Wear-resistant antistatic sofa fabric based on biocrystal powder and preparation method of wear-resistant antistatic sofa fabric
The problem of insufficient antistatic and wear resistance of existing sofa fabrics is solved by blending graphene oxide and modified biocrystal powder with polyester fibers in sofa fabrics and treated with blended fibers and hyperbranched polyethyleneimine. , achieves high-performance anti-static and wear-resistant effects, and has relaxing functions.
Patent Information
- Application Number
- CN202411103342.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-12
AI Technical Summary
Existing sofa fabrics have single performance in terms of antistatic and wear resistance, making it difficult to meet the demand for high-performance fabrics after improving living standards.
Graphene oxide and biocrystal powder are blended with polyester fibers. The biocrystal powder is modified to avoid its binding with graphene oxide, forming a conductive network to improve antistatic properties, and blended fibers and hyperbranched polyethyleneimine Reinforce the wear resistance of fibers.
It has achieved the improvement of anti-static and wear resistance of sofa fabrics, and has the effect of soothing mental stress and relaxing.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fabrics, and in particular to a wear-resistant and antistatic sofa fabric based on biological crystal powder and a preparation method thereof. Background Art
[0002] Sofa fabric is one of the important factors that affect the overall quality and comfort of the sofa. According to different needs and usage environments, the choice of sofa fabric can be divided into many types, including cloth, leather, linen, etc. The selection and application of sofa fabric is a comprehensive process, involving many aspects such as material type, production process, frame structure and filling material. Through reasonable design and strict production management, high-quality sofa products that are both beautiful and comfortable can be manufactured. Whether it is cloth, leather or linen fabric, it plays an indispensable role in modern furniture design.
[0003] Chinese patent publication number CN111593582 discloses a wear-resistant textile fabric for sofas and its preparation method. First, flax fiber is micronized and used for polypropylene to obtain coarser polypropylene fiber; further, the composite polypropylene and polyamide fiber are woven on a double-sided circular machine according to a double rib structure to obtain a base cloth, which is thick and has a good hemp feeling: in particular, hard coconut shell powder, walnut shell powder, acetate starch, itaconic acid, vinyl silane coupling agent, and sodium silicate are ground and composited for finishing the fabric, so that the wear resistance of the fabric is improved.
[0004] Chinese patent publication number CN106978664 discloses a sofa fabric with good wear resistance, which is prepared by coating anti-wear solution on both sides of the sofa blank, and the blank is prepared by weaving wear-resistant modified polyester fiber, ramie fiber, and polyurethane fiber, and the wear-resistant modified polyester fiber is prepared by polyethylene terephthalate masterbatch, polyurethane masterbatch, trioxymethylsilane, vinyl silane coupling agent, viscose fiber, nano silicon dioxide, nano magnesium oxide, and silicon nitride fiber. The present invention selects ramie fiber, polyurethane fiber and wear-resistant modified polyester fiber as raw materials to improve the wear resistance and wear resistance durability of the sofa fabric. At the same time, the wear-resistant layer formed by spraying the anti-wear solution on both sides of the sofa blank strengthens the wear resistance of the raw material fiber, so that the sofa fabric of the present invention has good wear resistance and durable wear resistance.
[0005] As people's living standards improve, people have higher and higher requirements on the performance of sofa fabrics. The sofa fabrics with single performance or function mentioned above are difficult to meet people's life needs. Summary of the invention
[0006] In order to overcome the above problems of the prior art, the present invention provides a wear-resistant and antistatic sofa fabric based on biological crystal powder and a preparation method thereof. The sofa fabric prepared by the present invention has both antistatic and wear-resistant properties, and can relieve the mental stress of the human body and achieve a relaxing effect.
[0007] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions: A method for preparing wear-resistant and antistatic sofa fabric based on biological crystal powder comprises the following steps: S1, preparation of modified polyester fiber: 1) Polyethylene terephthalate, polyurethane, biocrystal powder and graphene oxide are uniformly mixed to obtain a mixture; 2) The mixed material is added into a screw extruder to melt to obtain a spinning solution, and the spinning solution is sent to a spinneret in a spinning box to spin into primary fibers, which are then drawn and cooled to obtain the fibers; S2, blending spandex fiber, modified polyester fiber, polyester fiber and nylon fiber, and then weaving to obtain a grey cloth; S3, placing the embryo in a dyeing vat for dyeing, taking it out and drying it.
