Super-hydrophobic fabric containing super-crosslinked ionic polymer as well as preparation method and application of super-hydrophobic fabric

By polymerization of bisphosphonate and 2,6-bis(3-p-chloromethylbenzylimidazole)pyridine chloride under the action of catalyst, combined with ethyl cellulose and polydimethylsiloxane The treatment solves the complex and fluorine-containing problems of the existing superhydrophobic fabric preparation process, and achieves efficient and stable superhydrophobic performance and versatility, which is suitable for waterproofing and oil-water separation.

CN118932720APending Publication Date: 2024-11-12HAITAI TEXTILE SUZHOU
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410982094.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The preparation process of existing superhydrophobic fabrics is complex, time-consuming and often uses fluorine-containing substances, which limits its application in ecological environment and human health, and is difficult to achieve stable, long-lasting, multifunctional hydrophobic properties.

Method used

Binnaphthol bisphosphate, 2,6-bis(3-p-chloromethylbenzylimidazole) pyridine chloride and a catalyst were used to react in a solvent to form a supercrosslinked ionic polymer, and passed through an ethyl cellulose solution Dispersed and polydimethylsiloxane treatment to prepare fabrics with superhydrophobic properties.

Benefits of technology

It has achieved the preparation of chemically stable and reusable superhydrophobic fabrics, which have excellent waterproof and oil-water separation properties, and are simple in process and low in cost, which are suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932720A_ABST
    Figure CN118932720A_ABST
Patent Text Reader

Abstract

The invention provides a super-hydrophobic fabric containing a super-crosslinked ionic polymer as well as a preparation method and application of the super-hydrophobic fabric, and the method comprises the following steps: carrying out heating reaction on binaphthol diphosphate, chlorinated 2, 6-bis (3-p-chloromethyl benzyl imidazole) pyridine, a catalyst and a solvent to obtain the super-crosslinked ionic polymer; the method comprises the following steps: dispersing a super-crosslinked ionic polymer into ethyl cellulose-containing ethanol / deionized water to obtain a suspension solution, and pretreating a fabric by using the suspension solution to obtain a pretreated fabric; and carrying out hydrophobization treatment on the pretreated fabric by adopting a polydimethylsiloxane solution to obtain the super-hydrophobic fabric. The super-hydrophobic fabric prepared by the invention has excellent physical and chemical stability, reusability and excellent waterproof and oil-water separation performance.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The invention belongs to the technical field of textile function modification, and relates to a super-hydrophobic fabric containing a super-crosslinked ion polymer, and a preparation method and application thereof. [Background technology]

[0002] Textiles with hydrophobic properties have broad application prospects and use value. Due to their excellent waterproof, anti-fouling and self-cleaning properties, hydrophobic textiles can be widely used in outdoor rainproof clothing, industrial waterproof cloth, tents, military clothing and other fields. Due to the advantages of cheap and easy to obtain fabrics, soft and light, corrosion-resistant, and the fact that the fabric surface often has a certain degree of roughness and certain porosity, it has become one of the best materials for oil-water separation. At present, research on the preparation of super-hydrophobic fabrics based on fabric surface structure modification has made great progress, but there are often disadvantages such as complex preparation conditions, harsh and time-consuming. Therefore, it is of great significance to develop a method for preparing super-hydrophobic fabrics with mild conditions, easy operation, simple and efficient, and wide applicability to obtain stable, durable, and multifunctional super-hydrophobic fabrics and apply them to oil-water separation and hydrophobic fabric fabric research and development. For example, Ma et al. (Nature Communications 2021, 12 (1), 1) used dynamic borate and polydimethylsiloxane cross-linking to prepare a fluorine-free film with self-healing properties, which can withstand scratch tests without destroying the super-hydrophobic properties and has good durability. The construction of super-hydrophobic fabrics often requires the use of fluorinated substances, which often cause certain harm to the ecological environment and human health. Green, environmentally friendly, easy to prepare, cheap and readily available multi-functional textiles are the future development trend. On the other hand, hydrophobic fabrics still have defects such as complex preparation process and long preparation time, which limits their practical application.

