Spinning method capable of improving strength of natural colored cotton yarn

Through the combined ester bundling agent and low-ester pectin additives combined with jet vortex spinning technology, the strength and quality problems in spinning natural color cotton yarns are solved, and the preparation of high-strength yarns is realized, and the slurry-free weaving and biological enzyme refinement is achieved. Maintain good performance in the middle.

CN118932708APending Publication Date: 2024-11-12ZHEJIANG JIUSHUN TEXTILE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411170510.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Natural color cotton yarns are unstable in the spinning process and have low fiber quality, making it difficult to prepare high-strength yarns, especially in slurry-free weaving and biological enzyme refining processing.

Method used

Using an auxiliary agent composed of ester bundling agent and low-ester pectin, combined with jet vortex spinning technology, the fiber clamping force and yarn strength are improved through cotton grinding, steel cleaning, combed and stripping processes, and the fiber clamping force and yarn strength are improved, and the vortex spinning process is carried out. Use specific air pressure and spinning speed to prepare high-strength natural colored cotton yarns.

Benefits of technology

It significantly improves the strength and structural tightness of natural colored cotton yarns, meets the requirements of slurry-free weaving, and does not affect the subsequent biological enzyme refining effect, improving the biological enzyme degreasing effect of the yarn.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932708A_ABST
    Figure CN118932708A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of spinning, and particularly provides a spinning method capable of improving the strength of natural colored cotton yarn by means of auxiliaries. The auxiliary agent is composed of an effective component and water, wherein the effective component is composed of an ester bundling agent and low-ester pectin; the method comprises the following steps: respectively obtaining colored cotton combed slivers and white cotton combed slivers by using colored cotton raw cotton and white cotton raw cotton; the colored cotton combed slivers and the white cotton combed slivers are subjected to primary drawing, and then auxiliaries are sprayed; carrying out secondary drawing and tertiary drawing in sequence; and carrying out air jet vortex spinning on the mixed cotton slivers subjected to three-time drawing to obtain the high-strength natural colored cotton yarns. By the adoption of the method, the yarn which is compact in structure, bundled and improved in strength can be prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of textiles and relates to high-performance fiber materials, in particular to a spinning method capable of improving the strength of natural colored cotton yarn. The high-strength natural colored cotton yarn is suitable for subsequent bio-enzyme refining processing. Background Art

[0002] Natural colored cotton (abbreviated as colored cotton) does not require bleaching and dyeing, and has excellent antibacterial and antioxidant activity. It is a natural, green, and healthy functional fiber; it has great application prospects in the fields of sanitary and health textiles and medical textiles. However, natural colored cotton still has inherent defects, such as unstable color and relatively low fiber quality, which brings challenges to its high-value textile processing. Natural colored cotton products are not suitable for sizing and weaving, because strong alkali desizing will cause significant discoloration and discoloration of natural colored cotton, and its antibacterial functionality will also be greatly affected. Spinning special yarn for natural colored cotton sizing-free weaving, sizing-free weaving and subsequent composite bio-enzyme degreasing are the most gentle and suitable processing methods for natural colored cotton products. However, the poor fiber quality of natural colored cotton makes it quite difficult to prepare high-strength yarn for sizing-free weaving.

[0003] At present, many methods for making special cotton yarn for size-free weaving have been reported. For example, patent CN 201510246441.4 reports a method for preparing size-free cotton yarn by pre-treating with a padding solution and then spinning. The specific steps are as follows: prepare solvent: a pre-prepared padding solution obtained by mixing a strong alkali agent, a softener, a breaker, sodium chloride and water, and pre-cool it to -15℃~5℃; immerse the yarn; padding treatment; yarn cleaning; drying the finished product. However, this method is obviously not suitable for the processing of colored cotton, because strong alkali will change the color of colored cotton, and softeners (generally silicone oils) and the like covering the fiber surface will affect the bio-enzyme refining effect of colored cotton products. In the preparation of colored cotton yarn for size-free weaving, additives should be used with caution to avoid affecting the degreasing effect of the subsequent bio-complex enzyme (a complex of lipase, pectinase and cellulase). Because this type of polymer additive will form a film on the fiber surface, preventing the bio-enzyme from contacting the fiber surface. Therefore, it is very important to select suitable additives for preparing size-free cotton yarn using natural colored cotton and making it suitable for bio-enzyme refining processing.

