Durable anti-ultraviolet active printed real silk fabric and dyeing and finishing process thereof

By using a composite treatment of whitening agent and crosslinking agent in silk fabrics, the problem of affecting dyeing performance and washing resistance of silk fabrics is solved by combining the combination of whitening agent and crosslinking agent in silk fabrics, and the anti-ultraviolet function is sorted out after active printing. , achieving efficient UV resistance and durability.

CN118932694APending Publication Date: 2024-11-12ZHEJIANG SILK TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411199977.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, silk fabrics will affect the dyeing performance, feel and wash resistance of the fabric when they are resistant to UV treatment, and the UV-resistant effect is difficult to last.

Method used

Combined treatment of whitening agent and crosslinking agent is adopted to form a wash-resistant whitening anti-UV layer, and the anti-UV function is sorted after active printing to improve the UV resistance of silk fabrics and ensure that the fabric still meets the conditions after multiple washes. UV-resistant fabric indicators.

Benefits of technology

It significantly improves the UV resistance coefficient of silk fabrics, with UPF up to 50+, and maintains the fabric's wash resistance and dyeing performance, ensuring the durability of UV resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005017598380000091
    Figure BDA0005017598380000091
Patent Text Reader

Abstract

The invention discloses a durable anti-ultraviolet reactive printed real silk fabric and a dyeing and finishing process thereof, the real silk fabric is soaked in a pretreatment solution before dyeing, a washable whitening anti-ultraviolet layer is formed on the surface of the real silk fabric, the real silk fabric is subjected to dyeing and reactive printing, then the real silk fabric is subjected to padding / dip dyeing to an anti-ultraviolet functional finishing solution, and a reinforced anti-ultraviolet layer is formed on the surface of the real silk fabric; the pretreatment liquid comprises a whitening agent and a cross-linking agent. The whitening agent and the cross-linking agent are compounded to achieve a synergistic effect, whitening and cross-linking pretreatment is performed on the real silk fabric, so that the whitening agent is permanently attached to the surface of the real silk fabric, the washing resistance of the whitening agent is improved, the white ground part of the real silk fabric has washing resistance and ultraviolet resistance, and after-finishing is performed by compounding the ultraviolet resistance function, the whitening agent and the cross-linking agent have good anti-ultraviolet performance. According to the method, the semi-finished real silk fabric subjected to reactive printing is subjected to anti-ultraviolet functional after-finishing treatment, so that the anti-ultraviolet coefficient of the real silk fabric is greatly improved, the UPF can be up to 50 +, and the real silk fabric still meets the index requirements of the anti-ultraviolet fabric after being washed for multiple times.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of textiles, and in particular to a durable anti-ultraviolet active printed silk fabric and a dyeing and finishing process thereof. Background Art

[0002] Sunlight is composed of ultraviolet rays, infrared rays and visible light. Visible light is the part of the electromagnetic spectrum that can be sensed by the human eye. In the solar spectrum, ultraviolet rays account for 6.1%, visible light accounts for 51.8%, and infrared rays account for 42.1%. Ultraviolet rays are generally divided into three sections: UVA with a wavelength range of 320nm to 400nm; UVB with a wavelength range of 290nm to 320nm; and UVC with a wavelength range less than 290nm.

[0003] Ultraviolet radiation has a dual nature to the human body. When the human body receives an appropriate amount of ultraviolet radiation, it can keep the sympathetic nerve and adrenal system in the body in a proper tension, promote the secretion of multiple hormones, and prevent pediatric schwannosis and adult rickets. However, excessive ultraviolet radiation will induce sun spots and skin cancer, stimulate pigment production, cause skin aging, and cause cataracts and immune system diseases. The ultraviolet UVB band is the band that causes skin diseases, and it is also the main band for the formation of sun spots and irritation, and it is the most harmful to the human body. The UVA band itself only induces a slight photobiological effect, but it can enhance the effect produced by the UVB band.

[0004] In order to prevent the harm of ultraviolet rays in the sun, people apply sunscreen on their skin, use parasols, and wear clothes with anti-ultraviolet function. When ultraviolet rays are irradiated to fabrics or clothing, they are absorbed, reflected and projected, and the transmitted light is radiated to the human skin. Except for a small part of diffuse radiation, most of the radiation light is direct radiation. The more light that passes through, the greater the harm to the human body. From the perspective of protecting the human body, the dose of ultraviolet radiation that passes through fabrics should be reduced as much as possible.

