeding amount is 115.00±2.50g / m, the drafting multiple is 5.40, the number of sliver roots is 1, the gauge is 30mm, and the sliver quality is 21.50±0.05g / m;
[0094] Three-pass needle combing, feeding number of 4 strands, total feeding amount of 86.50±2.50g / m, drafting multiple of 5.05, sliver number of 2 strands, gauge of 30mm, sliver quality of 7.80±0.05g / m;
[0095] Four-pass needle comb, feeding number of 6 strands, total feeding amount of 96.45±2.50g / m, drafting multiple of 5.00, sliver number of 1 strand, gauge of 30mm, sliver quality of 19.30±0.05g / m;
[0096] Five-way needle comb, the number of feed strands is 4, the total feed amount is 77.17±2.50g / m, the draft multiple is 5.20, the number of sliver strands is 1, the gauge is 30mm, and the sliver quality is 14.50±0.25g / m;
[0097] The wool combing is done by ALFA worsted combing machine, the specific parameters are as follows:
[0098] The number of strands fed is 10×2 strands, the total feed amount is 220±1g / m, the clamping times are 130±10 times / min, the front and rear stretching distance is 30mm, and the sliver quality is 20±0.5g.
[0099] Optionally, the needle combing process in the spinning process is completed by using a VSN9+UV11 needle combing machine, and the specific operating parameters are as follows:
[0100] The number of slivers fed into the front spinning comb is 6, the total amount of slivers fed is 42.92±1.50g / m, the drafting multiple is 5.30, the number of slivers produced is 2, the gauge is 30mm, and the sliver quality is 8.10±0.05g / m;
[0101] The front spinning two-pass needle comb has 16 feeding roots, a total feeding amount of 32.56±1.50g / m, a drafting multiple of 5.50, 4 sliver roots, a gauge of 30mm, and a sliver quality of 5.90±0.05g / m;
[0102] The front spinning has three needle combs, the number of feeding roots is 16, the total feeding amount is 23.70±1.50g / m, the drafting multiple is 6.80, the number of sliver roots is 4, the gauge is 30mm, and the sliver quality is 3.14±0.25g / m;
[0103] In the yarn steaming process, the temperature is 80-85°C and the time is 25-30 minutes.
[0104] Optionally, the cashmere fiber has a length of 38±2 mm and an average fineness of 15 μm;
[0105] The length of soybean fiber is 42±2 mm and the average fineness is 14.78 μm.
[0106] In the present application, the yarn steaming process can shape the spun yarn and reduce the loosening of the yarn. The yarn steaming temperature is 80-85° C., which can reduce damage to the fiber.
[0107] In this application, in the wool roving process, the RF5a roving machine is used, the number of feeding roots is 1, the pulling multiple is 10 to 12 times, the sliver quality is 0.3 ± 0.1 g / m, and the speed is 100 to 120 rpm;
[0108] In the cotton spinning process, the JWF-1516 spinning frame is selected, with a traction multiple of 18-22, a twist of 650-800 T / m, a twist direction of Z, and a speed of 6400-7000 rpm;
[0109] The machine speed is 500-550rpm when doubling, 6000-6500rpm when twisting, the twist of yarn is 800-900T / m, twist direction is S; the doubling and twisting machine model is VTS-08
[0110] In the yarn steaming process, the temperature is 80-85°C and the time is 25-30 minutes.
[0111] Example 1
[0112] A soybean fiber-cashmere blended yarn is prepared by the following method:
[0113] S101, pre-treating soybean fiber (length 42±2 mm, average fineness 14.78 μm) and cashmere fiber (length 38±2 mm, average fineness 15 μm) respectively:
[0114] The soybean fiber was immersed in antistatic liquid for 40 minutes, wherein the amount of antistatic agent was 20 g / L, the bath ratio was 28:1, and the immersion temperature was 35°C;
[0115] Then the soybean fiber impregnated with the antistatic liquid was dehydrated at a speed of 600 rpm for 10 min;
[0116] The dehydrated soybean fiber was pre-baked in an inert atmosphere at 80°C for 15 minutes, and then the baking temperature was increased to 150°C and baked for 1.5 minutes;
[0117] The baked soybean fiber is placed in a sealed warehouse in an environment with a relative humidity of 55-60% and a temperature of 25-30°C for 20 hours;
[0118] The soybean fiber stacked in the sealed warehouse is washed twice with clean water, and then the washed soybean fiber is dehydrated at a speed of 800 rpm for 10 minutes to obtain the pretreated soybean fiber. The antistatic agent is the antistatic agent AEA synthesized in the above method.