[0008] Graphene oxide has a high electrical conductivity and can reduce the accumulation of static electricity through its conductive properties. When graphene oxide is compounded with a material, a conductive network can be formed, thereby improving the antistatic properties of the material. Biocrystalline powder can emit infrared rays and produce a unique and stable frequency. Since this special frequency is at the same vibration frequency as humans, it has the functions of reducing muscle tension, slowing down the heartbeat, relaxing breathing, increasing the body's oxygen content, and releasing stress to improve sleep. In the technical solution of the present invention, graphene oxide and biocrystalline powder are mixed with resin chips during the preparation of polyester fibers, thereby doping graphene oxide and biocrystalline powder inside the polyester fibers to obtain functional modified polyester fibers.
[0009] In addition, in the technical solution of the present invention, spandex fiber, modified polyester fiber, polyester fiber and nylon fiber are blended to produce a fabric with excellent wear resistance and a certain anti-wrinkle effect.
[0010] Preferably, in step S1, the biocrystal powder is mixed with the following substances: Tourmaline powder, bloodstone powder, fluorite powder, orange crystal calcite powder, gypsum powder, aragonite powder, amethyst powder, red jasper powder, serpentine powder.
[0011] Preferably, the biocrystal powder is modified, comprising the following steps: S11, adding the biological crystal powder to a mixed solution of ethanol and water, and ultrasonically vibrating the solution to evenly disperse the biological crystal powder in the solution to obtain a suspension; S12, adding a silane coupling agent to the above suspension, heating, stirring for reaction, centrifuging, washing, and drying to obtain a preliminary modified biocrystal powder; S13, adding polyethyleneimine into deionized water and stirring to dissolve to obtain polyethyleneimine solution, adding the preliminary modified biocrystal powder into the polyethyleneimine solution, heating to react, and obtaining the product.
[0012] In the technical solution of the present invention, as described above, graphene oxide and biocrystal powder are blended with resin slices, so that graphene oxide and biocrystal powder are doped inside the polyester fiber to obtain functional modified polyester fiber. However, the problem encountered is that biocrystal powder is easily combined with graphene oxide and coated on the surface of graphene oxide, which affects the improvement of the antistatic performance of sofa fabric by graphene oxide. This may be because both biocrystal powder and graphene oxide are inorganic materials, and both have a stronger interface bonding effect relative to the organic phase, and both have hydroxyl groups on their surfaces, and there is a hydrogen bond attraction between the hydroxyl groups. In order to solve the above problems, the present invention modifies the biocrystal powder, first grafts a silane coupling agent to the surface of the biocrystal powder, and then utilizes the amino group on polyethyleneimine to react with the epoxy group of the silane coupling agent, so that polyethyleneimine is grafted to the surface of the biocrystal powder, so that the surface of the biocrystal powder particles is organic, thereby avoiding the biocrystal powder and graphene oxide from being combined and coated on its surface, and improving the antistatic improvement effect of graphene oxide on the sofa fabric. On the other hand, since hyperbranched polyethyleneimine has more branched structures, the branched structures are dispersed in the polyester, playing a role in strengthening the skeleton and further improving the wear resistance of the sofa fabric.
[0013] Preferably, the mass ratio of the biocrystal powder to the silane coupling agent is 1:0.1-0.5.
[0014] Preferably, the mass ratio of the preliminary modified biological crystal powder to polyethyleneimine is 1:0.6-1.2.
[0015] Preferably, in step S1, the melting temperature of the raw material is 180-190°C.
[0016] Preferably, in step S3, the drying temperature is controlled at 70-80°C.
[0017] A wear-resistant and antistatic sofa fabric based on biological crystal powder is prepared by the method described in any one of claims 1 to 7 above.
