Superfine fiber non-woven material as well as preparation method and application thereof
Through the composite spinning and water-bath fiber opening treatment of water-soluble thermoplastic polymer and water-soluble thermoplastic polymer, the fiber fineness and uniformity control problems in microfiber production are solved, and environmentally friendly and efficient microfiber nonwovens are achieved. Material preparation improves material performance and reduces the impact of the production environment.
Patent Information
- Application Number
- CN202411187499.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-12
AI Technical Summary
The existing microfiber production technology has shortcomings in fiber fineness and uniformity control, and the chemicals used in the production process are burdens to the environment and have high energy consumption.
The melt composite spinning is carried out using water-soluble thermoplastic polymer and water-soluble thermoplastic polymer. The initial fiber web is formed by cooling and drafting, and the mesh is laid and reinforced, and the microfiber nonwoven material is obtained through water bath fiber opening treatment to avoid using Harmful solvents, simplify processes and reduce energy consumption.
Without using harmful solvents, the environmental impact of producing microfiber materials is significantly reduced, the breathability, hygroscopy and filtration efficiency of the materials are improved, the production process is simplified, energy consumption and cost are reduced, and it is in line with green production needs. .
Smart Images

Figure CN118932607A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nonwoven material preparation, and in particular to an ultrafine fiber nonwoven material and a preparation method and application thereof. Background Art
[0002] Nonwoven materials are highly valued for their outstanding performance and wide range of applications, especially in industries such as filtration, medical protection, clothing and cleaning products. In these applications, microfiber nonwoven materials exhibit excellent performance such as high filtration efficiency, good liquid absorption and superior skin friendliness due to their high surface area and special physical structure.
[0003] However, although the existing technology can produce ultrafine fibers, there are still deficiencies in controlling the fineness and uniformity of the fibers, which directly affects the performance and application range of the final product. In addition, in the production process of some ultrafine fibers, such as sea-island type, chemical fiber opening is required to obtain ultrafine fibers, and the solvents or chemicals used may burden the environment; the high-pressure hydroentanglement fiber opening process of orange-peel type fibers consumes a lot of energy. In view of the above problems, it is of great significance to develop a new, environmentally friendly and efficient method for preparing ultrafine fiber nonwoven materials, simplify the preparation process, reduce energy consumption, and effectively control the fineness and uniformity of the fibers without using harmful chemicals. Summary of the invention
[0004] The purpose of the present invention is to overcome the problems existing in the prior art and to provide an ultrafine fiber nonwoven material and a preparation method and application thereof.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing an ultrafine fiber nonwoven material, comprising the following steps:
[0007] (1) melting a water-soluble thermoplastic polymer and a water-insoluble thermoplastic polymer independently to obtain a melt of the water-soluble thermoplastic polymer and a melt of the water-insoluble thermoplastic polymer; and spinning the melt of the water-soluble thermoplastic polymer and the melt of the water-insoluble thermoplastic polymer together to obtain a two-component raw silk melt;
[0008] (2) cooling and drawing the bicomponent raw silk melt in sequence, and laying out the initial fiber web after drawing;
[0009] (3) Laying the initial fiber web to obtain a processed fiber web;
[0010] (4) reinforcing the treated fiber web to obtain a nonwoven material;
[0011] (5) The nonwoven material is subjected to a water bath fiber opening treatment to obtain the ultrafine fiber nonwoven material.
[0012] Preferably, the water-soluble thermoplastic polymer in step (1) comprises one or more of modified polyvinyl alcohol compounds and modified polyester compounds;
[0013] The water-insoluble thermoplastic polymer includes one or more of polyethylene terephthalate compounds, polyamide compounds, polypropylene compounds, polylactic acid compounds and polystyrene compounds;
[0014] The difference in solubility between the water-soluble thermoplastic polymer and the water-insoluble thermoplastic polymer in water is ≥ 0.5;
[0015] The volume ratio of the melt of the water-soluble thermoplastic polymer to the melt of the water-insoluble thermoplastic polymer is 3-7:7-3.
[0016] Preferably, the cooling air temperature in step (2) is 15-28° C., the cooling wind speed is 0.2-1 m / s, and the cooling relative humidity is 10-30%;
[0017] The stretching device in step (2) is a tubular stretching device or a slit stretching device, the stretching wind pressure is 0.1-1 MPa, the stretching temperature is 10-30° C., and the relative humidity is 0-10%.