[0003] Therefore, it is necessary to provide a new technical solution. [Summary of the invention]

[0004] In order to solve the above technical problems and overcome the shortcomings in the prior art books, the present invention provides a super hydrophobic fabric containing a super cross-linked ionic polymer and a preparation method and application thereof. The preparation method is simple and environmentally friendly, and the obtained hydrophobic fabric has excellent chemical stability and reusability, and has excellent waterproof and oil-water separation properties.

[0005] In order to achieve the above purpose, the following technical solutions are adopted:

[0006] In one aspect, the present invention provides a method for preparing a super-hydrophobic fabric containing a super-crosslinked ionomer, comprising the following steps:

[0007] S1, heating binaphthol bisphosphate, 2,6-bis(3-(p-chloromethylbenzylimidazole)pyridine chloride, a catalyst and a solvent to react to obtain a super cross-linked ion polymer;

[0008] S2, dispersing the hypercrosslinked ion polymer obtained in step S1 into ethanol / deionized water containing ethyl cellulose, ultrasonically obtaining a suspension solution, immersing the fabric in the suspension solution for pretreatment, and drying to obtain a pretreated fabric;

[0009] S3, immersing the pretreated fabric obtained in S2 in a polydimethylsiloxane (PDMS) solution for hydrophobic treatment, taking out and drying, to obtain a super-hydrophobic fabric.

[0010] Furthermore, step S1 specifically includes: adding binaphthol bisphosphate, 2,6-bis(3-p-chloromethylbenzylimidazole)pyridine chloride and a catalyst into a reaction bottle, adding a solvent to heat the reaction, filtering and washing after the reaction, and vacuum drying to obtain a super cross-linked ion polymer, wherein the molar ratio of the binaphthol bisphosphate, 2,6-bis(3-p-chloromethylbenzylimidazole)pyridine chloride and the catalyst is 1:0.1~10:0.1~20, and the molar ratio of the binaphthol bisphosphate to the solvent is 1mmol:1~100mL.

[0011] Furthermore, in step S1, the catalyst is one or more of ferric chloride, aluminum chloride, and ferric bromide.

[0012] Furthermore, in step S1, the solvent is one or more of dichloromethane, dichloroethane, chloroform, and trifluorotoluene.

[0013] Furthermore, the heating reaction temperature is 25-150° C., and the reaction time is 1-48 hours.

[0014] Furthermore, step S2 specifically includes: dispersing the hyper-crosslinked ionic polymer obtained in step S1 into ethanol / deionized water containing ethyl cellulose, obtaining a suspension solution after ultrasonic homogenization, immersing the fabric in the suspension and stirring, taking out and drying, and obtaining a pretreated fabric, wherein the concentration of the hyper-crosslinked ionic polymer suspension is 0.1-100 g / L, the concentration of the ethanol / deionized water containing ethyl cellulose is 0.1-100 g / L, and the volume ratio of ethanol / deionized water is 1:1-10:1.

[0015] Furthermore, step S3 specifically includes: immersing the pretreated fabric obtained in step S2 in a polydimethylsiloxane (PDMS) solution for hydrophobic treatment, and taking out the super hydrophobic fabric after the fabric drying treatment, wherein the polydimethylsiloxane concentration is 0.1 to 100 g / L, and the immersion time is 1 minute to 48 hours.

[0016] Furthermore, the fabric is one or more of cotton fabric, wool fabric, silk fabric, pure linen fabric, polyester fabric, and nylon fabric.

[0017] On the other hand, the present invention also provides a super hydrophobic fabric, which is prepared by the above preparation method.

[0018] In another aspect, the present invention further provides an application of the super hydrophobic fabric as described above, wherein the super hydrophobic fabric is applied to waterproofing and oil-water separation.