[0119] Add cashmere fiber into an activation solution prepared with 3%wt of Triton, and control the bath ratio to be 1:5;
[0120] Add a reducing solution prepared by ammonium persulfate-sodium sulfite to the added activation solution, stir, and ultrasonicate for 15 seconds, then heat to 60° C., add an aqueous solution of acrylonitrile monomer, adjust the concentration of acrylonitrile monomer to 0.3 mol / L, the bath ratio to 130:1, and keep the temperature for 60 minutes, wherein the molar ratio of ammonium persulfate-sodium sulfite is 3:2, and the amount of ammonium persulfate-sodium sulfite added is 6%wt of the amount of acrylonitrile monomer added;
[0121] The cashmere fibers after the reaction were dehydrated at 800 rpm for 10 min, immersed in 3 times the volume of clean water for ultrasonic treatment for 2 to 3 min, dehydrated at 800 rpm for 10 min, and then washed with clean water for 3 to 4 times;
[0122] The washed cashmere fibers are drained of water and dried at 80° C. to a constant weight to obtain modified cashmere fibers;
[0123] The modified cashmere fiber is fed into a cashmere mixing machine with a feeding speed controlled at 1.7 kg / min, and 0.6% antistatic agent, 1.5% wool oil and 25% water are added at the same time. After the cashmere is treated by the cashmere mixing machine, it is emptied once during the 24-hour stewing period with a stewing temperature of 25±2°C and a relative humidity of 75-85% to obtain pretreated cashmere fiber.
[0124] S102, weighing the pretreated cashmere fiber and soybean fiber according to corresponding proportions, and manually feeding them into a cotton mixer and feeding them into a cotton curtain for mixing to obtain a mixed fiber material, wherein the weight of the cashmere fiber accounts for 10% of the total weight of the mixed fiber;
[0125] S103, a sliver making process, wherein the mixed fiber material is subjected to a process of opening and cleaning cotton → combing wool → first needle combing → second needle combing → third needle combing → wool type combing → fourth needle combing → fifth needle combing to obtain wool sliver;
[0126] S104, spinning process, the wool tops are subjected to the process of front spinning first needle combing → front spinning second needle combing → front spinning third needle combing → wool type roving → cotton type spun yarn → winding → doubling → doubling → steaming → finished bobbin yarn to obtain soybean fiber-cashmere blended yarn.
[0127] Example 2
[0128] A soybean fiber-cashmere blended yarn is prepared by the following method:
[0129] S201, pre-treating soybean fiber (length 42±2mm, average fineness 14.78μm) and cashmere fiber (length 38±2mm, average fineness 15μm) respectively:
[0130] The soybean fiber was immersed in antistatic liquid for 60 minutes, wherein the amount of antistatic agent was 25 g / L, the bath ratio was 35:1, and the immersion temperature was 45°C;
[0131] Then the soybean fiber impregnated with the antistatic liquid was dehydrated at a speed of 800 rpm for 5 minutes;
[0132] The dehydrated soybean fiber was pre-baked in a nitrogen atmosphere at 90°C for 10 min, and then the baking temperature was increased to 150°C and baked for 2 min;
[0133] The baked soybean fiber is placed in a sealed warehouse in an environment with a relative humidity of 55-60% and a temperature of 25-30°C for 24 hours;
[0134] The soybean fiber stacked in the sealed warehouse is washed twice with clean water, and then the washed soybean fiber is dehydrated at a speed of 1000 rpm for 5 minutes to obtain the pretreated soybean fiber, wherein the antistatic agent is the antistatic agent AEA synthesized in the above method.