[0018] Preferably, the cross-sectional shape of the initial fiber web in step (2) is a pie-shaped, hollow pie-shaped, fixed island-shaped, irregular island-shaped, island-in-island-shaped or pie-shaped-island-shaped; the surface density of the fiber web is 50 to 150 g / m 2 .
[0019] Preferably, the web laying method in step (3) is parallel web laying and / or cross web laying.
[0020] Preferably, the surface density of the treated fiber web in step (3) is 100 to 1000 g / m 2 .
[0021] Preferably, the reinforcement method in step (4) is acupuncture and / or hydroentanglement; the acupuncture depth is 4 to 10 mm, and the acupuncture frequency is 400 to 1200 p / cm 2 ; The water spurt pressure is 5 to 20 MPa.
[0022] Preferably, the temperature of the water-soluble fiber-opening treatment in step (5) is 40 to 100° C., and the time of the water-soluble fiber-opening treatment is 10 to 120 min.
[0023] The surface density of the ultrafine fiber nonwoven material in step (5) is 50 to 800 g / m2 .
[0024] The invention also provides the ultra-fine fiber non-woven material prepared by the method for preparing the ultra-fine fiber non-woven material.
[0025] The present invention also provides application of the ultrafine fiber nonwoven material in the field of disposable sanitary products, medical protective products, filter materials or ultrafine leather products.
[0026] The beneficial effects of the present invention are:
[0027] The present invention provides a method for preparing a superfine fiber nonwoven material, comprising the following steps: melting a water-soluble thermoplastic polymer and a water-insoluble thermoplastic polymer independently to obtain respective melts; performing composite spinning on the melts to obtain a two-component primary silk melt; sequentially cooling and drawing the two-component primary silk melt, and laying out an initial fiber web after the drawing is completed; laying out the initial fiber web to obtain a treated fiber web; reinforcing the treated fiber web to obtain a nonwoven material; and performing water-soluble fiber opening treatment on the nonwoven material to obtain a superfine fiber nonwoven material. Among them, one component of the two polymers is a water-soluble thermoplastic polymer, and the other component is a water-insoluble thermoplastic polymer. The water-soluble polymer component can be dissolved by subsequent water bath heating to obtain a superfine fiber of the water-insoluble polymer component, thereby avoiding the use of organic solvents, being environmentally friendly and efficient, and being able to prepare superfine fiber nonwoven materials without using harmful solvents, significantly reducing the environmental impact of producing superfine fiber materials. In addition, the present invention also simplifies the production process, reduces energy consumption and costs. The present invention integrates environmentally friendly materials and advanced production technologies, which not only improves the performance of ultrafine fiber nonwoven materials, such as air permeability, moisture absorption and filtration efficiency, but also significantly reduces energy consumption and waste emissions in the production process, meeting the needs of green production and sustainable development. The prepared ultrafine fiber nonwoven materials can be used in disposable sanitary products, medical protective products, filtration materials or ultrafine leather products and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a schematic diagram of a device for preparing the ultrafine fiber nonwoven material of the present invention; Figure 1 In the figure, 1 is a hopper, 2 is a screw extruder, 3 is a metering pump, 4 is a two-component spinning assembly, 5 is a side-blowing cooling device, 6 is a drafting device, 7 is a web-forming curtain, 8 is a negative pressure suction device, 9 is an initial fiber web, 10 is a web laying device, 11 is a web fixing device, 12 is a nonwoven material, 13 is a tension roller, 14 is a water reduction tank, 15 is a guide roller, 16 is a cleaning tank, 17 is a drying box, 18 is an ultrafine fiber nonwoven material, and 19 is a winding device;
[0029] Figure 2This is a microscopic morphology of the TPVA / PA6-66 bicomponent orange segment fiber in Example 1;
[0030] Figure 3 Surface microscopic morphology of the nonwoven material in Example 1;
[0031] Figure 4 This is a surface microscopic morphology of the ultrafine fiber nonwoven material in Example 1;
[0032] Figure 5 It is a cross-sectional microscopic morphology image of the nonwoven material in Example 1;
[0033] Figure 6 This is a cross-sectional microscopic morphology of the ultrafine fiber nonwoven material in Example 1. DETAILED DESCRIPTION
[0034] The present invention provides a method for preparing an ultrafine fiber nonwoven material, comprising the following steps:
[0035] (1) melting a water-soluble thermoplastic polymer and a water-insoluble thermoplastic polymer independently to obtain a melt of the water-soluble thermoplastic polymer and a melt of the water-insoluble thermoplastic polymer; and spinning the melt of the water-soluble thermoplastic polymer and the melt of the water-insoluble thermoplastic polymer together to obtain a two-component raw silk melt;
[0036] (2) cooling and drawing the bicomponent raw silk melt in sequence, and laying out the initial fiber web after drawing;
[0037] (3) Laying the initial fiber web to obtain a processed fiber web;
[0038] (4) reinforcing the treated fiber web to obtain a nonwoven material;
[0039] (5) The nonwoven material is subjected to a water-soluble fiber-opening treatment to obtain the ultrafine fiber nonwoven material.