[0004] The conventional vortex spinning process of blended yarn is as follows:

[0005] Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a spinning method and auxiliary agents used for improving the strength of natural colored cotton yarn.

[0007] In order to solve the above technical problems, the present invention provides an auxiliary agent for improving the strength of natural colored cotton yarn, which is composed of an effective ingredient and water, wherein the effective ingredient is composed of an ester sizing agent and low-ester pectin;

[0008] The ester sizing agent accounts for 2% to 10% (preferably 2.5 to 7.5%) of the total weight of the auxiliary agent, the low-ester pectin accounts for 2% to 10% (preferably 3.5 to 9%) of the total weight of the auxiliary agent, and the balance is water.

[0009] As an improvement of the auxiliary agent of the present invention: the esterification degree of the low-ester pectin is 25% to 45% (preferably 30 to 40%).

[0010] As a further improvement of the auxiliary agent of the present invention: the ester sizing agent is at least any one of the following: sodium salt of n-butyl oleate sulfate, triethanolamine salt of lauryl sulfate, castor oil phosphate (ie, one or more).

[0011] As a further improvement of the adjuvant of the present invention: the ester clustering agent is sodium salt of n-butyl oleate sulfate, accounting for 5% of the total weight of the adjuvant; the esterification degree of low-ester pectin is 30%, accounting for 7.5% of the total weight of the adjuvant.

[0012] The present invention also provides a spinning method for improving the strength of natural colored cotton yarn by using the above-mentioned auxiliary agent, comprising the following steps:

[0013] 1) The colored cotton raw cotton and the white cotton raw cotton are respectively subjected to cotton picking, steel cleaning and combing in sequence, thereby obtaining colored cotton combed sliver and white cotton combed sliver respectively;

[0014] 2) According to the dry weight ratio (percentage) of colored cotton combed sliver to white cotton combed sliver of 30:70-100:0 (preferably 35:65-85:15), the colored cotton combed sliver and the white cotton combed sliver are combined to obtain a combined and mixed colored cotton / white cotton mixed sliver;

[0015] 3) Spraying the mixed colored cotton / white cotton sliver obtained in step 2) with an auxiliary agent, wherein the amount of the active ingredient in the auxiliary agent is 0.5% to 3% of the total weight (dry weight) of the mixed colored cotton / white cotton sliver;

[0016] 4) The product obtained in step 3) is subjected to double and triple combining in sequence to obtain a triple combined mixed cotton strip;

[0017] 5) The three-combined mixed cotton strips obtained in step 4) are subjected to jet vortex spinning to obtain high-strength natural colored cotton yarn.

[0018] As an improvement of the spinning method of the present invention that can improve the strength of natural colored cotton yarn:

[0019] In the step 5), the air pressure of the vortex spinning nozzle is 0.5-0.6 MPa, and the spinning speed is 280-330 m / min.

[0020] As a further improvement of the spinning method of the present invention that can improve the strength of natural colored cotton yarn:

[0021] White raw cotton is long-staple cotton, with an average fiber upper part length of >30.5mm, a uniformity index of >85.5%, and a micronaire value of >4.05.

[0022] The process flow of the spinning method of the high-strength natural colored cotton yarn of the present invention is as follows:

[0023]

[0024] Based on the problems existing in the prior art, the present invention proposes an auxiliary agent and a spinning process technology method for colored cotton spinning which can significantly enhance the fiber cohesion during vortex spinning to enhance the yarn strength to meet the requirements of pulp-free weaving, while not affecting the subsequent bio-enzyme refining effect.