[0135] Add cashmere fiber into an activation solution prepared with 5%wt of Triton, and control the bath ratio to be 1:3;
[0136] Add a reducing solution prepared by ammonium persulfate-sodium sulfite to the added activation solution, stir, and ultrasonicate for 30 seconds, then heat to 65° C., add an aqueous solution of acrylonitrile monomer, adjust the concentration of acrylonitrile monomer to 0.4 mol / L, the bath ratio to 150:1, and keep the temperature for 45 minutes, wherein the molar ratio of ammonium persulfate-sodium sulfite is 3:2, and the amount of ammonium persulfate-sodium sulfite added is 8%wt of the amount of acrylonitrile monomer added;
[0137] The cashmere fibers after the reaction were dehydrated at a speed of 1000 rpm for 5 minutes, immersed in 3 times the volume of clean water for ultrasonic treatment for 2 to 3 minutes, dehydrated at a speed of 1000 rpm for 5 minutes, and then washed with clean water for 3 to 4 times;
[0138] The washed cashmere fibers were drained of water and then dried at 100° C. to a constant weight to obtain modified cashmere fibers;
[0139] The modified cashmere fiber is fed into a cashmere mixing machine with a feeding speed controlled at 2.4 kg / min, and 0.7% antistatic agent, 1.8% wool oil and 30% water are added at the same time. After the cashmere is treated by the cashmere mixing machine, it is emptied once during the 24-hour stewing period with a stewing temperature of 25±2°C and a relative humidity of 75-85% to obtain pretreated cashmere fiber.
[0140] S202, weighing the pretreated cashmere fiber and soybean fiber according to corresponding proportions, and manually feeding them into a cotton mixer and feeding them into a cotton curtain for mixing to obtain a mixed fiber material, wherein the weight of the cashmere fiber accounts for 25% of the total weight of the mixed fiber;
[0141] S203, a sliver making process, wherein the mixed fiber material is subjected to the process of opening and cleaning cotton → combing wool → first needle combing → second needle combing → third needle combing → wool type combing → fourth needle combing → fifth needle combing to obtain wool sliver;
[0142] S204, spinning process, the wool tops are subjected to the process of front spinning first needle combing → front spinning second needle combing → front spinning third needle combing → wool type roving → cotton type spun yarn → winding → doubling → doubling → steaming → finished bobbin yarn to obtain soybean fiber-cashmere blended yarn.
[0143] Example 3
[0144] A soybean fiber-cashmere blended yarn is prepared by the following method:
[0145] S301, pre-treating soybean fiber (length 42±2mm, average fineness 14.78μm) and cashmere fiber (length 38±2mm, average fineness 15μm) respectively:
[0146] The soybean fiber was immersed in antistatic liquid for 50 minutes, wherein the amount of antistatic agent was 22 g / L, the bath ratio was 30:1, and the immersion temperature was 40°C;
[0147] Then the soybean fiber impregnated with the antistatic liquid was dehydrated at a speed of 700 rpm for 8 minutes;
[0148] The dehydrated soybean fiber was pre-baked in an inert atmosphere at 85°C for 12 minutes, and then the baking temperature was increased to 150°C for 1.5 to 2 minutes;
[0149] The baked soybean fiber is placed in a sealed warehouse in an environment with a relative humidity of 55-60% and a temperature of 25-30°C for 20-24 hours;
[0150] The soybean fiber stacked in the sealed warehouse is washed twice with clean water, and then the washed soybean fiber is dehydrated at a speed of 900 rpm for 8 minutes to obtain the pretreated soybean fiber, wherein the antistatic agent is the antistatic agent AEA synthesized in the above method.