[0019] Compared with the prior art, the present invention has the following advantages:

[0020] The present invention discloses a method for preparing a super-hydrophobic fabric containing a super-crosslinked ion polymer. The method comprises the following steps: chlorinating 2,6-bis(3-p-chloromethylbenzylimidazole)pyridine and binaphthol bisphosphate under a catalyst to generate a polymerization reaction to obtain a super-crosslinked ion polymer. The super-crosslinked ion polymer particles are uniformly arranged on the surface of the fabric by the dispersion of an ethyl cellulose solution, and then immersed in a polydimethylsiloxane (PDMS) solution to perform a hydrophobic treatment to obtain a super-hydrophobic fabric. The preparation process of the super-hydrophobic fabric containing a super-crosslinked ion polymer of the present invention is simple, easy to operate, free of fluorine-containing reagents, low in cost, green and environmentally friendly, and can be prepared on a large scale. The hydrophobic cotton fabric prepared by the present invention has a contact angle of up to 153.1°, has excellent chemical stability, reusability, and excellent waterproof and oil-water separation performance. The super-hydrophobic fabric prepared by the present invention can be used repeatedly, exhibits high separation efficiency in the oil-water separation process, and has good application prospects.

Brief Description of the Drawings

[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1 This is a schematic diagram of the reaction for preparing the hyper-crosslinked ionomer of the present invention;

[0023] Figure 2 The schematic diagram of the preparation process of the super hydrophobic cotton fabric of Example 1 of the present invention;

[0024] Figure 3 This is an infrared spectrum of the super hydrophobic cotton fabric prepared in Example 1 of the present invention;

[0025] Figure 4 This is a scanning electron microscope image of the super hydrophobic cotton fabric prepared in Example 1 of the present invention;

[0026] Figure 5 This is a water contact angle image of the super hydrophobic cotton fabric prepared in Example 1 of the present invention;

[0027] Figure 6 This is a graph showing the separation efficiency of super hydrophobic cotton fabric prepared in Example 1 of the present invention for different organic solvent / water mixtures;

[0028] Figure 7 This is a graph of the oil-water separation cycles of the super-hydrophobic cotton fabric prepared in Example 1 of the present invention. [Specific implementation method]

[0029] To further help understand the technical solution of the present invention, the technical solution of the present invention is described in more detail below by providing several specific implementation examples. All of the described embodiments are only partial embodiments of the present invention, not all of them. The following specific embodiments may be combined with each other, and the same or similar concepts or processes therein may not be repeated in some embodiments.

[0030] Example 1

[0031] This embodiment provides a method for preparing a super hydrophobic fabric containing a super cross-linked ionomer. Figure 2 , which is a schematic diagram of the preparation process of the super-hydrophobic cotton fabric of Example 1 of the present invention, the method comprises the following steps:

[0032] S1. Add binaphthol bisphosphate (0.2mmol, 70mg) and 2,6-bis(3-(p-chloromethylbenzylimidazole)pyridine chloride (0.4mmol, 280mg) into a reaction bottle, pump with nitrogen for 3 times, add 20mL of dichloroethane, add catalyst aluminum chloride (4mmol, 532mg) under nitrogen protection, heat and stir at 80℃ for 24 hours, filter and wash after the reaction, wash repeatedly with anhydrous methanol until the washing liquid is colorless, and dry in vacuo to obtain a hyper-crosslinked ionic polymer.

[0033] S2. Disperse the hypercrosslinked ionic polymer obtained in step S1 into a 20 g / L ethanol / deionized water solution containing ethyl cellulose, and obtain a 5 g / L hypercrosslinked ionic polymer suspension solution after ultrasonic homogenization. Immerse the fabric in the suspension and stir for 1 hour, then take it out and dry it.

[0034] S3, soaking the cotton fabric obtained in step S2 in a 10 g / L polydimethylsiloxane (PDMS) solution for hydrophobic treatment, and taking out the super hydrophobic fabric after the fabric drying treatment after soaking for 30 minutes.

[0035] Example 2

[0036] The difference from Example 1 is that in step S1, the molar ratio of binaphthol bisphosphate, 2,6-bis(3-(p-chloromethylbenzylimidazole)pyridine chloride and anhydrous aluminum chloride is 1:1:20, and the rest is the same as Example 1.

[0037] Example 3

[0038] The difference from Example 1 is that in step S1, the molar ratio of binaphthol bisphosphate, 2,6-di(3-(p-chloromethylbenzylimidazole)pyridine chloride and anhydrous aluminum chloride is 1:3:20, and the rest is the same as Example 1.