[0025] The principle of the present invention is: firstly, high-quality long-staple white cotton raw cotton is selected to prepare colored cotton combed slivers and white cotton combed slivers respectively, and then the slivers are drawn according to a predetermined ratio, and then the slivers are pre-treated by spraying a composite auxiliary agent containing an ester sizing agent and a low-ester pectin tackifier to increase the cohesion of the fiber in the yarn-forming process (yarn strength), thereby improving the yarn strength and reducing the hairiness. On the other hand, the added low-ester pectin also increases the fiber cohesion and reduces the static electricity generated by the friction of the fiber. Combined with the process flow of the present invention, the high-strength natural colored cotton yarn of the present invention is obtained.

[0026] In summary, the present invention has made a series of technical innovations, including the use of jet vortex spinning and the use of the special additives of the present invention to treat the fibers by spraying to prepare a yarn with a compact structure, bundled structure and improved strength (such as Figure 1 to Figure 4 ), and the compound auxiliary agent will not affect the refining effect of the biological compound enzyme of the colored cotton products after pulp-free weaving. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The specific implementation modes of the present invention are further described in detail below with reference to the accompanying drawings.

[0028] Figure 1 This is an electron microscope image of the vortex spun yarn prepared in Example 1 of the present invention.

[0029] Figure 2 This is an electron microscope image of the vortex spun yarn prepared in Example 2 of the present invention.

[0030] Figure 3 This is an electron microscope image of the vortex spun yarn prepared in Example 3 of the present invention.

[0031] Figure 4 This is an electron microscope image of the vortex spun yarn prepared in Example 4 of the present invention.

[0032] Figure 5 This is an electron microscope image of the vortex spun yarn prepared in Comparative Example 5 of the present invention.

[0033] Figure 6 This is an electron microscope image of the vortex spun yarn prepared in Comparative Example 6 of the present invention;

[0034] Note: During microscope testing, due to the relationship between the density of sample placement and the size of the screenshot, Figure 2-3 One yarn is shown, while the remaining figures show two yarns. DETAILED DESCRIPTION

[0035] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto:

[0036] The natural colored cotton raw cotton fiber selected by the present invention has the following quality indicators: the average length of the upper half of the fiber is 29.6 mm, the uniformity index is 83.8%, and the specific strength is 30.1 cN·tex -1 , elongation 6.5%, micronaire value 4.01. The natural colored cotton raw cotton fiber was purchased from China Color Cotton (Group) Co., Ltd. The following cases all use the same natural colored cotton raw cotton fiber.

[0037] Embodiment 1, a method for spinning high-strength natural colored cotton yarn:

[0038] The process flow is as follows: Process formula 2:

[0039]

[0040] The selected cotton was long-staple white cotton from Xinjiang with an average fiber upper half length of 31.1 mm, a uniformity index of 87.2%, and a micronaire value of 4.11.

[0041] The auxiliary agent is composed of 5% by mass concentration of the sizing agent sodium salt of n-butyl oleate sulfate, 7.5% by mass concentration of low-ester pectin (esterification degree is 30%) and the balance of water.

[0042] Combed colored cotton slivers and white cotton slivers in a dry weight percentage of 50:50 to obtain a mixed colored cotton / white cotton mixed sliver;

[0043] The sum of the ester sizing agent and the low-ester pectin is named as the effective component; the amount of the effective component is 1.5% of the total weight (dry weight) of the mixed colored cotton / white cotton slivers.

[0044] Note: The above-mentioned processes of cotton plucking, steel cleaning, combing and drawing are all basic processing processes in the spinning industry.

[0045] The cotton plucking process uses the FA002 disc plucking machine produced by Zhengzhou Haitong Heavy Industry Technology Co., Ltd.

[0046] The cleaning process uses the CLC1 cotton opener and TC10 cotton carding machine of German Trützschler Company and the SC-III cotton cleaning machine of Yancheng Jinda Textile Machinery Manufacturing Co., Ltd.