[0005] Real silk refers to silk made from real silk, which is a general term for silk processed from silk. The surface of silk is smooth, fine and clean, with a soft luster and bright and pure colors; it feels smooth, soft and has a light and elegant appearance. Real silk is both a biological polymer material and a noble textile material, known as the "Queen of Fibers". Real silk has the effect of skin care and beauty, and can protect human skin from the harm of ultraviolet rays.

[0006] In 1986, Jingdong Agricultural and Industrial University studied the use of grafted silk and ultraviolet absorbers. Various ultraviolet absorbers had obvious effects, especially water-soluble ultraviolet absorbers, but the washing resistance of the treated fabrics was poor. In 1997, Zhang Hanmin of Wuhan Textile Institute and Feng Yunfang of Zhejiang Silk Institute independently developed ultraviolet absorber F, which had a certain effect and had little effect on the strength and moisture absorption of the fabric, but had a greater impact on the dyeing performance of the fabric.

[0007] Therefore, it is urgent to develop a durable anti-ultraviolet reactive printed silk fabric and a dyeing and finishing process suitable for the silk fabric. Summary of the invention

[0008] The purpose of the present invention is to provide a durable anti-ultraviolet reactive printed silk fabric and its dyeing and finishing process, which solves the problems in the prior art that anti-ultraviolet treatment of silk fabric will affect the dyeing performance, feel, etc. of the fabric, and the treated fabric has poor wash resistance and the anti-ultraviolet effect is difficult to last. The durable anti-ultraviolet reactive printed silk fabric prepared in the present invention achieves durable whiteness and anti-ultraviolet performance, and the anti-ultraviolet coefficient of the silk fabric is greatly improved, the UPF can be as high as 50+, and it still meets the anti-ultraviolet fabric index requirements after multiple washings.

[0009] In order to achieve the above object, the present invention adopts the following technical solutions:

[0010] In a first aspect of the present invention, there is provided a durable anti-ultraviolet reactive printed silk fabric, wherein the silk fabric is immersed in a pretreatment liquid before dyeing to form a washable whitening anti-ultraviolet layer on its surface, and after dyeing and reactive printing, the silk fabric is then padded / dipped into an anti-ultraviolet functional finishing liquid to form a reinforced anti-ultraviolet layer on its surface;

[0011] The pre-treatment liquid includes a brightener and a cross-linking agent.

[0012] Using the above technical solution:

[0013] Conventional reactive printed fabric anti-ultraviolet treatment only involves padding / dyeing the printed fabric into an anti-ultraviolet functional finishing liquid to give the fabric anti-ultraviolet function. The white base of the fabric has extremely poor anti-ultraviolet protection and cannot meet the standard requirements for anti-ultraviolet fabrics. Even if the white base of the fabric is treated with anti-ultraviolet treatment in advance before reactive digital printing, the conventional pre-treatment whitening or anti-ultraviolet functional treatment will be completely washed away during the soaping process, resulting in the white base of the fabric still not meeting the standard requirements for anti-ultraviolet fabrics even after anti-ultraviolet finishing, since the reactive printing process includes sizing, steaming, soaping and other steps.

[0014] Before dyeing and reactive printing of silk fabrics, the fabrics are treated with a whitening agent to improve the UV protection performance of the fabrics. However, in the soaping step of reactive printing, the whitening agent attached to the fabric surface is easily washed off. In the present application, the whitening agent and the cross-linking agent are creatively compounded, and the two play a synergistic role. By performing a whitening and cross-linking pre-treatment on the silk fabric, the whitening agent is permanently attached to the surface of the silk fabric, and the washing resistance of the whitening agent is improved. The white base part of the silk fabric has washable and UV-resistant performance, and a composite anti-ultraviolet functional finishing is performed, that is, the semi-finished silk fabric after reactive printing is subjected to an anti-ultraviolet functional finishing treatment, which greatly improves the anti-ultraviolet coefficient of the silk fabric, and the UPF can be as high as 50+, and it still meets the anti-ultraviolet fabric index requirements after multiple washings.

[0015] Furthermore, the weight ratio of the whitening agent to the silk fabric is 1-5%, and the weight ratio of the cross-linking agent to the silk fabric is 5-10%.

[0016] The whitening agent and the cross-linking agent are used in the above-mentioned specific dosage ratio to pre-treat the silk fabric, which can achieve the durable anti-ultraviolet performance of the silk fabric, and the feel of the fabric before and after the treatment changes little, and will not affect the subsequent dyeing performance of the fabric.

[0017] Furthermore, the cross-linking agent is aziridine or blocked isocyanate.

