Micro-nano patterned porous fiber membrane as well as preparation method and application thereof

Through electrospinning technology, the pore-containing micro-nano structure and the addition of conductive fillers are solved, and the problems of high sensitivity and wide response of flexible pressure sensors are achieved, efficient and economical fiber membrane preparation is achieved, and sensor performance and production efficiency are improved.

CN118932603APending Publication Date: 2024-11-12WUYI UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410918545.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is difficult to achieve high sensitivity and wide response range of flexible pressure sensors simultaneously, and faces the problems of expensive materials and complex production processes.

Method used

Electrospinning technology is used to copy the pore-containing micro-nano structure template to the fiber membrane to form a patterned fiber membrane, and conductive fillers such as carbon nanotubes and graphene are added to the spinning membrane, which is formed by suction filtration. Sensitivity and wide response range of fiber membranes.

Benefits of technology

The high sensitivity and wide response range of fiber membranes are achieved, which reduces production costs and improves process efficiency and controllability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932603A_ABST
    Figure CN118932603A_ABST
Patent Text Reader

Abstract

The invention discloses a micro-nano patterned porous fiber membrane as well as a preparation method and application thereof. Relates to the technical field of pressure sensor materials. The fiber membrane comprises the following components: thermoplastic polyurethane; a conductive filler; according to the fiber membrane, a porous micro-nano structure on a template is copied to the fiber membrane through an electrostatic spinning technology, so that the fiber membrane with a patterned structure is formed. According to the fiber membrane disclosed by the invention, the porous micro-nano structure on the template is copied to the fiber membrane through an electrostatic spinning technology, and the obtained fiber membrane with a patterned structure has a relatively high surface area and a multi-stage sub-microstructure, so that the sensitivity of fibers to external stimulation can be remarkably improved. Therefore, the sensitivity of the sensor can be greatly improved, and the response range of the sensor can be expanded. The micro-nano patterned structure enables the spun fiber membrane to present patterns on the template, and the template has a specific shape and arrangement, so that the collection efficiency of fibers can be improved, the fibers are prevented from being wound and accumulated, and the uniformity of the fibers is kept.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of pressure sensor materials, and in particular to a micro-nano patterned porous fiber membrane and a preparation method and application thereof. Background Art

[0002] Thermoplastic polyurethane (TPU) strain-type flexible sensors have the remarkable characteristics of light weight, large strain range, and simple production. They have a wide range of applications and meet the various requirements of today's intelligent flexible devices very well, showing very good application prospects.

[0003] At the same time, electrospun nanofibers have a high specific surface area and porosity. Therefore, TPU electrospun membranes not only have the advantages of light weight, large strain range and easy production, but also have the characteristics of high specific surface area and porosity, which helps to increase the contact area between the sensor and the object being detected, greatly improving the sensitivity and other sensing properties of the sensor.

[0004] In particular, when the copper mesh is used as the receiver of the electrospinning microflow, a special pattern can be produced, and this structure significantly improves the performance of the sensor. The electrospinning membrane pattern based on this copper mesh breaks the tradition and provides a new research idea for obtaining sensor substrates by electrospinning.

[0005] Based on the new electrospinning mode, a flexible pressure sensing membrane designed by 3D graphene film grown by chemical vapor deposition (CVD) has been prepared by existing technology, which has a pressure range of 110 (kPa) in the pressure range of 0-0.2 kPa. -1 In addition, there are existing technologies for preparing multifunctional sensors designed and manufactured using natural lotus leaf bionic microstructures and independent polypyrrole / silver (PPy / Ag) hybrid membranes, as well as sensors designed based on PDMS micropatterned substrates, all of which have good strain performance due to their large effective contact area.

[0006] Nevertheless, sensors prepared by existing technical solutions still have the problem of being unable to achieve high sensitivity and wide response at the same time, and also face the challenges of expensive materials and complex manufacturing processes. Summary of the invention

[0007] The purpose of the present invention is to develop a micro-nano patterned porous fiber membrane loaded on a flexible pressure sensor, so that the flexible pressure sensor has the performance of high sensitivity and wide response.

[0008] The first aspect of the present invention is:

[0009] A fiber membrane is provided.

[0010] A second aspect of the present invention is:

[0011] Provided is a method for preparing a fiber membrane.

[0012] The third aspect of the present invention is:

[0013] Application of the fiber membrane.

[0014] The invention also provides a flexible pressure sensor.

[0015] Specifically, the technical solution adopted according to the first aspect of the present invention is:

[0016] A fiber membrane, the components of which include:

[0017] Thermoplastic polyurethane;

[0018] Conductive fillers;

[0019] The fiber membrane is formed by replicating the porous micro-nano structure on the template onto the fiber membrane through electrostatic spinning technology, thereby forming a fiber membrane with a patterned structure.