[0151] Add cashmere fiber into an activation solution prepared with 4%wt Triton, and control the bath ratio to be 1:4;
[0152] Add a reducing solution prepared by ammonium persulfate-sodium sulfite to the added activation solution, stir, and ultrasonicate for 25 seconds, then heat to 62.5° C., add an aqueous solution of acrylonitrile monomer, adjust the concentration of acrylonitrile monomer to 0.35 mol / L, the bath ratio to 140:1, and keep the temperature for 45 to 60 minutes, wherein the molar ratio of ammonium persulfate-sodium sulfite is 3:2, and the amount of ammonium persulfate-sodium sulfite added is 7%wt of the amount of acrylonitrile monomer added;
[0153] The cashmere fibers after the reaction were dehydrated at 900 rpm for 8 minutes, immersed in 3 times the volume of clean water for ultrasonic treatment for 2 to 3 minutes, dehydrated at 900 rpm for 8 minutes, and then washed with clean water for 3 to 4 times;
[0154] The washed cashmere fibers are drained of water and dried at 90° C. to a constant weight to obtain modified cashmere fibers;
[0155] The modified cashmere fiber is fed into a cashmere mixing machine with a feeding speed controlled at 2.0 kg / min, and 0.65% antistatic agent, 1.7% wool oil and 28% water are added at the same time. After the cashmere is treated by the cashmere mixing machine, it is emptied once during the 24-hour stewing period with a stewing temperature of 25±2°C and a relative humidity of 75-85% to obtain pretreated cashmere fiber.
[0156] S302, weighing the pretreated cashmere fiber and soybean fiber according to corresponding proportions, and manually feeding them into a cotton mixer and feeding them into a cotton curtain for mixing to obtain a mixed fiber material, wherein the weight of the cashmere fiber accounts for 20% of the total weight of the mixed fiber;
[0157] S303, a sliver making process, wherein the mixed fiber material is subjected to a process of opening and cleaning cotton → combing wool → first needle combing → second needle combing → third needle combing → wool type combing → fourth needle combing → fifth needle combing to obtain wool sliver;
[0158] S304, spinning process, the wool tops are subjected to the process of front spinning first needle combing → front spinning second needle combing → front spinning third needle combing → wool type roving → cotton type spun yarn → winding → doubling → doubling → steaming → finished bobbin yarn to obtain soybean fiber-cashmere blended yarn.
[0159] Example 4
[0160] A soybean fiber-cashmere blended yarn is prepared by the following method:
[0161] S401, the remaining operations are the same as S301, except that a hydrolysis operation is performed before drying the cashmere fibers:
[0162] The washed cashmere fiber is immersed in 2 volumes of acid water (the pH of the acid water is adjusted to 2.5-3 with chloroacetic acid), and then sodium iodide is added thereto, the amount of sodium iodide added is 1.2% of the mass of the cashmere fiber, and heated to 55°C for hydrolysis for 30 minutes;
[0163] After the hydrolysis is completed, the cashmere fiber is dehydrated, washed with clean water until neutral, dehydrated, and placed in an environment of 25±2°C and a relative humidity of 65-75% for 3 hours before drying.
[0164] S402, same as S302;
[0165] S403, same as S303;
[0166] S404, same as S303.
[0167] Comparative Example 1
[0168] A soybean fiber-cashmere blended yarn is prepared by the following method:
[0169] D101, the remaining operations are the same as S301, except that the cashmere fiber does not undergo cashmere modification operations, that is, the cashmere fiber is only post-processed.
[0170] D102, same as S302;
[0171] D103, same as S303;
[0172] D104, same as S303.
[0173] The sliver making process and the spinning process in the above-mentioned Examples 1 to 4 and Comparative Example 1 were carried out as follows:
[0174] The model of the velvet machine is L740 / 04;
[0175] The cotton blending machine is an A006B type cotton blending machine;
[0176] The cotton opening and cleaning process is completed by using A036C cotton opener, A092A double cotton box cotton feeder and A076C lap forming machine in sequence;
[0177] Among them, the beater speed of the A036C cotton opener is 540rpm; the beater speed of the A076C lap forming machine is 640rpm.