[0040] In the present invention, the water-soluble thermoplastic polymer in step (1) preferably includes one or more of modified polyvinyl alcohol compounds and modified polyester compounds; the modified polyvinyl alcohol compounds are preferably modified polyvinyl alcohol or a derivative of modified polyvinyl alcohol; the modified polyester compounds are preferably modified polyester or a derivative of modified polyester.
[0041] In the present invention, the water-insoluble thermoplastic polymer preferably includes one or more of polyethylene terephthalate compounds, polyamide compounds, polypropylene compounds, polylactic acid compounds and polystyrene compounds; the polyethylene terephthalate compounds are preferably polyethylene terephthalate or a derivative of polyethylene terephthalate; the polyamide compounds are preferably polyamide or a derivative of polyamide; the polypropylene compounds are preferably polypropylene or a derivative of polypropylene; the polylactic acid compounds are preferably polylactic acid or a derivative of polylactic acid; the polystyrene compounds are preferably polystyrene or a derivative of polystyrene.
[0042] In the present invention, in step (1), the difference in solubility in water between the water-soluble thermoplastic polymer and the water-insoluble thermoplastic polymer is preferably ≥ 0.5.
[0043] In the present invention, the types of the above derivatives are not specifically limited, as long as the water-insoluble thermoplastic polymer and the water-soluble thermoplastic polymer can be composite-spun.
[0044] In the present invention, the water-soluble thermoplastic polymer and the water-insoluble thermoplastic polymer in step (1) are preferably dried independently before melting. The purpose of the drying treatment is to remove moisture from the polymer to prevent hydrolysis during the melting process, while ensuring that the water content of the polymer meets the requirements of subsequent composite spinning. The drying treatment temperature is preferably 80-100°C, more preferably 85-95°C, and more preferably 90°C; the drying time is preferably 22-26h, more preferably 23-25h, and more preferably 24h.
[0045] In the present invention, during the composite spinning in step (1), the volume ratio of the melt of the water-soluble thermoplastic polymer to the melt of the water-insoluble thermoplastic polymer is preferably 3-7:7-3, more preferably 4-6:6-4, and even more preferably 5:5.
[0046] In the present invention, the cooling wind temperature in step (2) is preferably 15-28°C, more preferably 19-25°C, and more preferably 20-22°C; the cooling wind speed is preferably 0.2-1m / s, more preferably 0.3-0.8m / s, and more preferably 0.5-0.6m / s; the cooling relative humidity is preferably 10-30%, more preferably 15-20%, and more preferably 18%.
[0047] In the present invention, the cooling time of step (2) is determined according to conventional technical means in the art, and after cooling, the bicomponent raw silk melt forms a bicomponent fiber.
[0048] In the present invention, the stretching device in step (2) is a tubular stretching device or a slit stretching device, and the slit stretching device is preferably a wide slit stretching device or a narrow slit stretching device; the stretching wind pressure is preferably 0.1-1 MPa, more preferably 0.3-0.8 MPa, and more preferably 0.5-0.6 MPa; the stretching temperature is preferably 10-30°C, more preferably 15-25°C, and more preferably 20-22°C; the relative humidity of the stretching is preferably 0-10%, more preferably 2-8%, and more preferably 5-6%.
[0049] In the present invention, the cross-sectional shape of the initial fiber web in step (2) is preferably a segmented orange segment, a hollow segmented orange segment, a fixed island, an irregular island, an island-in-island, or a segmented orange segment-island-island type; the surface density of the initial fiber web is preferably 50 to 150 g / m 2 , more preferably 60 to 140 g / m 2 , more preferably 100 to 120 g / m 2 .
[0050] In the present invention, the web laying method in step (3) is preferably parallel web laying and / or cross web laying.
[0051] In the present invention, the surface density of the fiber web after the treatment in step (3) is preferably 100 to 1000 g / m 2 , more preferably 200 to 800 g / m 2 , more preferably 300 to 540 g / m 2 .