[0018] On the one hand, the two cross-linking agents, aziridine and blocked isocyanate, can synergize well with the whitening agent to attach it stably to the surface of silk fabric for a long time, and can effectively cross-link at low temperatures without affecting the whiteness and feel of the silk fabric.

[0019] Furthermore, the brightener is a distyrylbiphenyl compound derivative or a distyrylsulfonic acid derivative.

[0020] Specifically, the whitening agent is one or both of UVITEX BLH and UVITEX MST.

[0021] Furthermore, the anti-ultraviolet functional finishing liquid includes an anti-ultraviolet finishing agent, and the anti-ultraviolet finishing agent is a triazine derivative. Specifically, the anti-ultraviolet agent is one or more of 6160 of Chuanhua, UVR of Rudolf, and HTUV100 of Hurt.

[0022] The second aspect of the present invention provides a durable anti-ultraviolet dyeing and finishing process for reactive printed silk fabrics, comprising the following steps:

[0023] S1, immersing the silk fabric in a pretreatment solution at a temperature of 30 to 80° C. for a treatment time of 20 to 80 min, to form a washable whitening and anti-ultraviolet layer on the surface thereof, wherein the pretreatment solution comprises a whitening agent and a cross-linking agent;

[0024] S2, the treated silk fabric is dyed and then subjected to reactive printing;

[0025] S3, then padding / dyeing the semi-finished silk printed fabric into the anti-ultraviolet functional finishing liquid to form a reinforced anti-ultraviolet layer on its surface.

[0026] By adopting the dyeing and finishing process, during the pre-treatment of silk fabric, a whitening agent and a cross-linking agent are used for whitening and anti-ultraviolet finishing. The treatment time is relatively long, so that the white base part of the silk fabric has excellent wash-resistant and anti-ultraviolet performance. Even after digital sizing, steaming, soaping and other processes, its anti-ultraviolet performance can still meet the requirements. Then, the semi-finished silk fabric after reactive printing is subjected to anti-ultraviolet functional post-finishing treatment, which greatly improves the anti-ultraviolet coefficient of the silk fabric. The UPF can be as high as 50+, and it still meets the anti-ultraviolet fabric index requirements after multiple washings.

[0027] Furthermore, the cross-linking agent is aziridine or blocked isocyanate, and the brightener is a distyryl biphenyl compound derivative or a distyryl sulfonic acid derivative.

[0028] Furthermore, the weight ratio of the whitening agent to the silk fabric is 1-5%, and the weight ratio of the cross-linking agent to the silk fabric is 5-10%.

[0029] Furthermore, the anti-ultraviolet functional finishing liquid includes an anti-ultraviolet finishing agent, and the anti-ultraviolet finishing agent is a triazine derivative.

[0030] Furthermore, in the step S3, during the anti-ultraviolet functional finishing process, the treatment temperature is 110-150° C., and the treatment time is 30-150 seconds.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] The present invention creatively combines a brightener and a cross-linking agent, and the two play a synergistic role. By performing a whitening and cross-linking pre-treatment on the silk fabric, the brightener is permanently attached to the surface of the silk fabric, thereby improving the wash resistance of the brightener. The white base part of the silk fabric has wash resistance and UV resistance. In addition, a composite anti-ultraviolet functional post-finishing is performed, that is, the semi-finished silk fabric after reactive printing is subjected to an anti-ultraviolet functional post-finishing treatment, thereby greatly improving the anti-ultraviolet coefficient of the silk fabric, and the UPF can be as high as 50+. After multiple washings, the anti-ultraviolet fabric index requirements are still met. DETAILED DESCRIPTION

[0033] The technical solutions in the present invention will be described clearly and completely below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] The present invention is further described below by way of examples. Unless otherwise specified, the various reagents and raw materials used in the present invention are all commercially available products or products that can be prepared by known methods.

[0035] Example 1

[0036] Fabric: 11185 silk electrospun, whitening base reactive printed fabric (weight 65g / m 2 )

[0037] 1) Preparation: Weigh the fabric, roll up the fabric into the dyeing machine, and then add water to the dyeing machine, with a bath ratio of about 1:10. Let the water circulate for 5 minutes at room temperature. Weigh the auxiliary agent, the weight of the aziridine crosslinking agent is 5% of the weight of the fabric, and the weight of the brightener (UVITEX BLH) is 2% of the weight of the fabric, dissolve and stir evenly, add to the dyeing tank, and run for 10 minutes at room temperature;

[0038] 2) Raising the temperature of the pretreatment solution from room temperature to 50°C at a heating rate of 2°C / min, keeping the temperature for 30 minutes, performing pretreatment whitening and dyeing, and then draining the water;

[0039] 3) Add water into the dyeing machine with a bath ratio of about 1:10, wash the fabric for 10 minutes, and drain;

[0040] 4) After the dyeing process is completed, the fabric is taken out from the dyeing machine and dried in a tentering setting machine at 130°C for 1 minute.