[0047] The combing process uses the JSFA588 combing machine of Jiangsu Kaigong Machinery Co., Ltd.

[0048] The machine adopts three drawing processes, using the TMFD101L first drawing frame produced by Hubei Tianmen Textile Machinery Co., Ltd., and the TMFD81S and TMFD81L drawing frames for the second and third drawing processes;

[0049] The vortex spinning adopts the 870EX vortex spinning machine produced by Japan Murata Company.

[0050] in,

[0051] Cotton picking: The cotton picking process parameters for colored cotton and white cotton are the same, which are: cotton picking beater speed 850 rpm, cotton picking arm drop 3.0 mm / time, trolley rotation speed 2.0 rpm;

[0052] Cleaning and steel-cleaning process parameters for colored cotton and white cotton are the same, which are: licker-in speed is 900r / min, cylinder speed is 350r / min, cover speed is 190mm / min, licker-in-cylinder gauge is 0.22mm, cylinder-cover gauge is 0.25mm, cylinder-doffer gauge is 0.12mm.

[0053] Combing: Differentiate the combing process parameters for colored cotton and white cotton;

[0054] The combing parameters of colored cotton are: cylinder positioning index 36, cotton drop gauge 6mm, drafting gauge 6mm, carding gauge 0.34mm, top comb needle density 32 needles / cm.

[0055] The combing parameters of white cotton are: cylinder positioning index 38, cotton drop gauge 9mm, drafting gauge 9mm, carding gauge 0.36mm, top comb needle density 32 needles / cm.

[0056] Drawing: including first drawing, second drawing and third drawing;

[0057] When the heads are combined, a total of 8 colored cotton combed slivers and white cotton combed slivers are combined at a dry weight percentage of 50:50 to obtain a combined and mixed colored cotton / white cotton mixed sliver.

[0058] Spraying an additive: spraying an additive on the mixed colored cotton / white cotton mixed cotton strips, wherein the amount of the active ingredient in the additive accounts for 1.5% of the total weight (dry weight) of the mixed colored cotton / white cotton mixed cotton strips, to obtain the mixed colored cotton / white cotton mixed cotton strips after spraying the additive;

[0059] When the second cotton strips are combined, 6 mixed colored cotton strips / white cotton strips sprayed with additives are combined;

[0060] When combining three times, combine the eight mixed cotton strips after the second combination;

[0061] The delivery speeds of the first, second and third draws are 265, 265 and 260 m / min respectively, and the total drafting multiples are 6.0, 6.0 and 8.0 times respectively.

[0062] Vortex spinning: The mixed cotton strips after three-way spinning are subjected to vortex spinning, the air pressure of the air jet nozzle is 0.55MPa, the spinning speed is 300m / min, and the colored cotton yarn is spun. The thickness of the spun yarn is 14.5tex.

[0063] Embodiment 2, a method for spinning high-strength natural colored cotton yarn

[0064] With respect to Example 1, the following changes are made:

[0065] Imported long-staple white cotton (produced in Uzbekistan) with an average fiber upper half length of 30.8 mm, a uniformity index of 86.6%, and a micronaire value of 4.09 was selected.

[0066] Combed colored cotton slivers and white cotton slivers at a dry weight percentage of 35:65;

[0067] Additives: It is composed of 2.5% mass concentration of castor oil phosphate, 9.0% mass concentration of low-ester pectin (esterification degree is 30%) and water as the balance. The sum of the ester-type sizing agent and the low-ester pectin is named as the effective component; the amount of the effective component in the additive accounts for 0.8% of the total weight (dry weight) of the mixed colored cotton / white cotton sliver.

[0068] The vortex spinning nozzle air pressure was 0.52 MPa, and the spinning speed was 325 m / min, and the colored cotton yarn was spun.

[0069] The rest is the same as Example 1.

[0070] Embodiment 3, a method for spinning high-strength natural colored cotton yarn

[0071] With respect to Example 1, the following changes are made:

[0072] The Egyptian long-staple white cotton was selected, with an average fiber upper half length of 31.3 mm, a uniformity index of 87.5%, and a micronaire value of 4.13.