[0052] In the present invention, the reinforcement method in step (4) is preferably acupuncture and / or hydroentanglement, the depth of the acupuncture is preferably 4 to 10 mm, more preferably 5 to 9 mm, and more preferably 6 to 8 mm; the frequency of the acupuncture is preferably 400 to 1200 p / cm 2 , more preferably 600 to 1000 p / cm 2 , more preferably 700 to 900 p / cm 2 The water spunlace pressure is preferably 5-20 MPa, more preferably 7-15 MPa, and more preferably 10-12 MPa. Compared with conventional high-pressure water spunlace (>35 MPa), the water spunlace in the present invention significantly reduces the required energy consumption, and the reinforcement (needle punching and / or water spunlace) method is determined according to the needs using conventional technical means in the field, and the structural stability and strength of the material are increased by reinforcement.
[0053] In the present invention, the purpose of the water-soluble fiber opening treatment in step (5) is to dissolve the water-soluble polymer component, leaving the water-insoluble polymer component, forming ultrafine fibers, and obtaining an ultrafine fiber non-woven material; the temperature of the water-soluble fiber opening treatment is preferably 40 to 100°C, more preferably 50 to 90°C, and more preferably 60 to 80°C; the time of the water-soluble fiber opening treatment is preferably 10 to 120 min, more preferably 30 to 100 min, and more preferably 40 to 60 min.
[0054] In the present invention, after the water-soluble fiber opening treatment is completed, it is washed with water again to wash away the residual water-soluble polymer components, and finally dried to obtain an ultrafine fiber nonwoven material; the washing temperature is preferably 20-50°C, more preferably 30-40°C, and more preferably 35°C; the washing time is preferably 10-120min, more preferably 20-100min, and more preferably 30-80min; the drying temperature is preferably 50-120°C, more preferably 60-100°C, and more preferably 70-80°C.
[0055] In the present invention, the surface density of the ultrafine fiber nonwoven material in step (5) is preferably 50 to 800 g / m 2 , more preferably 200 to 600 g / m 2 , more preferably 300 to 500 g / m 2 .
[0056] The invention also provides the ultra-fine fiber non-woven material prepared by the method for preparing the ultra-fine fiber non-woven material.
[0057] The present invention also provides application of the ultrafine fiber nonwoven material in the field of disposable sanitary products, medical protective products, filter materials or ultrafine leather products.
[0058] In the present invention, disposable sanitary products preferably include facial masks or wiping materials, wiping materials preferably include dry wipes, disposable wet wipes or high-precision instrument wiping materials, and medical protective products preferably include medical protective clothing, medical masks, medical sheets or medical surgical gowns.
[0059] In the present invention, a schematic diagram of a preparation device for ultrafine fiber nonwoven material is shown as follows: Figure 1 As shown, Figure 1 In the figure, 1 is a hopper, 2 is a screw extruder, 3 is a metering pump, 4 is a two-component spinning assembly, 5 is a side-blowing cooling device, 6 is a drawing device, 7 is a web-forming curtain, 8 is a negative pressure suction device, 9 is an initial fiber web, 10 is a web-laying device, 11 is a web-fixing device, 12 is a nonwoven material, 13 is a tension roller, 14 is a water reduction tank, 15 is a guide roller, 16 is a cleaning tank, 17 is a drying box, 18 is an ultrafine fiber nonwoven material, and 19 is a winding device.
[0060] In the present invention, the web laying device preferably includes a parallel web laying machine and / or a cross web laying machine.
[0061] In the present invention, the water-soluble thermoplastic polymer and the water-insoluble thermoplastic polymer are dried independently, and then fed into respective screw extruders 2 through respective hoppers 1 for melting to obtain respective melts; then, impurities are filtered out through respective melt filtration systems, and after being metered by respective metering pumps 3, they are fed into a two-component spinning assembly 4 for composite spinning, and extruded from the spinneret holes in the spinneret of the two-component spinning assembly 4 in a regularly alternating arrangement to obtain a two-component raw silk melt; cooled by a side-blowing cooling device 5, and stretched by a stretching device 6 After that, it is laid on the mesh curtain 7 through the negative pressure suction device 8 to form an initial fiber web 9; the initial fiber web 9 is laid and formed through the mesh laying device 10 and then sent to the mesh fixing device 11 for reinforcement to obtain a non-woven material 12; the non-woven material 12 is placed in the water reduction tank 14 through the tension roller 13 for water-soluble fiber opening treatment, and the time of the water-soluble fiber opening treatment is controlled by the number of guide rollers 15, and then placed in the cleaning tank 16 for cleaning, and finally placed in the drying box 17 for drying to obtain an ultrafine fiber non-woven material 18, and finally wound up through the winding device 19.