[0041] 5) After the fabric is arranged on a tenter machine for dipping and sizing, it is digitally printed and then steamed (steamed at 105°C for 20 minutes). The steamed fabric is soaped at 95°C for 10 minutes. The washed fabric is dried at 130°C on a tenter setting machine for 1 minute.

[0042] 6) Finally, the semi-finished silk reactive printing product is dipped in an anti-ultraviolet functional finishing agent in a stenter setting machine. The concentration of the anti-ultraviolet finishing agent (Chuanhua 6160) in the finishing liquid is 10g / L, and the product is dried at 130°C for 1min.

[0043] Example 2

[0044] Fabric: 11185 silk electrospun, whitening base reactive printed fabric (weight 65g / m 2 )

[0045] 1) Ingredients: Weigh the fabric, roll up the fabric warp beam and put it into the dyeing machine, then fill the warp beam dyeing machine with water, with a bath ratio of about 1:10, let the water circulate for 5 minutes at room temperature, weigh the auxiliaries, the weight of the aziridine crosslinking agent is 10% of the weight of the fabric, and the weight of the brightener (UVITEX BLH) is 5% of the weight of the fabric, dissolve and stir evenly, add to the dyeing vat, and run at room temperature for 10 minutes;

[0046] 2) Raising the temperature of the pretreatment solution from room temperature to 50°C at a heating rate of 2°C / min, keeping the temperature for 30 minutes, performing pretreatment whitening and dyeing, and then draining the water;

[0047] 3) Add water into the dyeing machine with a bath ratio of about 1:10, wash the fabric for 10 minutes, and drain;

[0048] 4) After the dyeing process is completed, the fabric is taken out from the dyeing machine and dried in a tentering setting machine at 130°C for 1 minute.

[0049] 5) After the fabric is arranged on a tenter machine for dipping and sizing, it is digitally printed and then steamed (steamed at 105°C for 20 minutes). The steamed fabric is soaped at 95°C for 10 minutes. The washed fabric is dried at 130°C on a tenter setting machine for 1 minute.

[0050] 6) The reactive printed semi-finished silk fabric is dipped into an anti-ultraviolet functional finishing liquid for post-finishing, the concentration of the anti-ultraviolet finishing agent (6160 of Chuanhua) in the anti-ultraviolet functional finishing liquid is 10 g / L, and the fabric is dried at 130° C. for 1 min.

[0051] Example 3

[0052] Fabric: 11185 silk electrospun, whitening base reactive printed fabric (weight 65g / m 2 )

[0053] 1) Ingredients: weigh the fabric, roll up the fabric warp beam and put it into the dyeing machine, then fill the warp beam dyeing machine with water, with a bath ratio of about 1:10, let the water circulate for 5 minutes at room temperature, weigh the auxiliary agent, the weight of aziridine crosslinking agent is 5% of the weight of the fabric, the weight of brightener (UVITEX BLH) is 1% of the weight of the fabric, dissolve and stir evenly, add to the dyeing vat, and run for 10 minutes at room temperature;

[0054] 2) Raising the temperature of the pretreatment solution from room temperature to 50°C at a heating rate of 2°C / min, keeping the temperature for 30 minutes, performing pretreatment whitening and dyeing, and then draining the water;

[0055] 3) Add water into the dyeing machine with a bath ratio of about 1:10, wash the fabric for 10 minutes, and drain;

[0056] 4) After the dyeing process is completed, the fabric is taken out from the dyeing machine and dried in a tentering setting machine at 130°C for 1 minute.

[0057] 5) Arrange the fabric on a tenter machine for padding and sizing, perform digital inkjet printing, and then steam (steam for 20 minutes at 105°C). The steamed fabric is soaped at 95°C for 10 minutes. The washed fabric is dried at 130°C in a tenter setting machine for 1 minute.

[0058] 6) The reactive printed semi-finished silk fabric is dipped into an anti-ultraviolet functional finishing liquid for post-finishing, the concentration of the anti-ultraviolet finishing agent (6160 of Chuanhua) in the anti-ultraviolet functional finishing liquid is 10 g / L, and the fabric is dried at 130° C. for 1 min.