[0018] The present invention has the following beneficial effects: 1) Graphene oxide has high electrical conductivity and can reduce the accumulation of static electricity through its conductive properties. When graphene oxide is compounded with materials, it can form a conductive network, thereby improving the antistatic properties of the material; 2) Bio-crystal powder can emit infrared rays and produce a unique and stable frequency. Since this special frequency is at the same vibration frequency as humans, it has the functions of reducing muscle tension, slowing down heartbeat, relaxing breathing, increasing body oxygen content, releasing stress and improving sleep; 3) Modify the biocrystal powder to make the surface of the biocrystal powder particles organic, so as to avoid the biocrystal powder combining with graphene oxide and coating on its surface, and improve the antistatic improvement effect of graphene oxide on sofa fabrics. On the other hand, since hyperbranched polyethyleneimine has more branched structures, the branched structures are dispersed in polyester, which plays a role in strengthening the skeleton and can further improve the wear resistance of sofa fabrics. DETAILED DESCRIPTION
[0019] The present invention is further described in detail below in conjunction with specific embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.
[0020] Unless otherwise specified, the raw materials used in the examples of the present invention are all commercially available or available to those skilled in the art; unless otherwise specified, the methods used in the examples of the present invention are all methods known to those skilled in the art.
[0021] Example 1
[0022] A method for preparing wear-resistant and antistatic sofa fabric based on biological crystal powder comprises the following steps: S1, preparation of modified polyester fiber: 1) Polyethylene terephthalate, polyurethane, biocrystal powder and graphene oxide are uniformly mixed in a mass ratio of 20:12:3:0.5 to obtain a mixture; 2) The mixed material is added into a screw extruder for melting at a melting temperature of 187°C to obtain a spinning solution, which is then fed into a spinneret in a spinning box to spin into primary fibers, which are then stretched and cooled to obtain the fibers; S2, blending spandex fiber, modified polyester fiber, polyester fiber, and nylon fiber in a mass ratio of 2:2:1:1, and then weaving to obtain a grey cloth; S3, placing the embryo in a dyeing vat for dyeing, taking it out and drying it at a drying temperature of 80°C.
[0023] The above-mentioned biological crystal powder is mixed by the following substances of equal mass: Tourmaline powder, bloodstone powder, fluorite powder, orange crystal calcite powder, gypsum powder, aragonite powder, amethyst powder, red jasper powder, serpentine powder.
[0024] The above-mentioned biological crystal powder is subjected to modification treatment, comprising the following steps: S11, adding 5 g of biological crystal powder to a mixed solution of 600 mL of ethanol and 20 mL of water, and ultrasonically vibrating to evenly disperse the biological crystal powder in the solution to obtain a suspension; S12, adding silane coupling agent KH-560 to the above suspension, with the mass ratio of biological crystal powder to silane coupling agent being 1:0.4, heating to 50° C., stirring for reaction for 5 hours, centrifuging, washing, and drying to obtain preliminary modified biological crystal powder; S13, adding 1.5 g of polyethyleneimine into 300 mL of deionized water and stirring to dissolve to obtain a polyethyleneimine solution, adding the preliminary modified biocrystal powder into the polyethyleneimine solution, wherein the mass ratio of the preliminary modified biocrystal powder to the polyethyleneimine is 1:1, heating to 80° C., stirring to react for 3 h, and subjecting to centrifugal separation, washing, and drying, the product is obtained.
[0025] Example 2
[0026] A method for preparing wear-resistant and antistatic sofa fabric based on biological crystal powder comprises the following steps: S1, preparation of modified polyester fiber: 1) Polyethylene terephthalate, polyurethane, biocrystal powder and graphene oxide are uniformly mixed in a mass ratio of 20:12:3:0.5 to obtain a mixture; 2) The mixed material is added into a screw extruder and melted at a melting temperature of 183°C to obtain a spinning solution, which is then sent into a spinneret in a spinning box to be spun into primary fibers, which are then drawn and cooled to obtain the fibers; S2, blending spandex fiber, modified polyester fiber, polyester fiber, and nylon fiber in a mass ratio of 2:2:1:1, and then weaving to obtain a grey cloth; S3, placing the embryo in a dyeing vat for dyeing, taking it out and drying it at a drying temperature of 70°C.