[0020] According to the embodiments of the present invention, one of the technical solutions has at least one of the following advantages or beneficial effects:

[0021] The fiber membrane of the present invention copies the porous micro-nano structure on the template to the fiber membrane through electrostatic spinning technology to obtain a fiber membrane with a patterned structure, wherein the porous micro-nano structure on the template directly corresponds to the patterned structure. The fiber membrane with a patterned structure obtained by the present invention has a high surface area and a multi-level microstructure, which can significantly increase the sensitivity of the fiber to external stimuli. Therefore, the sensitivity of the sensor can be greatly improved and its response range can be expanded. The micro-nano patterned structure makes the woven fiber membrane present the pattern on the template. Since the template has a specific shape and arrangement, the collection efficiency of the fiber can be improved, the fiber entanglement and accumulation can be prevented, and the uniformity of the fiber can be maintained.

[0022] According to one embodiment of the present invention, the fiber membrane of the present invention is adjustable, and the micro-nano patterned structure can realize the direct manufacture of nanofibers by controlling the shape structure type of the receiving plate and controlling the distance and voltage between the nozzle and the collecting plate, thereby realizing precise control of the micro-nano structure.

[0023] According to one embodiment of the present invention, the conductive filler includes carbon nanotubes and graphene.

[0024] According to one embodiment of the present invention, the template includes a wire mesh and sandpaper.

[0025] Wire mesh and sandpaper can increase the fiber contact area and maintain fiber uniformity, thereby improving the sensitivity and response range of the sensor.

[0026] According to one embodiment of the present invention, the steel wire mesh is a steel wire mesh of 100-500 meshes.

[0027] According to one embodiment of the present invention, the sandpaper is 120-320 mesh sandpaper.

[0028] Specifically, the technical solution adopted according to the second aspect of the present invention is:

[0029] A method for preparing the fiber membrane comprises the following steps:

[0030] S1 mixes thermoplastic polyurethane with a solvent to prepare a spinning solution;

[0031] S2 uses the porous micro-nanostructure template as a pattern template on an electrospinning receiving device, and spins the spinning solution onto the template to obtain a spinning membrane;

[0032] S3 prepares the conductive filler into a dispersion liquid, mixes the dispersion liquid with the spinning membrane, and obtains the fiber membrane through suction filtration.

[0033] According to the embodiments of the present invention, one of the technical solutions has at least one of the following advantages or beneficial effects:

[0034] First, by using a porous micro-nanostructure template as a pattern template on the electrospinning receiving device, complex microstructures can be effectively replicated on the fiber membrane. This precise structural replication not only improves the surface properties and functionality of the fiber membrane, but also can directionally regulate the pore structure and surface morphology of the fiber membrane to meet the specific needs of different applications for the fiber membrane.

[0035] Secondly, the fiber membrane obtained by mixing the conductive filler into the spinning solution and filtering it has good conductive properties. This makes the fiber membrane widely used in electronic devices, sensors and smart materials, such as electronic skin, flexible electronic devices, etc., providing an important functional basis for these applications.

[0036] In addition, the entire preparation process is relatively efficient and controllable. By adjusting the formula of the spinning solution and the spinning parameters, the thickness, pore size and distribution of the fiber membrane, and the conductive properties can be precisely controlled. This precise process control not only improves the quality and consistency of the product, but also helps to reduce production costs and resource consumption.

[0037] According to one embodiment of the present invention, in the spinning solution, the mass percentage of thermoplastic polyurethane is 25-30%.

[0038] According to one embodiment of the present invention, the solvent in step S1 includes N,N-dimethylformamide and tetrahydrofuran.

[0039] According to one embodiment of the present invention, the volume ratio of N,N-dimethylformamide to tetrahydrofuran is 1-1.2:1-1.2.

[0040] According to one embodiment of the present invention, in step S2, when the spinning solution is spun onto the template, in order to prevent the jet thread from deviating up and down during spinning, a conductive copper foil tape is used to be made into a horn shape to control the spinning range.

[0041] According to one embodiment of the present invention, when the porous micro-nano structure template is a steel wire mesh, the spinning parameters during the spinning process are:

[0042]

[0043] Electrospinning is a method of spinning polymer solutions or molten polymers into fibers using an electric field. In this process, in particular, winding speed, humidity and receiving distance have an important influence on fiber formation and quality.

[0044] The winding speed affects the speed at which the fibers are collected. Too high a winding speed may cause insufficient stretching or incomplete solidification of the fibers, affecting the quality and morphology of the fibers. Humidity directly affects the viscosity of the solution or molten polymer. High humidity will increase the viscosity, resulting in uneven fiber formation or failure to form complete fibers. The receiving distance refers to the distance from the spinning nozzle to the collector. Too large a distance may cause the fibers to be incompletely solidified in the air or be affected by external factors, resulting in a decrease in quality.

[0045] Among them, the main spinning parameter that affects the fiber viscosity is humidity, which has a significant effect on the solvent evaporation rate and fiber solidification rate during electrospinning, thereby affecting the fiber morphology and mechanical properties. Higher humidity usually slows down the evaporation of the solvent, making the fibers more likely to aggregate and stick together during flight, thereby increasing the viscosity of the fibers.