[0059] Example 4

[0060] Fabric: 11185 silk electrospun, whitening base reactive printed fabric (weight 65g / m 2 )

[0061] 1) Ingredients: Weigh the fabric, roll up the fabric warp beam and put it into the dyeing machine, then fill the warp beam dyeing machine with water, with a bath ratio of about 1:10, and let the water circulate for 5 minutes at room temperature. Weigh the auxiliary agent, the weight of the blocked isocyanate is 7% of the weight of the fabric, and the weight of the brightener (UVITEX BLH) is 3% of the weight of the fabric, dissolve and stir evenly, add to the dyeing vat, and run for 10 minutes at room temperature;

[0062] 2) Raising the temperature of the pretreatment solution from room temperature to 50°C at a heating rate of 2°C / min, keeping the temperature for 30 minutes, performing pretreatment whitening and dyeing, and then draining the water;

[0063] 3) Add water into the dyeing machine with a bath ratio of about 1:10, wash the fabric for 10 minutes, and drain;

[0064] 4) After the dyeing process is completed, the fabric is taken out from the dyeing machine and dried in a tentering setting machine at 130°C for 1 minute;

[0065] 5) Arrange the fabric on a tenter machine for padding and sizing, perform digital inkjet printing, and then steam (steam for 20 minutes at 105°C). The steamed fabric is soaped at 95°C for 10 minutes. The washed fabric is dried at 130°C in a tenter setting machine for 1 minute.

[0066] 6) The reactive printed semi-finished silk fabric is dipped into an anti-ultraviolet functional finishing liquid for post-finishing, the concentration of the anti-ultraviolet finishing agent (6160 of Chuanhua) in the anti-ultraviolet functional finishing liquid is 10 g / L, and the fabric is dried at 130° C. for 1 min.

[0067] Example 5

[0068] Fabric: 11185 silk electrospun, whitening base reactive printed fabric (weight 65g / m 2 )

[0069] 1) Preparation: Weigh the fabric, roll up the fabric into the dyeing machine, and then add water to the dyeing machine, with a bath ratio of about 1:10. Let the water circulate for 5 minutes at room temperature. Weigh the auxiliary agent, the weight of the aziridine crosslinking agent is 5% of the weight of the fabric, and the weight of the brightener (UVITEX BLH) is 2% of the weight of the fabric, dissolve and stir evenly, add to the dyeing tank, and run for 10 minutes at room temperature;

[0070] 2) raising the temperature of the pretreatment solution from room temperature to 30°C at a heating rate of 2°C / min, maintaining the temperature for 60 minutes, performing pretreatment whitening and dyeing, and then draining the water;

[0071] 3) Add water into the dyeing machine with a bath ratio of about 1:10, wash the fabric for 10 minutes, and drain;

[0072] 4) After the dyeing process is completed, the fabric is taken out from the dyeing machine and dried in a tentering setting machine at 130°C for 1 minute.

[0073] 5) After the fabric is arranged on a tenter machine for dipping and sizing, it is digitally printed and then steamed (steamed at 105°C for 20 minutes). The steamed fabric is soaped at 95°C for 10 minutes. The washed fabric is dried at 130°C on a tenter setting machine for 1 minute.

[0074] 6) The reactive printed semi-finished silk fabric is dipped into an anti-ultraviolet functional finishing liquid for post-finishing, wherein the concentration of the anti-ultraviolet finishing agent (Rudolf's UVR) in the anti-ultraviolet functional finishing liquid is 10 g / L, and the fabric is dried at 150° C. for 30 seconds.

[0075] Example 6

[0076] Fabric: 11185 silk electrospun, whitening base reactive printed fabric (weight 65g / m 2 )

[0077] 1) Preparation: Weigh the fabric, roll up the fabric into the dyeing machine, and then add water to the dyeing machine, with a bath ratio of about 1:10. Let the water circulate for 5 minutes at room temperature. Weigh the auxiliary agent, the weight of the aziridine crosslinking agent is 5% of the weight of the fabric, and the weight of the brightener (UVITEX BLH) is 2% of the weight of the fabric, dissolve and stir evenly, add to the dyeing tank, and run for 10 minutes at room temperature;

[0078] 2) raising the temperature of the pretreatment solution from room temperature to 80°C at a heating rate of 2°C / min, keeping the temperature for 20 minutes, performing pretreatment whitening and dyeing, and then draining the water;

[0079] 3) Add water into the dyeing machine with a bath ratio of about 1:10, wash the fabric for 10 minutes, and drain;

[0080] 4) After the dyeing process is completed, the fabric is taken out from the dyeing machine and dried in a tentering setting machine at 130°C for 1 minute.