[0073] Combed colored cotton slivers and white cotton slivers at a dry weight percentage of 65:35;

[0074] Additives: It is composed of 3.5% mass concentration of sizing agent sodium salt of n-butyl oleate sulfate, 7.0% mass concentration of low-ester pectin (esterification degree is 40%) and water as the balance. The sum of the ester sizing agent and the low-ester pectin is named as the effective component; the amount of the effective component in the additive accounts for 2.0% of the total weight (dry weight) of the mixed colored cotton / white cotton sliver.

[0075] The vortex spinning nozzle air pressure was 0.55 MPa, and the spinning speed was 300 m / min, and the colored cotton yarn was spun.

[0076] The rest is the same as Example 1.

[0077] Embodiment 4, a method for spinning high-strength natural colored cotton yarn

[0078] With respect to Example 1, the following changes are made:

[0079] The selected cotton was long-staple white cotton from Xinjiang with an average fiber upper half length of 31.5 mm, a uniformity index of 88.1%, and a micronaire value of 4.14.

[0080] Combed colored cotton slivers and white cotton slivers at a dry weight percentage of 85:15;

[0081] Additives: It is composed of 7.5% mass concentration of sizing agent sodium salt of n-butyl oleate sulfate, 3.5% mass concentration of low-ester pectin (esterification degree is 40%) and water as the balance. The sum of the ester sizing agent and the low-ester pectin is named as the effective component; the amount of the effective component in the additive accounts for 2.8% of the total weight (dry weight) of the mixed colored cotton / white cotton sliver.

[0082] The vortex spinning nozzle air pressure was 0.58 MPa, and the spinning speed was 285 m / min, and colored cotton yarn was spun.

[0083] The rest is the same as Example 1.

[0084] In Example 5 series, the auxiliary agents of Example 2 are respectively replaced by the auxiliary agents described in Example 1, Example 3, and Example 4, and the rest are the same as Example 2, and Example 5-1, Example 5-2, and Example 5-3 are obtained accordingly; the auxiliary agents of Example 2 are respectively replaced by the auxiliary agents described in Table 1 below, and the rest are the same as Example 2, and Example 5-4 and Example 5-5 are obtained accordingly.

[0085] Table 1

[0086] Additives Example 2 2.5% of the sizing agent castor oil phosphate + 9.0% low ester pectin (esterification degree is 30%) Example 5-1 5% of the sizing agent sodium butyl oleate sulfate + 7.5% of low-ester pectin (esterification degree is 30%) Example 5-2 3.5% of the bulking agent sodium butyl oleate sulfate + 7.0% of low-ester pectin (esterification degree is 40%) Example 5-3 7.5% of the bulking agent sodium butyl oleate sulfate + 3.5% of low-ester pectin (esterification degree is 40%) Example 5-4 2.5% of the sizing agent sodium butyl oleate sulfate + 9.0% low-ester pectin (esterification degree is 30%) Example 5-5 2.5% of the sizing agent lauryl sulfate triethanolamine salt + 9.0% low-ester pectin (esterification degree is 30%)

[0087] experiment:

[0088] The yarn strength is tested according to the national standard GB / T 3916-1997 "Determination of breaking strength and breaking elongation of single yarn in textile packaged yarn".

[0089] The effect of bio-enzyme scouring of cotton yarn was tested as follows: first, the colored cotton yarn was scoured with bio-enzyme according to the conventional bio-enzyme scouring method (preparing a composite bio-enzyme treatment solution containing 5 mL / L alkaline pectinase, 5 mL / L lipase and 0.5% mass fraction of penetrant JFC, adjusting the pH of the enzyme solution to 9.0 with 20 g / L sodium carbonate aqueous solution, heating the enzyme solution temperature to 50°C, immersing the cotton yarn in the enzyme solution at a bath ratio of 1:100, and treating for 100 minutes), and then the refined cotton yarn was rinsed with 85°C hot water for 3 times, dried at 85°C, and 20 μL of pure water was added to the yarn, and the time taken for the water to be completely absorbed, i.e., the water wetting time, was calculated.