[0046] According to one embodiment of the present invention, when the porous micro-nano structure template is sandpaper, the spinning parameters in the spinning process are:

[0047]

[0048] According to one embodiment of the present invention, in S3, the filtration operation also includes the following steps: firstly mixing the carbon nanotube dispersion and the spinning membrane, filtering and drying them, and then mixing the spinning membrane and the graphene dispersion, filtering and drying them to obtain the fiber membrane.

[0049] Another aspect of the present invention further provides a flexible pressure sensor, which includes the fiber membrane as described in the first embodiment. Since the application adopts all the technical solutions of the fiber membrane, it has at least all the beneficial effects brought by the technical solutions of the above embodiment.

[0050] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be obvious from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0052] Figure 1 DSLM diagram of the template used in Examples 1-6.

[0053] Figure 2 DSLM images of the fiber membranes prepared in Examples 1-6.

[0054] Figure 3 The resistance change curve of the pressure sensor prepared by the fiber membrane of Examples 1-3 and Comparative Example 1 is shown.

[0055] Figure 4 It is a sensitivity coefficient diagram of the fiber membrane of Examples 1-3, Comparative Example 1, and the prepared pressure sensor.

[0056] Figure 5 This is a sensitivity coefficient diagram of the pressure sensors prepared using the fiber membranes of Examples 4-6 and Comparative Example 2.

[0057] Figure 6 This is a stability test chart of the pressure sensor prepared based on the fiber membrane of Example 6.

[0058] Figure 7 This is a response range test chart of the pressure sensor prepared based on the fiber membrane of Example 6. DETAILED DESCRIPTION

[0059] In the description of the present invention, if there is a description of first, second, etc., it is only for the purpose of distinguishing technical features, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features or implicitly indicating the order of the indicated technical features.

[0060] In the description of the present invention, it should be understood that descriptions involving orientation, such as orientation or positional relationship indicated as up, down, etc., are based on the orientation or positional relationship shown in the embodiments, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.

[0061] The words "preferably", "more preferably", etc. in the present invention refer to embodiments of the present invention that may provide certain beneficial effects in certain circumstances. However, other embodiments may also be preferred under the same circumstances or other circumstances. In addition, the description of one or more preferred embodiments does not imply that other embodiments are not applicable, nor is it intended to exclude other embodiments from the scope of the present invention.

[0062] When a numerical range is disclosed herein, the above range is considered to be continuous and includes the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0063] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of the present invention.

[0064] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0065] Example 1

[0066] A fiber membrane, the components of which include:

[0067] Thermoplastic polyurethane;

[0068] Conductive fillers;

[0069] The fiber membrane is formed by replicating the micro-nano structure on the steel wire mesh onto the fiber membrane through electrostatic spinning technology, thereby forming a fiber membrane with a patterned structure.

[0070] The method for preparing the above-mentioned fiber membrane comprises the following steps:

[0071] S1 uses N, N-dimethylformamide DMF and tetrahydrofuran THF in a volume ratio of 1:1 as solvent and thermoplastic polyurethane TPU particles as solute, and prepares a spinning solution with a TPU concentration of 25% by magnetic stirring;

[0072] 800 ml of 0.01% uniform carbon nanotube dispersion was prepared with a carbon nanotube dispersion having a mass percentage concentration of 5% produced by Suzhou Tanfeng Graphene Technology Co., Ltd., and ultrasonically treated for 3 minutes at low temperature (11-15°C) using an ultrasonic device, and 40 g of the upper layer of dispersion was taken to obtain a first conductive filler dispersion, which was evenly divided into four portions (10 g each); 0.4 g of graphene GR was weighed using an electronic balance, 60 g of isopropanol was added to a clean and dry reagent bottle, and ultrasonicated for 1 hour in an ultrasonic device, and after dispersion, 2 / 3 of the upper layer of dispersion (40 g) was taken to obtain a second conductive filler dispersion, which was evenly divided into four portions (10 g each);

[0073] S2 uses a 500-mesh steel wire mesh as a pattern template on an electrospinning receiving device, and uses an electrospinning machine for spinning. The prepared spinning solution is added to a 10 ml plastic syringe with a spinneret. In order to prevent the jet wire from deviating up and down during spinning, a conductive copper foil tape is used to make a horn shape to control the spinneret range, so that the spun fiber membrane has good uniformity. After 6 hours of spinning, a spinning membrane is obtained;

[0074] S3 sequentially mixes the spinning membrane with four portions of the first conductive filler dispersion and sequentially filters them. Between each two filtrations, the membrane needs to be washed with anhydrous ethanol and deionized water and dried. After the four filtrations, the membrane is washed with anhydrous ethanol and deionized water and dried. The fiber membrane treated with the first conductive filler dispersion is sequentially mixed with four portions of the second conductive filler dispersion and sequentially filtered. After washing and drying, the fiber membrane is obtained.