[0039] Example 4

[0040] The difference from Example 1 is that in step S1, the molar ratio of binaphthol bisphosphate, 2,6-di(3-(p-chloromethylbenzylimidazole)pyridine chloride and anhydrous aluminum chloride is 1:2:10, and the rest is the same as Example 1.

[0041] In embodiments 1-4, the fabric is cotton fabric, and the obtained super hydrophobic fabric is super hydrophobic cotton fabric. In other embodiments, the fabric can also be one or more of cotton fabric, wool fabric, silk fabric, pure linen fabric, polyester fabric, and nylon fabric.

[0042] In another embodiment, different from Embodiment 1-4, in step S1, the molar ratios of binaphthol bisphosphate, 2,6-bis(3-(p-chloromethylbenzylimidazole)pyridine chloride, and anhydrous aluminum chloride are 1:0.5:0.5, 1:0.1:0.1, 1:5:10, and 1:10:20, respectively, and the rest are the same as Embodiment 1-4.

[0043] The water contact angles of the modified cotton fabrics prepared in Examples 1-4 were measured to be 153.1°, 138.1°, 144.9°, and 124.8°, respectively. Figure 5 This is a water contact angle picture of the hydrophobic cotton fabric prepared in Example 1 of the present invention; Figure 5 As shown, the contact angle of the hydrophobic cotton fabric obtained by the present invention can reach 153.1°, and it has excellent hydrophobic properties.

[0044] Example 5

[0045] This embodiment provides a method for preparing a super-hydrophobic fabric containing a super-crosslinked ionomer, comprising the following steps:

[0046] S1. Add binaphthol bisphosphate (0.2mmol, 70mg) and 2,6-bis(3-(p-chloromethylbenzylimidazole)pyridine chloride (0.4mmol, 280mg) into a reaction bottle, pump with nitrogen for 3 times, add 20mL of dichloroethane, add catalyst aluminum chloride (4mmol, 532mg) under nitrogen protection, heat and stir at 80°C for 36 hours, filter and wash after the reaction, wash repeatedly with anhydrous methanol until the washing liquid is colorless, and dry in vacuo to obtain a hyper-crosslinked ion polymer;

[0047] S2, dispersing the super-crosslinked ion polymer obtained in S1 into a 20 g / L ethyl cellulose ethanol / deionized water solution, and obtaining a 5 g / L super-crosslinked ion polymer suspension solution after ultrasonic homogenization, immersing the fabric in the suspension and stirring for 1 hour, and then taking it out and drying it;

[0048] S3, soaking the fabric obtained in S2 in a 10 g / L polydimethylsiloxane (PDMS) solution for hydrophobic treatment, and taking out the fabric after drying to obtain a super hydrophobic fabric after soaking for 30 minutes.

[0049] Example 6

[0050] The difference from Example 5 is that in step S1, the reaction time is 12 hours, and the rest is the same as Example 5.

[0051] Example 7

[0052] The difference from Example 5 is that in step S1, the reaction time is 6 hours, and the rest is the same as Example 5.

[0053] In other embodiments, different from Embodiment 5-7, in step S1, the reaction times are 1 min, 10 min, 30 min, 1 h, 5 h and 48 h, respectively, and the rest are the same as Embodiment 5-7.

[0054] The water contact angles of the modified cotton fabrics prepared in Examples 5-7 were measured to be 151.1°, 147.3°, and 123.9°, respectively.

[0055] Example 8

[0056] This embodiment provides a method for preparing a super-hydrophobic fabric containing a super-crosslinked ionomer, comprising the following steps:

[0057] S1. Add binaphthol bisphosphate (0.2mmol, 70mg) and 2,6-bis(3-(p-chloromethylbenzylimidazole)pyridine chloride (0.4mmol, 280mg) into a reaction bottle, pump with nitrogen for 3 times, add 20mL of dichloroethane, add catalyst aluminum chloride (4mmol, 532mg) under nitrogen protection, heat and stir at 60°C for 24 hours, filter and wash after the reaction, wash repeatedly with anhydrous methanol until the washing liquid is colorless, and dry in vacuo to obtain a hyper-crosslinked ion polymer;

[0058] S2, dispersing the super-crosslinked ion polymer obtained in S1 into a 20 g / L ethyl cellulose ethanol / deionized water solution, and obtaining a 5 g / L super-crosslinked ion polymer suspension solution after ultrasonic homogenization, immersing the fabric in the suspension and stirring for 1 hour, and then taking it out and drying it;

[0059] S3, soaking the fabric obtained in S2 in a 10 g / L polydimethylsiloxane (PDMS) solution for hydrophobic treatment, and taking out the fabric after drying to obtain a super hydrophobic fabric after soaking for 30 minutes.