[0027] The above-mentioned biological crystal powder is mixed by the following substances of equal mass: Tourmaline powder, bloodstone powder, fluorite powder, orange crystal calcite powder, gypsum powder, aragonite powder, amethyst powder, red jasper powder, serpentine powder.
[0028] The above-mentioned biological crystal powder is subjected to modification treatment, comprising the following steps: S11, adding 5 g of biological crystal powder to a mixed solution of 600 mL of ethanol and 20 mL of water, and ultrasonically vibrating to evenly disperse the biological crystal powder in the solution to obtain a suspension; S12, adding silane coupling agent KH-560 to the above suspension, with the mass ratio of biological crystal powder to silane coupling agent being 1:0.2, heating to 50° C., stirring for reaction for 5 hours, centrifuging, washing, and drying to obtain preliminary modified biological crystal powder; S13, adding 1.5 g of polyethyleneimine into 300 mL of deionized water and stirring to dissolve to obtain a polyethyleneimine solution, adding the preliminary modified biocrystal powder into the polyethyleneimine solution, the mass ratio of the preliminary modified biocrystal powder to polyethyleneimine being 1:0.7, heating to 80°C, stirring to react for 3 hours, and subjecting to centrifugal separation, washing, and drying to obtain the product.
[0029] Example 3
[0030] A method for preparing wear-resistant and antistatic sofa fabric based on biological crystal powder comprises the following steps: S1, preparation of modified polyester fiber: 1) Polyethylene terephthalate, polyurethane, biocrystal powder and graphene oxide are uniformly mixed in a mass ratio of 20:12:3:0.5 to obtain a mixture; 2) The mixed material is added into a screw extruder and melted at a melting temperature of 185°C to obtain a spinning solution, which is then sent to a spinneret in a spinning box to be spun into primary fibers, which are then drawn and cooled to obtain the fibers; S2, blending spandex fiber, modified polyester fiber, polyester fiber, and nylon fiber in a mass ratio of 2:2:1:1, and then weaving to obtain a grey cloth; S3, placing the embryo in a dyeing vat for dyeing, taking it out and drying it at a drying temperature of 75°C.
[0031] The above-mentioned biological crystal powder is mixed by the following substances of equal mass: Tourmaline powder, bloodstone powder, fluorite powder, orange crystal calcite powder, gypsum powder, aragonite powder, amethyst powder, red jasper powder, serpentine powder.
[0032] The above-mentioned biological crystal powder is subjected to modification treatment, comprising the following steps: S11, adding 5 g of biological crystal powder to a mixed solution of 600 mL of ethanol and 20 mL of water, and ultrasonically vibrating to evenly disperse the biological crystal powder in the solution to obtain a suspension; S12, adding silane coupling agent KH-560 to the above suspension, with the mass ratio of biological crystal powder to silane coupling agent being 1:0.3, heating to 50° C., stirring for reaction for 5 hours, centrifuging, washing, and drying to obtain preliminary modified biological crystal powder; S13, adding 1.5g polyethyleneimine into 300mL deionized water and stirring to dissolve to obtain polyethyleneimine solution, adding the preliminary modified biological crystal powder into the polyethyleneimine solution, the mass ratio of the preliminary modified biological crystal powder to polyethyleneimine is 1:0.8, heating to 80°C, stirring to react for 3h, centrifuging, washing and drying to obtain.
[0033] Example 4
[0034] A method for preparing wear-resistant and antistatic sofa fabric based on biological crystal powder comprises the following steps: S1, preparation of modified polyester fiber: 1) Polyethylene terephthalate, polyurethane, biocrystal powder and graphene oxide are uniformly mixed in a mass ratio of 20:12:3:0.5 to obtain a mixture; 2) The mixed material is added into a screw extruder and melted at a melting temperature of 190°C to obtain a spinning solution, which is then sent to a spinneret in a spinning box to be spun into primary fibers, which are then drawn and cooled to obtain the fibers; S2, blending spandex fiber, modified polyester fiber, polyester fiber, and nylon fiber in a mass ratio of 2:2:1:1, and then weaving to obtain a grey cloth; S3, placing the embryo in a dyeing vat for dyeing, taking it out and drying it at a drying temperature of 80°C.