[0075] The spinning parameters during the spinning process are:

[0076]

[0077] Example 2

[0078] The difference between Example 2 and Example 1 is that the template used in Example 2 is a 300-mesh steel wire mesh.

[0079] A fiber membrane, the components of which include:

[0080] Thermoplastic polyurethane;

[0081] Conductive fillers;

[0082] The fiber membrane is formed by replicating the micro-nano structure on the steel wire mesh onto the fiber membrane through electrostatic spinning technology, thereby forming a fiber membrane with a patterned structure.

[0083] The method for preparing the above-mentioned fiber membrane comprises the following steps:

[0084] S1 uses N, N-dimethylformamide DMF and tetrahydrofuran THF in a volume ratio of 1:1 as solvent and thermoplastic polyurethane TPU particles as solute, and prepares a spinning solution with a TPU concentration of 25% by magnetic stirring;

[0085] 800 ml of 0.01% uniform carbon nanotube dispersion was prepared with a carbon nanotube dispersion having a mass percentage concentration of 5% produced by Suzhou Tanfeng Graphene Technology Co., Ltd., and ultrasonically treated for 3 minutes at low temperature (11-15°C) using an ultrasonic device, and 40 g of the upper layer of dispersion was taken to obtain a first conductive filler dispersion, which was evenly divided into four portions (10 g each); 0.4 g of graphene GR was weighed using an electronic balance, 60 g of isopropanol was added to a clean and dry reagent bottle, and ultrasonicated for 1 hour in an ultrasonic device, and after dispersion, 2 / 3 of the upper layer of dispersion (40 g) was taken to obtain a second conductive filler dispersion, which was evenly divided into four portions (10 g each);

[0086] S2 used a 300-mesh steel wire mesh as a pattern template on the electrospinning receiving device, and used an electrospinning machine for spinning. The prepared spinning solution was added to a 10 ml plastic syringe with a spinneret. In order to prevent the jet wire from deviating up and down during spinning, a conductive copper foil tape was used to make a horn shape to control the spinneret range, so that the spun fiber membrane had good uniformity. After 6 hours of spinning, a spinning membrane was obtained;

[0087] S3 sequentially mixes the spinning membrane with four portions of the first conductive filler dispersion and sequentially filters them. Between each two filtrations, the membrane needs to be washed with anhydrous ethanol and deionized water and dried. After the four filtrations, the membrane is washed with anhydrous ethanol and deionized water and dried. The fiber membrane treated with the first conductive filler dispersion is sequentially mixed with four portions of the second conductive filler dispersion and sequentially filtered. After washing and drying, the fiber membrane is obtained.

[0088] The spinning parameters during the spinning process are:

[0089]

[0090] Example 3

[0091] The difference between Example 3 and Example 1 is that the template used in Example 3 is a 100-mesh steel wire mesh.

[0092] A fiber membrane, the components of which include:

[0093] Thermoplastic polyurethane;

[0094] Conductive fillers;

[0095] The fiber membrane is formed by replicating the micro-nano structure on the steel wire mesh onto the fiber membrane through electrostatic spinning technology, thereby forming a fiber membrane with a patterned structure.

[0096] The method for preparing the above-mentioned fiber membrane comprises the following steps:

[0097] S1 uses N, N-dimethylformamide DMF and tetrahydrofuran THF in a volume ratio of 1:1 as solvent and thermoplastic polyurethane TPU particles as solute, and prepares a spinning solution with a TPU concentration of 25% by magnetic stirring;

[0098] 800 ml of 0.01% uniform carbon nanotube dispersion was prepared with a carbon nanotube dispersion having a mass percentage concentration of 5% produced by Suzhou Tanfeng Graphene Technology Co., Ltd., and ultrasonically treated for 3 minutes at low temperature (11-15°C) using an ultrasonic device, and 40 g of the upper layer of dispersion was taken to obtain a first conductive filler dispersion, which was evenly divided into four portions (10 g each); 0.4 g of graphene GR was weighed using an electronic balance, 60 g of isopropanol was added to a clean and dry reagent bottle, and ultrasonicated for 1 hour in an ultrasonic device, and after dispersion, 2 / 3 of the upper layer of dispersion (40 g) was taken to obtain a second conductive filler dispersion, which was evenly divided into four portions (10 g each);

[0099] S2 uses a 100-mesh steel wire mesh as a pattern template on an electrospinning receiving device, and uses an electrospinning machine for spinning. The prepared spinning solution is added to a 10 ml plastic syringe with a spinneret. In order to prevent the jet wire from deviating up and down during spinning, a conductive copper foil tape is used to make a horn shape to control the spinneret range, so that the spun fiber membrane has good uniformity. After 6 hours of spinning, a spinning membrane is obtained;

[0100] S3 sequentially mixes the spinning membrane with four portions of the first conductive filler dispersion and sequentially filters them. Between each two filtrations, the membrane needs to be washed with anhydrous ethanol and deionized water and dried. After the four filtrations, the membrane is washed with anhydrous ethanol and deionized water and dried. The fiber membrane treated with the first conductive filler dispersion is sequentially mixed with four portions of the second conductive filler dispersion and sequentially filtered. After washing and drying, the fiber membrane is obtained.