[0081] 5) After the fabric is arranged on a tenter machine for dipping and sizing, it is digitally printed and then steamed (steamed at 105°C for 20 minutes). The steamed fabric is soaped at 95°C for 10 minutes. The washed fabric is dried at 130°C on a tenter setting machine for 1 minute.

[0082] 6) The reactive printed semi-finished silk fabric is dipped into an anti-ultraviolet functional finishing liquid for post-finishing, the concentration of the anti-ultraviolet finishing agent (6160 of Chuanhua) in the anti-ultraviolet functional finishing liquid is 10 g / L, and the fabric is dried at 110° C. for 150 s.

[0083] Comparative Example 1

[0084] Fabric: 11185 silk electrospun, whitening base reactive printed fabric (weight 65g / m 2 )

[0085] 1) Preparation: Weigh the fabric, roll up the fabric warp beam and put it into the dyeing machine, then fill the warp beam dyeing machine with water, with a bath ratio of about 1:10, and let the water circulate for 5 minutes at room temperature. Weigh the auxiliary agent, the weight of the aziridine crosslinking agent is 4% of the weight of the fabric, and the weight of the brightener (UVITEX BLH) is 0.8% of the weight of the fabric, dissolve and stir evenly, add to the dyeing vat, and run at room temperature for 10 minutes;

[0086] 2) Raise the temperature of the pretreatment solution from room temperature to 50°C at a heating rate of 2°C / min, keep warm for 30 minutes, perform pretreatment whitening and dyeing, and then drain;

[0087] 3) Add water into the dyeing machine with a bath ratio of about 1:10, wash the fabric for 10 minutes, and drain;

[0088] 4) After the dyeing process is completed, the fabric is taken out from the dyeing machine and dried in a tentering setting machine at 130°C for 1 minute.

[0089] 5) After the fabric is arranged on a tenter machine for dipping and sizing, it is digitally printed and then steamed (steamed at 105°C for 20 minutes). The steamed fabric is soaped at 95°C for 10 minutes. The washed fabric is dried at 130°C on a tenter setting machine for 1 minute.

[0090] 6) The reactive printed semi-finished silk fabric is dipped into an anti-ultraviolet functional finishing liquid for post-finishing, the concentration of the anti-ultraviolet finishing agent (6160 of Chuanhua) in the anti-ultraviolet functional finishing liquid is 10 g / L, and the fabric is dried at 130° C. for 1 min.

[0091] Comparative Example 2

[0092] Fabric: 11185 silk electrospun, whitening base reactive printed fabric (weight 65g / m 2 )

[0093] 1) Ingredients: Weigh the fabric, roll up the fabric warp beam and put it into the dyeing machine, then fill the warp beam dyeing machine with water, with a bath ratio of about 1:10, let the water circulate for 5 minutes at room temperature, weigh the auxiliaries, the weight of the aziridine crosslinking agent is 12% of the weight of the fabric, and the weight of the brightener (UVITEX BLH) is 6% of the weight of the fabric, dissolve and stir evenly, add to the dyeing tank, and operate at room temperature for 10 minutes;

[0094] 2) Raising the temperature of the pretreatment solution from room temperature to 50°C at a heating rate of 2°C / min, keeping the temperature for 30 minutes, performing pretreatment whitening and dyeing, and then draining the water;

[0095] 3) Add water into the dyeing machine with a bath ratio of about 1:10, wash the fabric for 10 minutes, and drain;

[0096] 4) After the dyeing process is completed, the fabric is taken out from the dyeing machine and dried in a tentering setting machine at 130°C for 1 minute.

[0097] 5) After the fabric is arranged on a tenter machine for dipping and sizing, it is digitally printed and then steamed (steamed at 105°C for 20 minutes). The steamed fabric is soaped at 95°C for 10 minutes. The washed fabric is dried at 130°C on a tenter setting machine for 1 minute.

[0098] 6) The reactive printed semi-finished silk fabric is dipped into an anti-ultraviolet functional finishing liquid for post-finishing, the concentration of the anti-ultraviolet finishing agent (6160 of Chuanhua) in the anti-ultraviolet functional finishing liquid is 10 g / L, and the fabric is dried at 130° C. for 1 min.