[0090] Result analysis:

[0091] The microscopic images of the yarns obtained in Examples 1 to 4 of the present invention are as follows: Figures 1 to 4 As shown. It can be seen from the figure that the yarns obtained in Examples 1 to 4 have a tight structure, uniform thickness, and less hairiness. The strength values ​​of the yarns obtained in the examples and the water wetting time after bio-enzyme refining are shown in Table 2. The strength range of the yarns obtained in the examples is 214 to 227 cN, which is significantly higher than the strength of the commercially available colored cotton blended yarns of the same specifications (ranging from 180 to 200 cN). After practical testing of slurry-free weaving, the weaving process was relatively smooth, the yarn breakage was relatively small, and the slurry-free weaving effect of the yarn was good. Moreover, after bio-enzyme refining, the water wetting time on the yarn surface was less than 1 s, that is, the wax on the fiber surface was basically removed, and the yarn had good hydrophilicity, indicating that the spinning auxiliaries (bundling agents and viscosity enhancers) developed by the present invention will not significantly affect the bio-enzyme refining effect of subsequent colored cotton products.

[0092] Table 2

[0093] Yarn samples Yarn strength / cN Water wetting time / s Example 1 218 <1 Example 2 225 <1 Example 3 214 <1 Example 4 221 <1 Example 5-1 227 <1 Example 5-2 224 <1 Example 5-3 222 <1 Example 5-4 220 <1 Example 5-5 219 <1

[0094] Description: Commercially available vortex-spun natural colored cotton combed yarn (specifications: colored cotton / white cotton blending ratio of 50 / 50, thickness of 14.5 tex, similar to the blending ratio and thickness of the yarn obtained in Example 1) was purchased from Beijing Zhongcai Tianxing Textile Co., Ltd., China Color Cotton (Group) Co., Ltd., and Shandong Honghe Textile Co., Ltd. The yarn strengths were 183 cN, 188 cN, and 185 cN, respectively, and the water wetting time after scouring was <1 s.

[0095] Compared with the strength of the yarn purchased from the above three companies, the strength of the yarn obtained in Example 1 is more than 15% higher, which proves that the method of the present invention improves the strength of the yarn, is suitable for subsequent pulp-free weaving, and will not significantly affect the bio-enzyme refining effect of the subsequent colored cotton products.

[0096] Comparative Example 1

[0097] The long-staple white cotton in Example 2 was replaced with imported ordinary white cotton from India (variety Shankar-6, average length of the upper half 28.3 mm), that is, the length index of the white cotton fiber did not meet the requirements of the present invention, and the rest was the same as in Example 2.

[0098] Result analysis: As shown in Table 3, the strength of the colored cotton blended yarn obtained in this example is 196 cN, the yarn strength is relatively low, the yarn breaks frequently during the actual size-free weaving process, the production efficiency is low, and the requirements of size-free weaving are not met.

[0099] Table 3

[0100] Yarn samples Yarn strength / cN Water wetting time / s Comparative Example 1 196 <1 Comparative Example 2 199 <1 Comparative Example 3 212 >10 Comparative Example 4 218 >10 Comparative Example 5 201 <1 Comparative Example 6 203 <1 Comparative Example 7 208 <1

[0101] Comparative Example 2

[0102] The long-staple white cotton with a micronaire value of 4.09 in Example 2 is replaced by long-staple cotton fiber also produced in Uzbekistan with similar other indicators but a micronaire value of 3.77, that is, the micronaire value of the white cotton fiber does not meet the requirements of the present invention, and the rest is the same as in Example 2.