[0101] The spinning parameters during the spinning process are:

[0102]

[0103] Example 4

[0104] The difference between Example 4 and Example 1 is that the template used in Example 4 is 120-mesh sandpaper.

[0105] A fiber membrane, the components of which include:

[0106] Thermoplastic polyurethane;

[0107] Conductive fillers;

[0108] The fiber membrane is formed by replicating the micro-nano structure on the sandpaper onto the fiber membrane through electrostatic spinning technology, thereby forming a fiber membrane with a patterned structure.

[0109] The method for preparing the above-mentioned fiber membrane comprises the following steps:

[0110] S1 uses N, N-dimethylformamide DMF and tetrahydrofuran THF in a volume ratio of 1:1 as solvent and thermoplastic polyurethane TPU particles as solute, and prepares a spinning solution with a TPU concentration of 25% by magnetic stirring;

[0111] 800 ml of 0.01% uniform carbon nanotube dispersion was prepared with a carbon nanotube dispersion having a mass percentage concentration of 5% produced by Suzhou Tanfeng Graphene Technology Co., Ltd., and ultrasonically treated for 3 minutes at low temperature (11-15°C) using an ultrasonic device, and 40 g of the upper layer of dispersion was taken to obtain a first conductive filler dispersion, which was evenly divided into four portions (10 g each); 0.4 g of graphene GR was weighed using an electronic balance, 60 g of isopropanol was added to a clean and dry reagent bottle, and ultrasonicated for 1 hour in an ultrasonic device, and after dispersion, 2 / 3 of the upper layer of dispersion (40 g) was taken to obtain a second conductive filler dispersion, which was evenly divided into four portions (10 g each);

[0112] S2 uses 120-mesh sandpaper as the pattern template on the electrospinning receiving device, uses an electrospinning machine for spinning, and adds the prepared spinning solution into a 10 ml plastic syringe with a spinneret. In order to prevent the jet wire from shifting up and down during spinning, a conductive copper foil tape is used to make a horn shape to control the spinneret range, so that the spun fiber membrane has good uniformity. After 6 hours of spinning, a spinning membrane is obtained;

[0113] S3 sequentially mixes the spinning membrane with four portions of the first conductive filler dispersion and sequentially filters them. Between each two filtrations, the membrane needs to be washed with anhydrous ethanol and deionized water and dried. After the four filtrations, the membrane is washed with anhydrous ethanol and deionized water and dried. The fiber membrane treated with the first conductive filler dispersion is sequentially mixed with four portions of the second conductive filler dispersion and sequentially filtered. After washing and drying, the fiber membrane is obtained.

[0114] The spinning parameters during the spinning process are:

[0115]

[0116] Example 5

[0117] The difference between Example 5 and Example 1 is that the template used in Example 5 is 220-mesh sandpaper.

[0118] A fiber membrane, the components of which include:

[0119] Thermoplastic polyurethane;

[0120] Conductive fillers;

[0121] The fiber membrane is formed by replicating the micro-nano structure on the sandpaper onto the fiber membrane through electrostatic spinning technology, thereby forming a fiber membrane with a patterned structure.

[0122] The method for preparing the above-mentioned fiber membrane comprises the following steps:

[0123] S1 uses N, N-dimethylformamide DMF and tetrahydrofuran THF in a volume ratio of 1:1 as solvent and thermoplastic polyurethane TPU particles as solute, and prepares a spinning solution with a TPU concentration of 25% by magnetic stirring;

[0124] 800 ml of 0.01% uniform carbon nanotube dispersion was prepared with a carbon nanotube dispersion having a mass percentage concentration of 5% produced by Suzhou Tanfeng Graphene Technology Co., Ltd., and ultrasonically treated for 3 minutes at low temperature (11-15°C) using an ultrasonic device, and 40 g of the upper layer of dispersion was taken to obtain a first conductive filler dispersion, which was evenly divided into four portions (10 g each); 0.4 g of graphene GR was weighed using an electronic balance, 60 g of isopropanol was added to a clean and dry reagent bottle, and ultrasonicated for 1 hour in an ultrasonic device, and after dispersion, 2 / 3 of the upper layer of dispersion (40 g) was taken to obtain a second conductive filler dispersion, which was evenly divided into four portions (10 g each);

[0125] S2 uses 220-mesh sandpaper as the pattern template on the electrospinning receiving device, and uses an electrospinning machine for spinning. The prepared spinning solution is added to a 10 ml plastic syringe with a spinneret. In order to prevent the jet wire from deviating up and down during spinning, a conductive copper foil tape is used to make a horn shape to control the spinneret range, so that the spun fiber membrane has good uniformity. After 6 hours of spinning, a spinning membrane is obtained;

[0126] S3 sequentially mixes the spinning membrane with four portions of the first conductive filler dispersion and sequentially filters them. Between each two filtrations, the membrane needs to be washed with anhydrous ethanol and deionized water and dried. After the four filtrations, the membrane is washed with anhydrous ethanol and deionized water and dried. The fiber membrane treated with the first conductive filler dispersion is sequentially mixed with four portions of the second conductive filler dispersion and sequentially filtered. After washing and drying, the fiber membrane is obtained.