[0035] The above-mentioned biological crystal powder is mixed by the following substances of equal mass: Tourmaline powder, bloodstone powder, fluorite powder, orange crystal calcite powder, gypsum powder, aragonite powder, amethyst powder, red jasper powder, serpentine powder.
[0036] The above-mentioned biological crystal powder is subjected to modification treatment, comprising the following steps: S11, adding 5 g of biological crystal powder to a mixed solution of 600 mL of ethanol and 20 mL of water, and ultrasonically vibrating to evenly disperse the biological crystal powder in the solution to obtain a suspension; S12, adding silane coupling agent KH-560 to the above suspension, with the mass ratio of biological crystal powder to silane coupling agent being 1:0.5, heating to 50° C., stirring for reaction for 5 hours, centrifuging, washing, and drying to obtain preliminary modified biological crystal powder; S13, adding 1.5 g of polyethyleneimine into 300 mL of deionized water and stirring to dissolve to obtain a polyethyleneimine solution, adding the preliminary modified biocrystal powder into the polyethyleneimine solution, the mass ratio of the preliminary modified biocrystal powder to polyethyleneimine being 1:1.2, heating to 80°C, stirring to react for 3 hours, and subjecting to centrifugal separation, washing, and drying to obtain the product.
[0037] Example 5
[0038] A method for preparing wear-resistant and antistatic sofa fabric based on biological crystal powder comprises the following steps: S1, preparation of modified polyester fiber: 1) Polyethylene terephthalate, polyurethane, biocrystal powder and graphene oxide are uniformly mixed in a mass ratio of 20:12:3:0.5 to obtain a mixture; 2) The mixed material is added into a screw extruder and melted at a melting temperature of 180°C to obtain a spinning solution, which is then sent to a spinneret in a spinning box to be spun into primary fibers, which are then drawn and cooled to obtain the fibers; S2, blending spandex fiber, modified polyester fiber, polyester fiber, and nylon fiber in a mass ratio of 2:2:1:1, and then weaving to obtain a grey cloth; S3, placing the embryo in a dyeing vat for dyeing, taking it out and drying it at a drying temperature of 70°C.
[0039] The above-mentioned biological crystal powder is mixed by the following substances of equal mass: Tourmaline powder, bloodstone powder, fluorite powder, orange crystal calcite powder, gypsum powder, aragonite powder, amethyst powder, red jasper powder, serpentine powder.
[0040] The above-mentioned biological crystal powder is subjected to modification treatment, comprising the following steps: S11, adding 5 g of biological crystal powder to a mixed solution of 600 mL of ethanol and 20 mL of water, and ultrasonically vibrating to evenly disperse the biological crystal powder in the solution to obtain a suspension; S12, adding silane coupling agent KH-560 to the above suspension, with the mass ratio of biological crystal powder to silane coupling agent being 1:0.1, heating to 50° C., stirring for reaction for 5 hours, centrifuging, washing, and drying to obtain preliminary modified biological crystal powder; S13, adding 1.5 g of polyethyleneimine into 300 mL of deionized water and stirring to dissolve to obtain a polyethyleneimine solution, adding the preliminary modified biocrystal powder into the polyethyleneimine solution, the mass ratio of the preliminary modified biocrystal powder to polyethyleneimine being 1:0.6, heating to 80°C, stirring to react for 3 hours, and subjecting to centrifugal separation, washing, and drying to obtain the product.
[0041] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that: No graphene oxide is added during the preparation of the modified polyester fiber.
[0042] The remaining steps are the same as those in Example 1.
[0043] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is: No biological crystal powder is added during the preparation of the modified polyester fiber.
[0044] The remaining steps are the same as those in Example 1.
[0045] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that: The biocrystal powder used in the preparation of modified polyester fiber has not been modified.
[0046] The remaining steps are the same as those in Example 1.