[0103] Result analysis: The strength of the colored cotton blended yarn obtained in this example is 199cN, which is relatively low. In the actual size-free weaving process, the yarn breaks frequently, the production efficiency is low, and the requirements of size-free weaving are not met. This is because the white cotton fiber has a low micronaire value, poor fiber maturity, and low fiber quality, which leads to low strength of the colored cotton blended yarn. In the actual size-free weaving process, the yarn breaks frequently, which does not meet the requirements of size-free weaving.

[0104] Comparative Example 3

[0105] The sizing agent sodium salt of n-butyl oleate sulfate in Example 4 is replaced by a non-ester sizing agent polyacrylic acid, that is, the type and properties of the sizing agent do not meet the requirements of the present invention, and the rest is the same as Example 4.

[0106] Result analysis: The strength of the colored cotton blended yarn obtained in this example is 212 cN, which is similar to that of the yarn obtained in Example 4. However, after bioenzyme refining, the water wetting time of the yarn is greater than 10 s. That is, the obtained yarn seriously affects the subsequent bioenzyme refining processing effect. This is because the non-ester sizing agent polyacrylic acid used forms a protective layer on the fiber surface, and the bioenzyme cannot decompose the sizing agent, let alone completely contact and decompose the wax layer of the fiber, and cannot achieve a significant bioenzyme refining and degreasing effect.

[0107] Comparative Example 4

[0108] The low-ester pectin thickener in Example 3 was replaced with a non-pectin thickener polyvinyl alcohol, that is, the type and properties of the thickener did not meet the requirements of the present invention, and the rest was the same as Example 4.

[0109] Result analysis: The strength of the colored cotton blended yarn obtained in this example is 218cN, and the yarn strength is even higher than that of the yarn obtained in Example 3. However, after bio-enzyme refining, the water wetting time of the yarn is greater than 10s. That is, the obtained yarn seriously affects the subsequent bio-enzyme refining processing effect. This is because the thickener polyvinyl alcohol used is neither pectin nor ester, and the pectinase and lipase in the composite bio-enzyme cannot decompose it. Polyvinyl alcohol is attached to the fiber surface to form a protective layer, and the bio-enzyme cannot completely contact and decompose the wax layer of the fiber, making it difficult to achieve a significant refining and degreasing effect.

[0110] Comparative Example 5

[0111] The low-ester pectin, the thickener in Example 4, was replaced with a high-ester pectin with an esterification degree of 58%, that is, the esterification degree of the pectin did not meet the requirements of the present invention, and the rest was the same as Example 4.

[0112] Result analysis: The electron microscope image of the yarn obtained in this example is as follows Figure 5 As shown. Although this example uses a blend of good quality long-staple white cotton and colored cotton, the obtained colored cotton blended yarn has a loose structure, the fiber bonding is significantly poor, and the yarn strength is only 201cN, which is significantly lower than the strength of the yarn obtained in Example 4. In the actual pulp-free weaving process, the yarn breaks frequently, the production efficiency is not high, and the requirements of pulp-free weaving are not met. This is because the pectin used in this example has a high degree of esterification, a low viscosity, and a poor viscosity-enhancing effect, making it difficult to fully bond the fibers.

[0113] Comparative Example 6

[0114] The amount of the auxiliary agent in Example 2 is replaced by 0.3% of the total weight of the colored cotton and white cotton, that is, the amount of the auxiliary agent does not meet the requirements of the present invention, and the rest is the same as Example 2.

[0115] Result analysis: The electron microscope image of the yarn obtained in this example is as follows Figure 6As shown. Although this example uses a blend of good quality long-staple white cotton and colored cotton, the strength of the obtained colored cotton blended yarn is only 203 cN, which is significantly lower than that of the yarn obtained in Example 2. In the actual sizing-free weaving process, the yarn breaks relatively frequently, and the production efficiency is not high, which does not meet the requirements of sizing-free weaving. This is because the amount of the spinning aid is too small, the bundling and viscosity-increasing effects are limited, and it is difficult to make the fibers fully cohesive, resulting in low yarn strength.