[0127] The spinning parameters during the spinning process are:

[0128]

[0129] Example 6

[0130] The difference between Example 6 and Example 1 is that the template used in Example 6 is 320-mesh sandpaper.

[0131] A fiber membrane, the components of which include:

[0132] Thermoplastic polyurethane;

[0133] Conductive fillers;

[0134] The fiber membrane is formed by replicating the micro-nano structure on the sandpaper onto the fiber membrane through electrostatic spinning technology, thereby forming a fiber membrane with a patterned structure.

[0135] The method for preparing the above-mentioned fiber membrane comprises the following steps:

[0136] S1 uses N, N-dimethylformamide DMF and tetrahydrofuran THF in a volume ratio of 1:1 as solvent and thermoplastic polyurethane TPU particles as solute, and prepares a spinning solution with a TPU concentration of 25% by magnetic stirring;

[0137] 800 ml of 0.01% uniform carbon nanotube dispersion was prepared with a carbon nanotube dispersion having a mass percentage concentration of 5% produced by Suzhou Tanfeng Graphene Technology Co., Ltd., and ultrasonically treated for 3 minutes at low temperature (11-15°C) using an ultrasonic device, and 40 g of the upper layer of dispersion was taken to obtain a first conductive filler dispersion, which was evenly divided into four portions (10 g each); 0.4 g of graphene GR was weighed using an electronic balance, 60 g of isopropanol was added to a clean and dry reagent bottle, and ultrasonicated for 1 hour in an ultrasonic device, and after dispersion, 2 / 3 of the upper layer of dispersion (40 g) was taken to obtain a second conductive filler dispersion, which was evenly divided into four portions (10 g each);

[0138] S2 used 320-mesh sandpaper as the pattern template on the electrospinning receiving device, and used an electrospinning machine for spinning. The prepared spinning solution was added to a 10 ml plastic syringe with a spinneret. In order to prevent the jet wire from shifting up and down during spinning, a conductive copper foil tape was used to make a horn shape to control the spinneret range, so that the spun fiber membrane had good uniformity. After 6 hours of spinning, a spinning membrane was obtained;

[0139] S3 sequentially mixes the spinning membrane with four portions of the first conductive filler dispersion and sequentially filters them. Between each two filtrations, the membrane needs to be washed with anhydrous ethanol and deionized water and dried. After the four filtrations, the membrane is washed with anhydrous ethanol and deionized water and dried. The fiber membrane treated with the first conductive filler dispersion is sequentially mixed with four portions of the second conductive filler dispersion and sequentially filtered. After washing and drying, the fiber membrane is obtained.

[0140] The spinning parameters during the spinning process are:

[0141]

[0142] Comparative Example 1

[0143] The difference between Comparative Example 1 and Example 1 is that the template used in Comparative Example 1 is tin foil.

[0144] Comparative Example 2

[0145] The difference between Comparative Example 2 and Example 1 is that the template used in Comparative Example 2 is smooth silicone oil paper.

[0146] Comparative Example 3

[0147] The difference between Comparative Example 3 and Example 1 is that the electrospinning parameters are different. Among them, the spinning parameters of Example 1 are:

[0148]

[0149] Among them, the electrospinning parameters of Comparative Example 3 are:

[0150]

[0151] The viscosity of the fiber spun by using the parameters of Comparative Example 3 is very high and a fiber film cannot be spun.

[0152] Comparative Example 4

[0153] The difference between Comparative Example 4 and Example 2 is that the electrospinning parameters are different. Among them, the spinning parameters of Example 2 are:

[0154]

[0155]

[0156] Wherein, the spinning parameters of Comparative Example 4 are:

[0157]

[0158] The viscosity of the fiber spun by the parameters of Comparative Example 4 is very high, and a fiber film cannot be spun.

[0159] Performance Testing:

[0160] The templates used in Examples 1-6 were characterized by using a microscope. The template structure is shown in FIG. Figure 1 As shown. Figure 1 (a) is a super depth of field microscope (DSLM) image of the template used in Example 1, Figure 1 (b) is a DSLM diagram of the template used in Example 2; Figure 1 (c) is a DSLM diagram of the template used in Example 3; Figure 1 (d) is a DSLM diagram of the template used in Example 4; Figure 1 (e) is a DSLM diagram of the template used in Example 5; Figure 1 (f) in the figure is the DSLM image of the template used in Example 6.