[0062] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0063] Example 1
[0064] Modified polyvinyl alcohol (TPVA) slices and polyamide (PA6-66) slices were dried independently in a drying tower at 90°C for 24 hours, wherein TPVA had a weight average molecular weight of 6600, a degree of alcoholysis of 88%, a degree of polymerization of 500, and a melt flow index of 45 g / 10 min, and was prepared according to patent CN116876153A. PA6-66 had an intrinsic viscosity of 2.350 dL / g and was purchased from Shanghai Huafeng Group; the dried TPVA and PA6-66 were independently fed into a screw extruder through a hopper to be melted to obtain TPVA melt and PA6-66 melt; the TPVA melt and the PA6-66 melt (the volume ratio of the TPVA melt to the PA6-66 melt was 7:3) were melted through their respective melts. The impurities are filtered by the filtering system, and after being metered by respective metering pumps, the fibers are fed into a segmented (16+16) bicomponent spinning assembly for spinning, and are extruded from the spinneret holes in a regular alternating arrangement in the spinneret of the bicomponent spinning assembly to obtain segmented bicomponent raw silk melt; the fibers are cooled by a side-blowing cooling device (the wind temperature is set to 25° C., the wind speed is 1 m / s, and the relative humidity is 20%) to obtain TPVA / PA6-66 bicomponent segmented fibers, and then stretched by a narrow slit stretching device (the stretching wind pressure is set to 0.5 MPa, the temperature is 20° C., and the relative humidity is 5%). After the stretching, the fibers are laid on a mesh curtain by a negative pressure suction device to form a TPVA / PA6-66 bicomponent segmented initial fiber web, and the surface density of the initial fiber web is 140 g / m 2 The TPVA / PA6-66 two-component orange-segment initial fiber web was laid by a web laying device (parallel web laying machine) to obtain a treated fiber web, and the surface density of the treated fiber web was 300g / m 2 , sent to the fixing net device for needle punching and reinforcement into nonwoven material, wherein the needle punching depth is 9mm and the needle punching frequency is 700p / cm 2 ; The nonwoven material is placed in a water reduction tank through a tension roller for water-soluble fiber opening treatment, and the temperature of the water-soluble fiber opening treatment is set to 80°C, and the time is 60 minutes (the time of the water-soluble fiber opening treatment is controlled by the number of guide rollers); after the water-soluble fiber opening treatment is completed, it is placed in a cleaning tank for cleaning, and the cleaning temperature is set to 50°C and the time is 30 minutes; finally, it is placed in a drying device for drying, and the drying temperature is set to 120°C to obtain a PA6-66 ultrafine fiber nonwoven material, and finally it is wound up by a winding device.
[0065] The microscopic morphology of the TPVA / PA6-66 two-component orange peel fiber in this embodiment is as follows: Figure 2 As shown; the surface microscopic morphology of the nonwoven material in this embodiment, as shown Figure 3 As shown; the surface microscopic morphology of the ultrafine fiber nonwoven material in this embodiment, as shown Figure 4 As shown; the cross-sectional microscopic morphology of the nonwoven material in this embodiment, as shown Figure 5 As shown; the cross-sectional microscopic morphology of the ultrafine fiber nonwoven material in this embodiment, as shown Figure 6 shown; from Figures 2 to 6 It can be seen that the orange-peel type composite fiber (16+16) has a clear primary fiber cross-section. After needle punching, the composite fibers are entangled together. The average diameter of the composite fibers is 23μm. After water-soluble fiber opening, the composite fibers are completely split to form ultrafine fibers. The average equivalent diameter of the ultrafine fibers is about 2.5μm.