[0047] Performance Testing 1. Antistatic performance test: The antistatic performance of sofa fabrics is tested according to the method specified in GB / T24249-2009. The higher the resistivity, the better the antistatic performance of the fabric. The test results are shown in Table 1: Table 1
[0048] 2. Wear resistance test The wear resistance of sofa fabrics was tested using a Martindale abrasion tester. The mass of the sample holder was 200g, the mass of the weight was 300g, the effective diameter of the friction head was 30.0±0.5mm, and the abrasive was standard wool abrasive. Before the test, the sample was placed in a test environment in a relaxed state for more than 18b. During the test, the test was paused every 1000 wear cycles, the holder was removed, and the debris on the surface of the sample and the abrasive was gently cleaned with a brush, and then the test was continued until obvious holes appeared in the sample. The value on the reading disk was recorded at this time, and the average value of the three groups of samples was taken as the wear cycle number of the sample. The test results are shown in Table 2: Table 2
[0049] The far-infrared emission performance of sofa fabrics was tested using the GB / T30127-2013 method. The test results are shown in Table 3: Table 3
[0050] The above are only preferred embodiments of the present invention. It should be noted that the above preferred embodiments should not be regarded as limiting the present invention, and the protection scope of the present invention should be based on the scope defined by the claims. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the spirit and scope of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.
Claims
1. A method for preparing wear-resistant and antistatic sofa fabric based on biological crystal powder, characterized in that: The following steps are involved: S1, preparation of modified polyester fiber: 1) Polyethylene terephthalate, polyurethane, biocrystal powder and graphene oxide are uniformly mixed to obtain a mixture; 2) The mixed material is added into a screw extruder to melt to obtain a spinning solution, and the spinning solution is sent to a spinneret in a spinning box to spin into primary fibers, which are then drawn and cooled to obtain the fibers; S2, blending spandex fiber, modified polyester fiber, polyester fiber and nylon fiber, and then weaving to obtain a grey cloth; S3, placing the embryo in a dyeing vat for dyeing, taking it out and drying it.
2. The method for preparing a wear-resistant and antistatic sofa fabric based on biological crystal powder according to claim 1, characterized in that: In step S1, the biocrystal powder is mixed with the following substances: Tourmaline powder, bloodstone powder, fluorite powder, orange crystal calcite powder, gypsum powder, aragonite powder, amethyst powder, red jasper powder, serpentine powder.
3. The method for preparing a wear-resistant and antistatic sofa fabric based on biological crystal powder according to claim 2, characterized in that: The biological crystal powder is subjected to a modification process, comprising the following steps: S11, adding the biological crystal powder to a mixed solution of ethanol and water, and ultrasonically vibrating the solution to evenly disperse the biological crystal powder in the solution to obtain a suspension; S12, adding a silane coupling agent to the above suspension, heating, stirring for reaction, centrifuging, washing, and drying to obtain a preliminary modified biocrystal powder; S13, adding polyethyleneimine into deionized water and stirring to dissolve to obtain polyethyleneimine solution, adding the preliminary modified biocrystal powder into the polyethyleneimine solution, heating to react, and obtaining the product.
4. The method for preparing a wear-resistant and antistatic sofa fabric based on biological crystal powder according to claim 3, characterized in that: The mass ratio of the biological crystal powder to the silane coupling agent is 1:0.1-0.
5.
5. The method for preparing a wear-resistant and antistatic sofa fabric based on biological crystal powder according to claim 3, characterized in that: The mass ratio of the preliminary modified biological crystal powder to polyethyleneimine is 1:0.6-1.
2.
6. The method for preparing a wear-resistant and antistatic sofa fabric based on biological crystal powder according to claim 1, characterized in that: In step S1, the melting temperature of the raw materials is 180-190°C.
7. The method for preparing a wear-resistant and antistatic sofa fabric based on biological crystal powder according to claim 1, characterized in that: In step S3, the drying temperature is controlled at 70-80°C.
8. A wear-resistant and antistatic sofa fabric based on biological crystal powder, characterized in that: The method is prepared by any one of claims 1 to 7 above.
Citation Information
Patent Citations
Sofa fabric good in abrasion resistance
CN106978664A
Preparation method of graphene modified polyester blended fabric
CN109082727A
Antistatic and wear-resistant sofa fabric and preparation method thereof
CN113684691A
Fabric treatment process for improving wear resistance of clothes fabric
CN116200951A
Anti-static fabric and preparation method thereof
CN117684315A