[0161] The fiber membranes prepared in Examples 1-6 were characterized by using a microscope. The fiber membrane structure is shown in FIG. Figure 2 As shown. Figure 2 (a) is a DSLM image of the fiber membrane of Example 1, Figure 2 (b) is a DSLM image of the fiber membrane of Example 2; Figure 2 (c) is a DSLM image of the fiber membrane of Example 3; Figure 2 (d) is the DSLM image of the fiber membrane of Example 4; Figure 2 (e) is a DSLM image of the fiber membrane of Example 5; Figure 2 (f) in the figure is the DSLM image of the fiber membrane of Example 6.

[0162] pass Figure 1-2 By comparison, it can be observed that the fiber membrane prepared in the embodiment is affected by the pattern structure of the steel wire mesh or sandpaper with different mesh sizes, forming different micro-nano patterned structures.

[0163] The fiber membranes prepared in Examples 1-6 were used as sensing elements and packaged into pressure sensors in combination with electrodes to test the sensitivity, stability and response range of the pressure sensors.

[0164] Among them, the sensitivity test method is: use a flexible electronic tester to measure the deformation and resistance of the sample, thereby calculating the strain and its resistance change. By measuring the relationship between strain and resistance change, the sensitivity coefficient and response range characteristics of the sample can be determined.

[0165] Specifically, the sensitivity test method of the pressure sensor prepared by the fiber membrane (the template is a steel mesh) of Examples 1-3 is as follows:

[0166] Cut the fiber membrane into 50mmX10mm specifications, reserve 20mm in the middle, and stick copper foil tape on both sides. Take the reserved part in the middle of the clamped sample with an original length of 20mm and pre-stretch 1mm. Set different stretching distances, 3, 20, and 40mm respectively. Set different stretching speeds, 1mm / s and 40mm / s respectively. Combined test.

[0167] The sensitivity of the strain sensor (G F )The formula is as follows:

[0168] G F =(△R / R0) / ε;

[0169] In the above formula: ΔR is the resistance change, unit is Ω; R0 is the original resistance, unit is Ω; ε is the material strain rate, unit is %.

[0170] After the above method is used to measure, the resistance change curve of the pressure sensor prepared by the fiber membrane of Examples 1-3 is as follows: Figure 3 As shown, the sensitivity coefficients of the pressure sensors prepared by the fiber membranes of Examples 1-3 at different stretching distances and speeds are as follows: Figure 4 shown.

[0171] in, Figure 3 m in the figure is the resistance change curve of the strain type pressure sensor of the micro-nano patterned fiber membrane with a 100 mesh steel wire mesh as the receiving template (corresponding to Example 3), Figure 3 In Figure n, the resistance change curve of the strain type pressure sensor of the micro-nano patterned fiber membrane using a 300 mesh steel wire mesh as the receiving template (corresponding to Example 2) is shown. Figure 3 Figure o is a resistance change curve of a strain type pressure sensor of a micro-nano patterned fiber membrane using a 500 mesh steel wire mesh as a receiving template (corresponding to Example 1). Figure 3 Figure p is the resistance change curve of the strain pressure sensor of the micro-nano patterned fiber membrane using tin foil as the template (blank test of comparative example 1). It can be seen that the sensor resistance change of the 300-mesh steel wire mesh template is the most stable, and the response is more stable.

[0172] in, Figure 4 It can be seen that the sensitivity coefficient of the 300-mesh steel mesh template (corresponding to Example 2) in three kinds of stretching changes is the highest, so it is proved that the 300-mesh steel mesh template can improve the sensitivity coefficient of the sensor. Wherein, the 300-mesh steel mesh, as a receiving template, can lead to the highest sensitivity during electrostatic spinning. This is because the 300-mesh grid has a moderate pore size, which can effectively capture the fiber formed by electrostatic spinning, and maintain the uniformity and morphology of the fiber membrane. In addition, the 300-mesh grid has an appropriate surface roughness, which helps to form a more uniform and dense fiber mesh, thereby improving the responsiveness of the fiber membrane to external changes. During the stretching process, the 300-mesh grid can provide enough support and stability to ensure that the fiber maintains structural integrity during the stretching process. Even when the stretching speed is low (1mm / s), the 300-mesh grid can still maintain its advantage, because the lower stretching speed helps to more finely control the morphology of the fiber, further enhancing the sensitivity of the fiber membrane.

[0173] Specifically, the sensitivity test method of the pressure sensor prepared based on the fiber membranes of Examples 4-6 (the template is sandpaper) and the fiber membrane of Comparative Example 2 is as follows: the fiber membranes obtained in Examples 4-6 are cut into 5 cm × 1 cm strip samples, and double-sided conductive copper foil is attached to both sides. The parameters are uniformly set on the flexibility tester: the clamping distance is 20 mm, the stretching distance is 3 mm and 5 mm, the stretching speed is uniformly 1 mm / s, and the number of stretching times is 20 times.