[0066] Example 2
[0067] Modified polyester (WSPET) chips and polyamide (PA6) chips were dried independently in a drying tower at 90°C for 24 hours, wherein the intrinsic viscosity of WSPET was 0.680 dL / g and was prepared according to patent CN113929889B, and the intrinsic viscosity of PA6 was 2.460 dL / g and was purchased from Hunan Yuehua Chemical Co., Ltd.; the dried WSPET and PA6 were fed independently into a screw extruder through a hopper to melt to obtain WSPET melt and PA6 melt; the WSPET melt and the PA6 melt (the volume ratio of the WSPET melt to the PA6 melt was 5:5) were filtered for impurities by their respective melt filtration systems, and the impurities were removed by their respective metering pumps. After metering, the fiber is fed into a sea-island type (37 islands) bicomponent spinning assembly for spinning, and extruded from the spinneret holes in the spinneret of the bicomponent spinning assembly in a regular alternating arrangement to obtain a sea-island type bicomponent raw silk melt; it is cooled by a side-blowing cooling device (the wind temperature is set to 22°C, the wind speed is 0.5m / s, and the relative humidity is 10%) to obtain WSPET / PA6 bicomponent sea-island fibers, and then stretched by a tubular stretching device (the stretching wind pressure is set to 0.5MPa, the temperature is 22°C, and the relative humidity is 5%). After the stretching, it is laid on a mesh curtain by a negative pressure suction device to form a WSPET / PA6 bicomponent sea-island type initial fiber web, and the surface density of the initial fiber web is 50g / m 2 The WSPET / PA6 two-component island-in-sea type initial fiber web was laid by a web laying device (cross-lapping machine) to obtain a treated fiber web, and the surface density of the treated fiber web was 200g / m 2 , sent to the fixed network device for water spunlace reinforcement into a non-woven material, wherein the water spunlace pressure is 10Mpa; the non-woven material is placed in a water reduction tank through a tension roller for water-soluble fiber opening treatment, and the temperature of the water-soluble fiber opening treatment is set to 90°C, and the time is 40min (the time of the water-soluble fiber opening treatment is controlled by the number of guide rollers); after the water-soluble fiber opening treatment is completed, it is placed in a cleaning tank for cleaning, and the cleaning temperature is set to 50°C, and the time is 30min; finally, it enters the drying device for drying, and the drying temperature is set to 120°C to obtain a PA6 ultrafine fiber non-woven material, and finally it is wound up by a winding device.
[0068] Example 3
[0069] Modified polyvinyl alcohol (TPVA) slices and polylactic acid (PLA) slices were dried independently in a drying tower at 90°C for 24h, wherein TPVA had a weight average molecular weight of 7000, a degree of alcoholysis of 98%, a degree of polymerization of 600, and a melt flow index of 50g / 10min, and was prepared according to patent CN116876153A; PLA had a melting temperature of 165°C and was purchased from Zhuhai Jinfa Biomaterials Co., Ltd.; the dried TPVA and PLA were independently fed into a screw extruder through a hopper to be melted to obtain a TPVA melt and a PLA melt; the TPVA melt and the PLA melt (the volume ratio of the TPVA melt to the PLA melt was 3:7) were filtered for impurities through their respective melt filtration systems, and then After being metered by respective metering pumps, the fibers are fed into a hollow segment-shaped (8+8) bicomponent spinning assembly for spinning, and are extruded from the spinneret holes in a regularly alternating arrangement in the spinneret of the bicomponent spinning assembly to obtain a hollow segment-shaped bicomponent raw silk melt; the fibers are cooled by a side-blowing cooling device (the wind temperature is set to 20° C., the wind speed is set to 0.6 m / s, and the relative humidity is set to 10%) to obtain TPVA / PLA bicomponent hollow segment-shaped fibers, and then stretched by a narrow slit stretching device (the stretching wind pressure is set to 0.6 MPa, the temperature is set to 20° C., and the relative humidity is set to 5%). After the stretching, the fibers are laid on a mesh curtain by a negative pressure suction device to form a TPVA / PLA bicomponent hollow segment-shaped initial fiber web, and the surface density of the initial fiber web is 50 g / m 2 The TPVA / PLA two-component hollow orange-segment initial fiber web was laid by a web laying device (cross-lapping machine) to obtain a treated fiber web, and the surface density of the treated fiber web was 300g / m 2 , sent to the fixing net device for needle punching and reinforcement into nonwoven material, wherein the needle punching depth is 6mm and the needle punching frequency is 1000p / cm 2 ; The nonwoven material is placed in a water reduction tank through a tension roller for water-soluble fiber opening treatment, and the temperature of the water-soluble fiber opening treatment is set to 80°C, and the time is 30 minutes (the time of the water-soluble fiber opening treatment is controlled by the number of guide rollers); after the water-soluble fiber opening treatment is completed, it is placed in a cleaning tank for cleaning, and the cleaning temperature is set to 40°C and the time is 20 minutes; finally, it is placed in a drying device for drying, and the drying temperature is set to 100°C to obtain a PLA ultrafine fiber nonwoven material, and finally it is wound up by a winding device.