[0060] Example 9

[0061] The difference from Example 8 is that in step S1, the reaction temperature is 100° C., and the rest is the same as Example 8.

[0062] In another embodiment, different from Embodiment 8-9, in step S1, the reaction temperatures are 25°C, 50°C, 120°C and 150°C, respectively, and the rest is the same as Embodiment 8-9.

[0063] The water contact angles of the modified cotton fabrics prepared in Examples 8-9 were measured to be 132.7° and 152.6°, respectively.

[0064] Example 10

[0065] This embodiment provides a method for preparing a super-hydrophobic fabric containing a super-crosslinked ionomer, comprising the following steps:

[0066] S1. Add binaphthol bisphosphate (0.2mmol, 70mg) and 2,6-bis(3-(p-chloromethylbenzylimidazole)pyridine chloride (0.4mmol, 280mg) into a reaction bottle, pump with nitrogen for 3 times, add 20mL of dichloroethane, add catalyst ferric chloride (4mmol, 648mg) under nitrogen protection, heat and stir at 80℃ for 24 hours, filter and wash after the reaction, wash repeatedly with anhydrous methanol until the washing liquid is colorless, and dry in vacuo to obtain a hyper-crosslinked ionomer;

[0067] S2, dispersing the super-crosslinked ion polymer obtained in S1 into a 20 g / L ethyl cellulose ethanol / deionized water solution, and obtaining a 5 g / L super-crosslinked ion polymer suspension solution after ultrasonic homogenization, immersing the fabric in the suspension and stirring for 1 hour, and then taking it out and drying it;

[0068] S3, soaking the fabric obtained in S2 in a 10 g / L polydimethylsiloxane (PDMS) solution for hydrophobic treatment, and taking out the fabric after drying to obtain a super hydrophobic fabric after soaking for 30 minutes.

[0069] Embodiment 11

[0070] The difference from Example 10 is that in step S1, the reaction catalyst is ferric bromide, and the rest is the same as Example 10.

[0071] The water contact angles of the modified cotton fabrics prepared in Examples 10-11 were measured to be 112.7° and 121.6°, respectively.

[0072] Example 12

[0073] This embodiment provides a method for preparing a super-hydrophobic fabric containing a super-crosslinked ionomer, comprising the following steps:

[0074] S1. Add binaphthol bisphosphate (0.2mmol, 70mg) and 2,6-bis(3-(p-chloromethylbenzylimidazole)pyridine chloride (0.4mmol, 280mg) into a reaction bottle, pump with nitrogen for 3 times, add 20mL of dichloroethane, add catalyst aluminum chloride (4mmol, 532mg) under nitrogen protection, heat and stir at 80°C for 24 hours, filter and wash after the reaction, wash repeatedly with anhydrous methanol until the washing liquid is colorless, and dry in vacuo to obtain a hyper-crosslinked ion polymer;

[0075] S2, dispersing the hyper-crosslinked ion polymer obtained in S1 into a 20 g / L ethyl cellulose ethanol / deionized water solution, and obtaining a 3 g / L hyper-crosslinked ion polymer suspension solution after ultrasonic homogenization, immersing the fabric in the suspension and stirring for 1 hour, and then taking it out and drying it;

[0076] S3, soaking the fabric obtained in S2 in a 10 g / L polydimethylsiloxane (PDMS) solution for hydrophobic treatment, and taking out the fabric after drying to obtain a super hydrophobic fabric after soaking for 30 minutes.

[0077] Example 13

[0078] The difference from Example 12 is that in step S2, the concentration of the hyper-crosslinked ionic polymer suspension solution is 10 g / L, and the rest is the same as Example 12.