[0178] The carding process is completed by a CL / CASH worsted carding machine, and its operating parameters are as follows:
[0179] The feeding amount is 300-400g / min, the feeding cycle is 60s-80s, the sliver delivery speed is 24-32m / min, the sliver delivery quality is 12±2g, and the spacing between the cylinder and the doffer is 0.12mm.
[0180] The gilling process in the strip making process is completed by a VSN9+UV11 gilling machine. The specific operating parameters are as follows:
[0181] The first needle comb, the number of feeding roots is 10, the total feeding amount is 105.50±2.50g / m, the drafting multiple is 5.15, the number of sliver roots is 1, and the sliver quality is 21.5±0.05g / m;
[0182] Two-pass needle comb, the number of feeding roots is 5, the total feeding amount is 115.00±2.50g / m, the drafting multiple is 5.40, the number of sliver roots is 1, the gauge is 30mm, and the sliver quality is 21.50±0.05g / m;
[0183] Three-pass needle combing, feeding number of 4 strands, total feeding amount of 86.50±2.50g / m, drafting multiple of 5.05, sliver number of 2 strands, gauge of 30mm, sliver quality of 7.80±0.05g / m;
[0184] Four-pass needle comb, feeding number of 6 strands, total feeding amount of 96.45±2.50g / m, drafting multiple of 5.00, sliver number of 1 strand, gauge of 30mm, sliver quality of 19.30±0.05g / m;
[0185] Five-way needle comb, the number of feed strands is 4, the total feed amount is 77.17±2.50g / m, the draft multiple is 5.20, the number of sliver strands is 1, the gauge is 30mm, and the sliver quality is 14.50±0.25g / m;
[0186] The wool combing is done by ALFA worsted combing machine, the specific parameters are as follows:
[0187] The number of strands fed is 10×2 strands, the total feed amount is 220±1g / m, the clamping times are 130±10 times / min, the front and rear stretching distance is 30mm, and the sliver quality is 20±0.5g.
[0188] The needle combing process in the spinning process is completed by using a VSN9+UV11 needle combing machine, and the specific operating parameters are as follows:
[0189] The number of slivers fed into the front spinning comb is 6, the total amount of slivers fed is 42.92±1.50g / m, the drafting multiple is 5.30, the number of slivers produced is 2, the gauge is 30mm, and the sliver quality is 8.10±0.05g / m;
[0190] The front spinning two-pass needle comb has 16 feeding roots, a total feeding amount of 32.56±1.50g / m, a drafting multiple of 5.50, 4 sliver roots, a gauge of 30mm, and a sliver quality of 5.90±0.05g / m;
[0191] The front spinning has three needle combs, the number of feeding roots is 16, the total feeding amount is 23.70±1.50g / m, the drafting multiple is 6.80, the number of sliver roots is 4, the gauge is 30mm, and the sliver quality is 3.14±0.25g / m;
[0192] In the wool roving process, the RF5a roving machine is used, the number of feeding roots is 1, the pulling multiple is 10-12 times, the sliver quality is 0.3±0.1g / m, and the speed is 100-120rpm;
[0193] In the cotton spinning process, the JWF-1516 spinning frame is selected, with a traction multiple of 18-22, a twist of 800T / m, a twist direction of Z, and a speed of 6400rpm;
[0194] Winding process: SAVIO automatic winder is used, the speed is 1100m / min, the winding tension is 4CN / tex; the yarn clearer is set to N: 250; S: 150%×1.6; L: 32%×18; T: -32%×15;
[0195] The machine speed is 550rpm when doubling and 6500rpm when twisting. The twist of the yarn is 860T / m and the twist direction is S. The doubling and twisting machine model is VTS-08.
[0196] In the yarn steaming process, the temperature is 80°C and the time is 30 minutes.
[0197] Experimental example
[0198] The yarns prepared according to the above method were tested according to the following method, and the results are shown in Table 1:
[0199] Breaking strength and breaking elongation: tested according to GB / T 3916-2013 standard;
[0200] Antistatic performance: GB / T12703.2-2009 standard test;
[0201] Anti-pilling performance: in accordance with GB / T4802.3-2008.