[0070] Example 4
[0071] Modified polyvinyl alcohol (TPVA) slices and polyamide (PA6) slices were dried independently in a drying tower at 90°C for 24 hours, wherein TPVA had a weight average molecular weight of 6800, a degree of alcoholysis of 96%, a degree of polymerization of 560, and a melt flow index of 46 g / 10 min, and was prepared according to patent CN116876153A; PA6 had an intrinsic viscosity of 2.460 dL / g and was purchased from Hunan Yuehua Chemical Co., Ltd.; the dried TPVA and PA6 were independently fed into a screw extruder through a hopper to be melted to obtain TPVA melt and PA6 melt; the TPVA melt and the PA6 melt (the volume ratio of the TPVA melt to the PA6 melt was 4:6) were filtered for impurities through their respective melt filtration systems After being metered by respective metering pumps, the fibers are fed into a hollow orange segment type (16+16) bicomponent spinning assembly for spinning, and are extruded from the spinneret holes in a regular alternating arrangement in the spinneret of the bicomponent spinning assembly to obtain a hollow orange segment type bicomponent raw silk melt; after being cooled by a side-blowing cooling device (the wind temperature is set to 22°C, the wind speed is set to 0.8m / s, and the relative humidity is set to 15%), TPVA / PA6 bicomponent hollow orange segment fibers are obtained, and then drawn by a narrow slit drawing device (the drawing wind pressure is set to 0.8MPa, the temperature is set to 22°C, and the relative humidity is set to 5%). After the drawing is completed, the fibers are laid on a mesh curtain by a negative pressure suction device to form a TPVA / PA6 bicomponent hollow orange segment type initial fiber web, and the surface density of the initial fiber web is 60g / m 2 The TPVA / PA6 two-component hollow orange-segment initial fiber web was laid by a web laying device (cross-lapping machine) to obtain a treated fiber web, and the surface density of the treated fiber web was 540g / m 2 , sent to the fixing net device for needle punching and hydroentanglement in sequence to reinforce the nonwoven material, wherein the needle punching depth is 10mm and the needle punching frequency is 1200p / cm 2 , the water spunlace pressure is 15MPa; the non-woven material is placed in a water reduction tank through a tension roller for water-soluble fiber opening treatment, and the temperature of the water-soluble fiber opening treatment is set to 90°C, and the time is 60min (the time of the water-soluble fiber opening treatment is controlled by the number of guide rollers); after the water-soluble fiber opening treatment is completed, it is placed in a cleaning tank for cleaning, and the cleaning temperature is set to 50°C, and the time is 30min; finally, it enters the drying device for drying, and the drying temperature is set to 120°C to obtain a PA6 ultrafine fiber non-woven material, and finally it is wound up by a winding device.
[0072] The properties of the materials before and after the water-soluble fiber opening treatment in Examples 1 to 4, that is, the properties of the nonwoven material and the ultrafine fiber nonwoven material, were tested, and the performance test results of the nonwoven material and the ultrafine fiber nonwoven material in Examples 1 to 4 were obtained, as shown in Table 1.
[0073] Table 1 Performance test results of nonwoven materials and ultrafine fiber nonwoven materials in Examples 1 to 4
[0074]
[0075]
[0076] As can be seen from the above embodiments, the present invention provides a method for preparing an ultrafine fiber nonwoven material, comprising the following steps: melting a water-soluble thermoplastic polymer and a water-insoluble thermoplastic polymer independently to obtain respective melts; performing composite spinning on the melts to obtain a two-component primary silk melt; sequentially cooling and drawing the two-component primary silk melt, and laying out the initial fiber web after the drawing is completed; laying out the initial fiber web to obtain a treated fiber web; reinforcing the treated fiber web to obtain a nonwoven material; and performing water-soluble fiber opening treatment on the nonwoven material to obtain an ultrafine fiber nonwoven material. Among them, one component of the two polymers is a water-soluble thermoplastic polymer, and the other component is a water-insoluble thermoplastic polymer. The water-soluble polymer component can be dissolved by subsequent water bath heating to obtain an ultrafine fiber of the water-insoluble polymer component, thereby avoiding the use of organic solvents, being environmentally friendly and efficient, and being able to prepare ultrafine fiber nonwoven materials without using harmful solvents, significantly reducing the environmental impact of producing ultrafine fiber materials. In addition, the present invention also simplifies the production process, reduces energy consumption and costs. The present invention integrates environmentally friendly materials and advanced production technologies, which not only improves the performance of ultrafine fiber nonwoven materials, such as air permeability, moisture absorption and filtration efficiency, but also significantly reduces energy consumption and waste emissions in the production process, meeting the needs of green production and sustainable development. The prepared ultrafine fiber nonwoven materials can be used in disposable sanitary products, medical protective products, filtration materials or ultrafine leather products and other fields.