[0079] In another embodiment, different from Embodiments 12 and 13, in step S2, the concentration of the hyper-crosslinked ionic polymer suspension solution is any one of 0.1 g / L, 1 g / L, 30 g / L, 50 g / L, 80 g / L and 100 g / L, and the rest is the same as Embodiments 12 and 13.

[0080] The water contact angles of the modified cotton fabrics prepared in Examples 12-13 were measured to be 142.7° and 150.6°, respectively.

[0081] Embodiment 14

[0082] This embodiment provides a method for preparing a super-hydrophobic fabric containing a super-crosslinked ionomer, comprising the following steps:

[0083] S1. Add binaphthol bisphosphate (0.2mmol, 70mg) and 2,6-bis(3-(p-chloromethylbenzylimidazole)pyridine chloride (0.4mmol, 280mg) into a reaction bottle, pump with nitrogen for 3 times, add 20mL of dichloroethane, add catalyst aluminum chloride (4mmol, 532mg) under nitrogen protection, heat and stir at 80°C for 24 hours, filter and wash after the reaction, wash repeatedly with anhydrous methanol until the washing liquid is colorless, and dry in vacuo to obtain a hyper-crosslinked ion polymer;

[0084] S2, dispersing the hyper-crosslinked ion polymer obtained in S1 into a 10 g / L ethanol / deionized water solution containing ethyl cellulose, and obtaining a 5 g / L hyper-crosslinked ion polymer suspension solution after ultrasonic homogenization, immersing the fabric in the suspension and stirring for 1 hour, and then taking it out and drying it;

[0085] S3, soaking the fabric obtained in S2 in a 10 g / L polydimethylsiloxane (PDMS) solution for hydrophobic treatment, and taking out the fabric after drying to obtain a super hydrophobic fabric after soaking for 30 minutes.

[0086] Embodiment 15

[0087] The difference from Example 14 is that in step S2, the concentration of the ethanol / deionized water solution containing ethyl cellulose is 30 g / L, and the rest is the same as Example 14.

[0088] In other embodiments, different from Embodiments 14 and 15, in step S2, the concentrations of the ethanol / deionized water solution containing ethyl cellulose are 0.1 g / L, 1 g / L, 5 g / L, 50 g / L, 80 g / L and 100 g / L, respectively, and the rest are the same as Embodiments 14 and 15.

[0089] The water contact angles of the modified cotton fabrics prepared in Examples 14-15 were measured to be 148.7° and 144.6°, respectively.

[0090] Example 16

[0091] This embodiment provides a method for preparing a super-hydrophobic fabric containing a super-crosslinked ionomer, comprising the following steps:

[0092] S1. Add binaphthol bisphosphate (0.2mmol, 70mg) and 2,6-bis(3-(p-chloromethylbenzylimidazole)pyridine chloride (0.4mmol, 280mg) into a reaction bottle, pump with nitrogen for 3 times, add 20mL of dichloroethane, add catalyst aluminum chloride (4mmol, 532mg) under nitrogen protection, heat and stir at 80°C for 24 hours, filter and wash after the reaction, wash repeatedly with anhydrous methanol until the washing liquid is colorless, and dry in vacuo to obtain a hyper-crosslinked ion polymer;

[0093] S2, dispersing the super-crosslinked ion polymer obtained in S1 into a 20 g / L ethyl cellulose ethanol / deionized water solution, and obtaining a 5 g / L super-crosslinked ion polymer suspension solution after ultrasonic homogenization, immersing the fabric in the suspension and stirring for 1 hour, and then taking it out and drying it;

[0094] S3, soaking the fabric obtained in S2 in a 5 g / L polydimethylsiloxane (PDMS) solution for hydrophobic treatment, and taking out the fabric after drying to obtain a super hydrophobic fabric after soaking for 30 minutes.

[0095] Embodiment 17

[0096] The difference from Example 16 is that in step S3, the concentration of polydimethylsiloxane (PDMS) is 15 g / L, and the rest is the same as Example 16.

[0097] In other embodiments, different from Embodiments 16 and 17, in step S3, the concentrations of polydimethylsiloxane (PDMS) are 0.1 g / L, 1 g / L, 30 g / L, 50 g / L, 80 g / L and 100 g / L, respectively, and the rest are the same as Embodiments 16 and 17.