[0174] The sensitivity coefficients of the pressure sensors prepared based on the fiber membranes of Examples 4-6 (the template is sandpaper) and the fiber membrane of Comparative Example 2 under different tensile strains are shown in the figure below: Figure 5 shown.

[0175] from Figure 5 It is known that the sensitivity of the sensor with sandpaper template is generally higher than that of the sensor with silicone oil paper blank control (corresponding to Example 2). And when the tensile strain rate is 15%, the sensor sensitivity coefficient of the 320-mesh sandpaper template (corresponding to Example 6) is as high as 7.65, which is 89.3% higher than the sensitivity coefficient of the silicone oil paper template under the same strain. Therefore, using sandpaper as a receiving template can improve the sensitivity performance of the sensor. It should be noted that because the 320-mesh sandpaper can produce a smoother and more uniform surface, it is beneficial to the detection of small changes in applications such as sensors, so that when stretched 20 times at a stretch rate of 15%, the fiber membrane prepared using 320-mesh sandpaper shows a higher sensitivity. However, when the stretch rate is increased to 25%, the sensitivity of the fiber membrane prepared using 320-mesh sandpaper decreases the most. This is because under higher stress, the surface of the 320-mesh fiber membrane will undergo slight changes or damage, thereby reducing its ability to respond to changes. In contrast, fiber membranes prepared with coarser sandpaper (e.g., 120-mesh or 220-mesh) performed more stably under high tensile conditions because their surfaces were more able to withstand higher tensile stresses without being damaged.

[0176] The stability of the pressure sensor prepared based on the fiber membrane of Example 6 was tested. The test results are as follows: Figure 6 The test method is: the pressure sensor is stretched 100 times at a tensile strain rate of 25%. Figure 6 It is known that after 100 times of stretching at a strain rate of 25%, the resistance change rate and the sensor response speed remain almost unchanged, which shows that the micro-nanostructure sensor of the sandpaper template has good long-term stability.

[0177] The response range of the pressure sensor prepared based on the fiber membrane of Example 6 was measured. The test results are as follows: Figure 7 The test method is: set the tensile strain rate of the pressure sensor to 200%. Figure 7It is known that, under the condition of 200% tensile strain rate, although the resistance change rate is greatly increased, its response time is almost unchanged. In addition, the data obtained after the tensile test is as stable as the data obtained in the previous small strain range. This shows that the pressure sensor prepared in Example 6 has a large response range (15% < ε < 200%).

[0178] The above are only embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the contents of the present invention specification, or directly or indirectly applied in related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A fiber membrane, Features: The components of the fiber membrane include: Thermoplastic polyurethane; Conductive fillers; The fiber membrane is formed by replicating the porous micro-nano structure on the template onto the fiber membrane through electrostatic spinning technology, thereby forming a fiber membrane with a patterned structure.

2. A fiber membrane according to claim 1, Features: The conductive filler includes carbon nanotubes and graphene.

3. A fiber membrane according to claim 1, Features: The template includes a wire mesh and sandpaper.

4. A fiber membrane according to claim 3, Features: The steel wire mesh is a steel wire mesh of 100-500 meshes.

5. A fiber membrane according to claim 3, Features: The sandpaper is 120-320 grit sandpaper.

6. A method for preparing a fiber membrane as claimed in any one of claims 1 to 5, Features: The following steps are involved: S1 mixes thermoplastic polyurethane with a solvent to prepare a spinning solution; S2 uses the porous micro-nanostructure template as a pattern template on an electrospinning receiving device, and spins the spinning solution onto the template to obtain a spinning membrane; S3 prepares the conductive filler into a dispersion liquid, mixes the dispersion liquid with the spinning membrane, and obtains the fiber membrane through suction filtration.

7. The method according to claim 6, Features: In the spinning solution, the mass percentage of thermoplastic polyurethane is 25-30%.

8. The method according to claim 6, Features: When the porous micro-nano structure template is a steel wire mesh, the spinning parameters during the spinning process are:

9. The method according to claim 6, Features: When the porous micro-nano structure template is sandpaper, the spinning parameters during the spinning process are:

10. A flexible pressure sensor, Features: It comprises a fiber membrane as described in any one of claims 1 to 5.

Citation Information

Patent Citations

  • Force-sensitive stretchable electro-spinning patterning conductive nanofiber membrane and preparation method thereof

    CN104894750A

  • Preparation methods for composite nanofiber membrane and flexible strain sensor

    CN112900080A

  • Elastomer film with multistage microstructure, preparation method of elastomer film and flexible pressure sensor comprising elastomer film

    CN113503993A

  • A TPU flexible strain membrane, a flexible strain sensor and its fabrication method

    CN116804529A

  • Method for manufacturing artificial fur and apparatus for manufacturing artificial fur

    KR1020220017540A