[0099] Comparative Example 3

[0100] Fabric: 11185 silk electrospun, white background reactive printed fabric (weight 65g / m 2 )

[0101] 1) Add a conventional amount of dye to the dyeing machine, the dye is 0.05% of the weight of the fabric, stir evenly, soak the fabric and place it in the dyeing machine, keep it warm at 50°C for 30 minutes for dyeing;

[0102] 2) After the dyeing process is completed, the fabric is taken out from the dyeing machine and dried in a tentering setting machine at 130°C for 1 minute.

[0103] 3) After the fabric is arranged on a tenter machine for dipping and sizing, it is digitally printed and then steamed (steamed at 105°C for 20 minutes). The steamed fabric is soaped at 95°C for 10 minutes. The washed fabric is dried at 130°C on a tenter setting machine for 1 minute.

[0104] 4) The reactive printed semi-finished silk fabric was dipped into an anti-ultraviolet functional finishing liquid for post-finishing, the concentration of the anti-ultraviolet finishing agent (6160 of Chuanhua) in the anti-ultraviolet functional finishing liquid was 60 g / L, and the fabric was dried at 130° C. for 1 min.

[0105] Comparative Example 4

[0106] Fabric: 11185 silk electrospun, whitening base reactive printed fabric (weight 65g / m 2 )

[0107] 1) Ingredients: Weigh the fabric, roll up the fabric warp beam and put it into the dyeing machine, then fill the warp beam dyeing machine with water, with a bath ratio of about 1:10, let the water circulate for 5 minutes at room temperature, weigh the auxiliary agent, the whitening agent (UVITEX BLH) is 2% of the weight of the fabric, dissolve and stir evenly, add it to the dyeing tank, and run it at room temperature for 10 minutes;

[0108] 2) Raising the temperature of the pretreatment solution from room temperature to 50°C at a heating rate of 2°C / min, keeping the temperature for 30 minutes, performing pretreatment whitening and dyeing, and then draining the water;

[0109] 3) Add water into the dyeing machine with a bath ratio of about 1:10, wash the fabric for 10 minutes, and drain;

[0110] 4) After the dyeing process is completed, the fabric is taken out from the dyeing machine and dried in a tentering setting machine at 130°C for 1 minute.

[0111] 5) After the fabric is arranged on a tenter machine for dipping and sizing, it is digitally printed and then steamed (steamed at 105°C for 20 minutes). The steamed fabric is soaped at 95°C for 10 minutes. The washed fabric is dried at 130°C on a tenter setting machine for 1 minute.

[0112] 6) The reactive printed semi-finished silk fabric is dipped into an anti-ultraviolet functional finishing liquid for post-finishing, wherein the concentration of the anti-ultraviolet finishing agent (6160 of Chuanhua) in the anti-ultraviolet functional finishing liquid is 60 g / L, and the fabric is dried at 130° C. for 1 min.

[0113] The ultraviolet protection performance of the silk fabrics (including white embryos, fabrics after pretreatment, fabrics after dyeing, sizing, steaming and soaping, and fabrics after finishing) at each stage of the preparation process in Examples 1-6 and Comparative Examples 1-4 was tested respectively. The test standard for the ultraviolet protection performance of fabrics was based on GB / T 18830-2009 Evaluation of the ultraviolet protection performance of textiles. The test results are shown in Table 1.

[0114] Table 1

[0115]

[0116] It can be seen from the test results in Table 1 that in Examples 1-6, after the fabric is treated with the pretreatment liquid (quantitative compound of brightener and crosslinking agent), the UPF value increases significantly, and the UVA value and UVB value passing through the fabric decrease significantly, indicating that after the silk fabric is subjected to whitening and crosslinking pretreatment, the white base part of the silk fabric has excellent anti-ultraviolet performance.

[0117] The UPF value, UVA value and UVB value of the fabrics in Examples 1-6 did not change much before and after the dyeing, sizing, steaming and soaping treatments, indicating that after the fabrics were treated with the pre-treatment solution with a specific formula in the present invention, the brightener was durably attached to the surface of the silk fabric, improving the wash resistance of the brightener, and the white base part of the silk fabric had wash-resistant and UV-resistant properties.

[0118] The fabrics in Examples 1-6 were subjected to anti-ultraviolet functional post-finishing, which could further significantly improve the anti-ultraviolet coefficient of the finished silk fabrics, and the finished products still had excellent anti-ultraviolet performance after being washed 5 times.

[0119] When the dosage of aziridine crosslinker and brightener in the pretreatment liquid of Comparative Example 1 is too low, the anti-ultraviolet performance of the fabric after pretreatment is reduced, and the anti-ultraviolet performance of the final finished silk fabric cannot meet the national standard requirements for anti-ultraviolet fabrics after 5 washes.