[0098] The water contact angles of the modified cotton fabrics prepared in Examples 16-17 were measured to be 132.7° and 143.6°, respectively.

[0099] Embodiment 18

[0100] The present invention also provides a super-hydrophobic fabric containing a super-crosslinked ion polymer, which is prepared by the method of the above embodiment.

[0101] Embodiment 19

[0102] The invention also provides an application of a super-hydrophobic fabric containing a super-crosslinked ion polymer, which is applied to waterproofing and oil-water separation.

[0103] The modified cotton fabric prepared in Example 1 was tested for performance. The test results are as follows:

[0104] Figure 3 The infrared spectrum of the hydrophobic cotton fabric prepared in Example 1 of the present invention is as follows: Figure 3 As shown in the FTIR spectrum, 3324.1 cm -1 The absorption peak attributed to the stretching vibration of hydroxyl groups on cotton fibers is 2956.9 cm -1 , 2927.1cm -1 The absorption peaks are attributed to the methylene stretching and bending vibrations, 1617.6 cm -1 ,1535,1463cm -1 The absorption peak at 1314.9 cm-1 is attributed to the vibration of the aromatic ring skeleton. -1Attributable to P=O absorption peak, 1217.9cm -1 Belong to CN + Absorption peak, 1053 cm -1 Belonging to the absorption peak of silicon-oxygen stretching vibration, the infrared spectrum shows that the superhydrophobic fabric containing super-cross-linked ionic polymer was successfully prepared. Figure 4 The scanning electron microscope image of the super hydrophobic cotton fabric prepared in Example 1 of the present invention is as follows: Figure 4 As shown, the surface of the fabric is covered with a layer of granular material, and binaphthol bisphosphate and 2,6-bis(3-p-chloromethylbenzylimidazole)pyridine chloride undergo polymerization reaction under the catalysis of aluminum chloride to generate micro-nano organic polymers, which are attached to the surface of the fabric to form a rough structure. The fabric is then hydrophobized by PDMS to obtain a fabric with super hydrophobic properties.

[0105] See also Figure 6 and Figure 7 , Figure 6 This is a graph showing the separation efficiency of the hydrophobic cotton fabric prepared in Example 1 of the present invention for different organic solvent / water mixtures; Figure 7The figure is a diagram of the oil-water separation cycle number of the hydrophobic cotton fabric prepared in Example 1 of the present invention. The super-hydrophobic fabric containing super-crosslinked ion polymer prepared in Example 1 was subjected to an oil-water separation test on a mixed solution of organic solvents such as carbon tetrachloride, dichloromethane, cyclohexane, o-dichlorobenzene, petroleum ether and a methylene blue aqueous solution (volume ratio of 1:1), and the specific operation steps were: dyeing the aqueous phase with methylene blue, taking 20 mL of the aqueous phase and 20 mL of the oil phase and pouring them into an oil-water separation device, the selected oil phases were cyclohexane and petroleum ether, and the density was less than that of the aqueous phase, therefore, when the oil-water mixture was poured into the separation device, the oil phase would preferentially pass through the hydrophobic fabric when poured out of the beaker, and pass through the fabric under the action of gravity, while the aqueous phase was retained in the upper container, thereby achieving separation of the oil-water mixture. When the selected oil phase is dichloromethane, carbon tetrachloride and o-dichlorobenzene, their density is greater than that of the water phase. Therefore, when the oil-water mixture is poured into the separation device, the oil phase is below the water phase and passes through the fabric under the action of gravity, while the water phase is retained in the upper container, thereby achieving the separation of the oil-water mixture. In order to examine the separation ability of the fabric for various oil phases, the separation efficiency (R) is used as the evaluation standard, R = (V1 / V0) × 100%, where V1 is the volume of the oil phase after passing through the fabric, and V0 is the initial volume of the oil phase. After testing, the volume of dichloromethane after passing through the fabric is 19.1mL, the initial volume is 20mL, and the separation efficiency of the fabric for dichloromethane is 95%; the mass of carbon tetrachloride after passing through the fabric is 19.3mL, the initial volume is 20mL, and the separation efficiency of the fabric for dichloromethane is 96%; the volume of cyclohexane after passing through the fabric is 19.0mL, the initial volume is 20mL, and the separation efficiency of the fabric for cyclohexane is 95%; the volume of petroleum ether after passing through the fabric is 18.8mL, the initial volume is 20mL, and the separation efficiency of the fabric for petroleum ether is 94%; the mass of o-dichlorobenzene after passing through the fabric is 19.7mL, the initial volume is 20mL, and the separation efficiency of the fabric for o-dichlorobenzene is 98%. Figure 7 As shown, an oil-water separation test was carried out on a mixed solution of dichloromethane and water to evaluate the recycling performance of the prepared super-hydrophobic fabric containing super-cross-linked ionic polymer. After 10 cycles of oil-water separation experiments, the separation performance was reduced.