[0077] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a superfine fiber nonwoven material, characterized in that: It includes the following steps: (1) melting a water-soluble thermoplastic polymer and a water-insoluble thermoplastic polymer independently to obtain a melt of the water-soluble thermoplastic polymer and a melt of the water-insoluble thermoplastic polymer; and spinning the melt of the water-soluble thermoplastic polymer and the melt of the water-insoluble thermoplastic polymer together to obtain a two-component raw silk melt; (2) cooling and drawing the bicomponent raw silk melt in sequence, and laying out the initial fiber web after drawing; (3) Laying the initial fiber web to obtain a processed fiber web; (4) reinforcing the treated fiber web to obtain a nonwoven material; (5) The nonwoven material is subjected to a water-soluble fiber-opening treatment to obtain the ultrafine fiber nonwoven material.
2. The method for preparing the ultrafine fiber nonwoven material according to claim 1, characterized in that: The water-soluble thermoplastic polymer in step (1) includes one or more of modified polyvinyl alcohol compounds and modified polyester compounds; The water-insoluble thermoplastic polymer includes one or more of polyethylene terephthalate compounds, polyamide compounds, polypropylene compounds, polylactic acid compounds and polystyrene compounds; The difference in solubility between the water-soluble thermoplastic polymer and the water-insoluble thermoplastic polymer in water is ≥ 0.5; The volume ratio of the melt of the water-soluble thermoplastic polymer to the melt of the water-insoluble thermoplastic polymer is 3-7:7-3.
3. The method for preparing the ultrafine fiber nonwoven material according to claim 1 or 2, characterized in that: The cooling air temperature of step (2) is 15-28° C., the cooling wind speed is 0.2-1 m / s, and the cooling relative humidity is 10-30%; The stretching device in step (2) is a tubular stretching device or a slit stretching device, the stretching wind pressure is 0.1-1 MPa, the stretching temperature is 10-30° C., and the relative humidity is 0-10%.
4. The method for preparing the ultrafine fiber nonwoven material according to claim 3, characterized in that: The cross-sectional shape of the initial fiber web in step (2) is orange segment type, hollow orange segment type, fixed island type, irregular island type, island-in-island type or orange segment-island type; the surface density of the initial fiber web is 50 to 150 g / m 2 .
5. The method for preparing the ultrafine fiber nonwoven material according to claim 4, characterized in that: The web laying method in step (3) is parallel web laying and / or cross web laying.
6. The method for preparing the ultrafine fiber nonwoven material according to claim 5, characterized in that: The surface density of the treated fiber web in step (3) is 100 to 1000 g / m 2 .
7. The method for preparing the ultrafine fiber nonwoven material according to claim 6, characterized in that: The reinforcement method in step (4) is acupuncture and / or hydroentanglement; the depth of acupuncture is 4 to 10 mm, and the frequency of acupuncture is 400 to 1200 p / cm 2 ; The water spurt pressure is 5 to 20 MPa.
8. The method for preparing the ultrafine fiber nonwoven material according to claim 7, characterized in that: The temperature of the water-soluble fiber-opening treatment in step (5) is 40 to 100° C., and the time of the water-soluble fiber-opening treatment is 10 to 120 minutes; The surface density of the ultrafine fiber nonwoven material in step (5) is 50 to 800 g / m 2 .
9. The ultrafine fiber nonwoven material prepared by the method for preparing an ultrafine fiber nonwoven material according to any one of claims 1 to 8.
10. Use of the ultrafine fiber nonwoven material according to claim 9 in the field of disposable sanitary products, medical protective products, filter materials or ultrafine leather products.
Citation Information
Patent Citations
Orange petal type superfine fiber simulation leather base cloth preparation method
CN106521956A
Preparation method of degradable superfine mask base cloth
CN113279145A
Orange segment type spunbonded spunlaced superfine fiber non-woven filtering material based on water-soluble splitting and preparation method and application of orange segment type spunbonded spunlaced superfine fiber non-woven filtering material
CN116876153A
Method for manufacturing ultrafine fiber nonwoven fabric or leather-like sheet base material
JP2013072166A
Method for producing light weight ultrafine fiber fabric
US20040070101A1
Cited By
Abrasion-resistant, breathable, soft, and skin-friendly nonwoven material and method for making the same
CN122980116A