[0202]
[0203] The above results show that the soybean fiber-cashmere blended yarn of the present application has excellent performance in breaking strength, antistatic performance and anti-pilling performance.
[0204] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, ordinary technicians in the field should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solution to deviate from the scope of the technical solutions of the embodiments of the present application.
Claims
1. A method for preparing soybean fiber-cashmere blended yarn, It is characterized in that include: The soybean fiber and the cashmere fiber are pretreated respectively; The pretreated cashmere fiber and soybean fiber are weighed according to the corresponding proportions, and then manually fed into a cotton mixer and then fed into a cotton curtain for mixing to obtain a mixed fiber material, wherein the weight of the cashmere fiber accounts for 10-25% of the total weight of the mixed fiber; In the process of making tops, the mixed fiber material is subjected to the following processes: cotton opening and cleaning → combing → first needle combing → second needle combing → third needle combing → wool type combing → fourth needle combing → fifth needle combing to obtain tops; In the spinning process, the wool tops are subjected to the process of front spinning first needle combing → front spinning second needle combing → front spinning third needle combing → wool type roving → cotton type spun yarn → winding → doubling → doubling → steaming → finished cone yarn to produce soybean fiber-cashmere blended yarn.
2. The method for preparing soybean fiber-cashmere blended yarn according to claim 1, It is characterized in that The pretreatment of the soybean fiber comprises: The soybean fiber is immersed in the antistatic liquid for 40 to 60 minutes, wherein the amount of the antistatic agent is 20 to 25 g / L, the bath ratio is 28 to 35:1, and the immersion temperature is 35 to 45°C; Then, the soybean fiber impregnated with the antistatic liquid is dehydrated at a speed of 600 to 800 rpm for 5 to 10 minutes; The dehydrated soybean fiber is pre-baked in an inert gas atmosphere at 80-90°C for 10-15 minutes, and then the baking temperature is increased to 150°C and baked for 1.5-2 minutes; The baked soybean fiber is placed in a sealed warehouse in an environment with a relative humidity of 55-60% and a temperature of 25-30°C for 20-24 hours; The soybean fiber stacked in the sealed warehouse is washed twice with clean water, and then the washed soybean fiber is dehydrated at a speed of 800-1000 rpm for 5-10 minutes to obtain the pretreated soybean fiber.
3. The method for preparing soybean fiber-cashmere blended yarn according to claim 1, It is characterized in that The pretreatment of the cashmere fiber includes cashmere modification and cashmere modification post-treatment; Cashmere finishing includes: Add cashmere fiber into an activation solution prepared by 3-5%wt of Triton, and control the bath ratio to be 1:3-5; Adding a reducing solution prepared by ammonium persulfate-sodium sulfite to the activated solution, stirring, ultrasonicating for 15-30 seconds, then heating to 60-65° C., adding an aqueous solution of acrylonitrile monomer, adjusting the concentration of acrylonitrile monomer to 0.3-0.4 mol / L, the bath ratio to 130-150:1, keeping the temperature for reaction for 45-60 minutes, wherein the molar ratio of ammonium persulfate-sodium sulfite is 3:2, and the amount of ammonium persulfate-sodium sulfite added is 6-8%wt of the amount of acrylonitrile monomer added; The cashmere fiber after the reaction is dehydrated at a speed of 800-1000 rpm for 5-10 minutes, immersed in 3 times the volume of clean water for ultrasonic 2-3 minutes, dehydrated at a speed of 800-1000 rpm for 5-10 minutes, and then washed with clean water for 3-4 times; The washed cashmere fibers are drained of water and then dried at 80-100° C. to a constant weight to obtain modified cashmere fibers.
4. The method for preparing soybean fiber-cashmere blended yarn according to claim 3, It is characterized in that The cashmere modification post-treatment comprises: The modified cashmere fiber is fed into a cashmere mixing machine with a feeding speed controlled at 1.7-2.4 kg / min, and 0.6-0.7% antistatic agent, 1.5-1.8% wool oil and 25-30% water are added at the same time. After the cashmere is treated by the cashmere mixing machine, it is stewed for 24 hours, during which time the warehouse is turned over once. The stewing temperature is 25±2°C and the relative humidity is 75-85% to obtain pretreated cashmere fiber.