[0120] When the dosage of aziridine crosslinker and brightener in the pretreatment liquid of Comparative Example 2 is too high, the fabric after pretreatment has good UV resistance and good wash resistance. The finished product still has excellent UV resistance after 5 washings, but the improvement of the fabric's UV protection performance is not obvious. Considering the cost comprehensively, Examples 1-6 are more economical.

[0121] In Comparative Example 3, the fabric was not pre-treated, and was directly dyed, reactively printed, and subjected to anti-ultraviolet functional post-finishing. On the one hand, the ultraviolet protection performance of the fabric after dyeing and soaping was very poor. Even if the concentration of the anti-ultraviolet auxiliary agent was increased to 60 g / L, the anti-ultraviolet performance of the finished fabric could not meet the national standard for anti-ultraviolet fabrics. Moreover, the anti-ultraviolet performance of the fabric decreased significantly after 5 washings, indicating that the anti-ultraviolet and water-washing resistance of the fabric decreased significantly.

[0122] In Comparative Example 4, no cross-linking agent was added to the pretreatment liquid, only a brightener was added. The anti-ultraviolet performance of the fabric after pretreatment was significantly improved compared with the white blank, but the anti-ultraviolet performance of the fabric decreased significantly after dyeing, sizing, steaming and soaping treatment, and the final product index after anti-ultraviolet finishing was not good. The anti-ultraviolet performance of the silk fabric decreased significantly after 5 washings, and the anti-ultraviolet and water-washing resistance were not ideal.

[0123] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A durable UV-resistant reactive printed silk fabric, characterized in that: The silk fabric is immersed in a pretreatment liquid before dyeing to form a washable whitening anti-ultraviolet layer on its surface. After dyeing and reactive printing, the silk fabric is then padded / dipped into an anti-ultraviolet functional finishing liquid to form a reinforced anti-ultraviolet layer on its surface. The pre-treatment liquid includes a brightener and a cross-linking agent.

2. The durable UV-resistant reactive printed silk fabric according to claim 1, characterized in that: The weight ratio of the whitening agent to the silk fabric is 1-5%, and the weight ratio of the cross-linking agent to the silk fabric is 5-10%.

3. The durable UV-resistant reactive printed silk fabric according to claim 1 or 2, characterized in that: The cross-linking agent is aziridine or blocked isocyanate.

4. The durable UV-resistant reactive printed silk fabric according to claim 3, characterized in that: The brightener is a distyrylbiphenyl compound derivative or a distyrylsulfonic acid derivative.

5. The durable UV-resistant reactive printed silk fabric according to claim 1, characterized in that: The anti-ultraviolet functional finishing liquid comprises an anti-ultraviolet finishing agent, and the anti-ultraviolet finishing agent is a triazine derivative.

6. A durable anti-ultraviolet dyeing and finishing process for reactive printed silk fabrics, characterized in that: The steps include: S1, immersing the silk fabric in a pretreatment solution at a temperature of 30 to 80° C. for a treatment time of 20 to 80 min, to form a washable whitening and anti-ultraviolet layer on the surface thereof, wherein the pretreatment solution comprises a whitening agent and a cross-linking agent; S2, the treated silk fabric is dyed and then subjected to reactive printing; S3, then padding / dyeing the semi-finished silk printed fabric into the anti-ultraviolet functional finishing liquid to form a reinforced anti-ultraviolet layer on its surface.

7. The durable anti-ultraviolet dyeing and finishing process for silk fabric according to claim 6, characterized in that: The cross-linking agent is aziridine or blocked isocyanate, and the brightener is a distyryl biphenyl compound derivative or a distyryl sulfonic acid derivative.

8. The durable anti-ultraviolet dyeing and finishing process for silk fabric according to claim 7, characterized in that: The weight ratio of the whitening agent to the silk fabric is 1-5%, and the weight ratio of the cross-linking agent to the silk fabric is 5-10%.

9. The durable anti-ultraviolet dyeing and finishing process of silk fabric according to claim 6, characterized in that: The anti-ultraviolet functional finishing liquid comprises an anti-ultraviolet finishing agent, and the anti-ultraviolet finishing agent is a triazine derivative.

10. The durable anti-ultraviolet dyeing and finishing process of silk fabric according to claim 9, characterized in that: In the step S3, during the anti-ultraviolet finishing process, the treatment temperature is 110-150° C. and the treatment time is 30-150 seconds.