[0116] Comparative Example 7: Change to That is, after cotton is picked, the two fiber raw materials are mixed and then cleaned and combed together, and the combing parameters refer to the combing parameters corresponding to the colored cotton in Example 1; the rest are the same as Example 1.

[0117] Result analysis: The yarn strength obtained in this example is 206cN, which is significantly lower than the yarn strength (218cN) obtained in Example 1. In the actual pulp-free weaving process, the yarn breaks relatively frequently, and the production efficiency is not high, which does not meet the requirements of pulp-free weaving. This is because the colored cotton and white cotton are mixed after the cotton plucking process, and the mixed fibers are subsequently cleaned and combed, and the process parameters suitable for colored cotton are used. Since the colored cotton fibers are shorter, the cotton drop spacing and combing spacing parameters used are smaller for white long-staple cotton, resulting in the inability to effectively remove the short lint in the white long-staple cotton, which results in too much white cotton lint in the colored cotton / white cotton blended yarn, resulting in low yarn strength.

[0118] Finally, it should be noted that the above examples are only some specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and there are many variations. All variations that can be directly derived or associated with the content disclosed by a person skilled in the art should be considered as the protection scope of the present invention.

Claims

1. An auxiliary agent for improving the strength of natural colored cotton yarn, characterized in that It consists of active ingredients and water, wherein the active ingredients consist of ester sizing agents and low-ester pectin; The ester sizing agent accounts for 2% to 10% of the total weight of the additives, the low-ester pectin accounts for 2% to 10% of the total weight of the additives, and the balance is water.

2. The auxiliary agent according to claim 1, characterized in that: The esterification degree of the low-ester pectin is 25% to 45%.

3. The auxiliary agent according to claim 1 or 2, characterized in that: The ester sizing agent is at least any one of the following: sodium salt of n-butyl oleate sulfate, triethanolamine salt of lauryl sulfate, and castor oil phosphate.

4. The auxiliary agent according to claim 3, characterized in that: The ester sizing agent is sodium salt of n-butyl oleate sulfate, accounting for 5% of the total weight of the additive; The esterification degree of the low-ester pectin is 30%, accounting for 7.5% of the total weight of the auxiliary agent.

5. A spinning method for improving the strength of natural colored cotton yarn using the auxiliary agent as claimed in any one of claims 1 to 4, characterized in that The following steps are involved: 1) The colored cotton raw cotton and the white cotton raw cotton are respectively subjected to cotton picking, steel cleaning and combing in sequence, thereby obtaining colored cotton combed sliver and white cotton combed sliver respectively; 2) According to the dry weight ratio of colored cotton combed sliver to white cotton combed sliver of 30-100:70-0, the colored cotton combed sliver and the white cotton combed sliver are combined to obtain a combined and mixed colored cotton / white cotton mixed sliver; 3) spraying the mixed colored cotton / white cotton sliver obtained in step 2) with an auxiliary agent, wherein the amount of the active ingredient in the auxiliary agent is 0.5% to 3% of the total weight of the mixed colored cotton / white cotton sliver; 4) The product obtained in step 3) is subjected to double and triple combining in sequence to obtain a triple combined mixed cotton strip; 5) The three-combined mixed cotton strips obtained in step 4) are subjected to air jet vortex spinning to obtain high-strength natural colored cotton yarn.

6. The spinning method capable of improving the strength of natural colored cotton yarn according to claim 5, characterized in that: In the step 5), the air pressure of the vortex spinning nozzle is 0.5-0.6 MPa, and the spinning speed is 280-330 m / min.

7. The spinning method capable of improving the strength of natural colored cotton yarn according to claim 5 or 6, characterized in that: White raw cotton is long-staple cotton, with an average fiber upper part length of >30.5mm, a uniformity index of >85.5%, and a micronaire value of >4.

05.

8. The spinning method capable of improving the strength of natural colored cotton yarn according to claim 7, characterized in that: The dry weight ratio of colored cotton combed sliver to white cotton combed sliver is 35-85:65-15.