5. The method for preparing soybean fiber-cashmere blended yarn according to claim 1, It is characterized in that The beater speed of the cotton opener is 540rpm; the beater speed of the lap forming machine is 640rpm.
6. The method for preparing soybean fiber-cashmere blended yarn according to claim 1, It is characterized in that The operating parameters of the combing process are as follows: The feeding amount is 300g / min, the feeding cycle is 60-80s, the sliver delivery speed is 24-32m / min, the sliver delivery mass is 12±2g, and the spacing between the cylinder and the doffer is 0.12mm.
7. The method for preparing soybean fiber-cashmere blended yarn according to claim 1, It is characterized in that The specific operating parameters in the strip making process are as follows: The first needle comb, the number of feeding roots is 10, the total feeding amount is 105.50±2.50g / m, the drafting multiple is 5.15, the number of sliver roots is 1, and the sliver quality is 21.5±0.05g / m; Two-pass needle comb, the number of feeding roots is 5, the total feeding amount is 115.00±2.50g / m, the drafting multiple is 5.40, the number of sliver roots is 1, the gauge is 30mm, and the sliver quality is 21.50±0.05g / m; Three-pass needle combing, feeding number of 4 strands, total feeding amount of 86.50±2.50g / m, drafting multiple of 5.05, sliver number of 2 strands, gauge of 30mm, sliver quality of 7.80±0.05g / m; Four-pass needle comb, feeding number of 6 strands, total feeding amount of 96.45±2.50g / m, drafting multiple of 5.00, sliver number of 1 strand, gauge of 30mm, sliver quality of 19.30±0.05g / m; Five-way needle comb, the number of feed strands is 4, the total feed amount is 77.17±2.50g / m, the draft multiple is 5.20, the number of sliver strands is 1, the gauge is 30mm, and the sliver quality is 14.50±0.25g / m; The specific parameters of the wool combing process are as follows: The number of strands fed is 10×2 strands, the total feed amount is 220±1g / m, the clamping times are 130±10 times / min, the front and rear stretching distance is 30mm, and the sliver quality is 20±0.5g.
8. The method for preparing soybean fiber-cashmere blended yarn according to claim 1, It is characterized in that The specific operating parameters in the spinning process are as follows: The number of slivers fed into the front spinning comb is 6, the total amount of slivers fed is 42.92±1.50g / m, the drafting multiple is 5.30, the number of slivers produced is 2, the gauge is 30mm, and the sliver quality is 8.10±0.05g / m; The front spinning two-pass needle comb has 16 feeding roots, a total feeding amount of 32.56±1.50g / m, a drafting multiple of 5.50, 4 sliver roots, a gauge of 30mm, and a sliver quality of 5.90±0.05g / m; The front spinning has three needle combs, the number of feeding roots is 16, the total feeding amount is 23.70±1.50g / m, the drafting multiple is 6.80, the number of sliver roots is 4, the gauge is 30mm, and the sliver quality is 3.14±0.25g / m; In the yarn steaming process, the temperature is 80-85°C and the time is 25-30 minutes.
9. The method for preparing soybean fiber-cashmere blended yarn according to claim 1, It is characterized in that The cashmere fiber has a length of 38±2 mm and an average fineness of 15 μm; The length of soybean fiber is 42±2 mm and the average fineness is 14.78 μm.
10. A soybean fiber-cashmere blended yarn, It is characterized in that The method is prepared by the preparation method described in any one of claims 1 to 9.
Citation Information
Patent Citations
Nzymatic synthesis grafting functional finishing method for wool
CN101435156A
Method for grafting and modifying cashmere
CN105350319A
High-color-fastness semi-worsted double-surface flannel fabric and processing technology thereof
CN109537138A
Soybean fiber / goat cashmere fabric
CN1410609A