[0106] The invention discloses a method for preparing a super-hydrophobic fabric containing a super-crosslinked ion polymer, wherein 2,6-bis(3-p-chloromethylbenzylimidazole)pyridine and binaphthol bisphosphate are subjected to a polymerization reaction under the action of a catalyst, aluminum chloride, to obtain a super-crosslinked ion polymer, and the super-crosslinked ion polymer particles are uniformly arranged on the surface of the fabric through the dispersion of an ethyl cellulose solution, and then immersed in a polydimethylsiloxane (PDMS) solution, and subjected to a hydrophobic treatment to obtain a super-hydrophobic fabric. The hydrophobic fabric preparation process of the invention is simple, low in cost, suitable for large-scale production, can be repeatedly used, exhibits high separation efficiency in an oil-water separation process, and has good application prospects.

[0107] It should be noted that any changes made by those skilled in the art to the specific embodiments of the present invention do not deviate from the scope of the claims of the present invention. Accordingly, the scope of the claims of the present invention is not limited to the above specific embodiments.

Claims

1. A method for preparing a super-hydrophobic fabric containing a super-crosslinked ionomer, characterized in that: It includes the following steps: S1, heating binaphthol bisphosphate, 2,6-bis(3-(p-chloromethylbenzylimidazole)pyridine chloride, a catalyst and a solvent to react to obtain a super cross-linked ion polymer; S2, dispersing the hypercrosslinked ion polymer obtained in step S1 into ethanol / deionized water containing ethyl cellulose to obtain a suspension solution, and pretreating the fabric with the suspension solution to obtain a pretreated fabric; S3, using a polydimethylsiloxane solution to perform a hydrophobic treatment on the pretreated fabric obtained in step S2 to obtain a super-hydrophobic fabric.

2. The preparation method according to claim 1, characterized in that: Step S1 specifically includes: Adding binaphthol bisphosphate, 2,6-bis(3-p-chloromethylbenzylimidazole)pyridine chloride and a catalyst into a reaction bottle, adding a solvent and heating for reaction, filtering and washing after the reaction, and vacuum drying to obtain a super cross-linked ion polymer, wherein the molar ratio of the binaphthol bisphosphate, 2,6-bis(3-p-chloromethylbenzylimidazole)pyridine chloride and the catalyst is 1:0.1-10:0.1-20, and the molar ratio of the binaphthol bisphosphate to the solvent is 1 mmol:1-100 mL.

3. The preparation method according to claim 1, characterized in that: In step S1, the catalyst is one or more of ferric chloride, aluminum chloride, and ferric bromide.

4. The preparation method according to claim 1, characterized in that: In step S1, the solvent is one or more of dichloromethane, dichloroethane, chloroform, and trifluorotoluene.

5. The preparation method according to claim 1, characterized in that: The heating reaction temperature is 25-150° C., and the reaction time is 1-48 hours.

6. The preparation method according to claim 1, characterized in that: Step S2 specifically includes: The hyper-crosslinked ionic polymer obtained in step S1 is dispersed in ethanol / deionized water containing ethyl cellulose, and a suspension solution is obtained after ultrasonic homogenization. The fabric is immersed in the suspension and stirred, and then taken out and dried to obtain a pretreated fabric, wherein the concentration of the hyper-crosslinked ionic polymer suspension is 0.1-100 g / L, the concentration of the ethanol / deionized water containing ethyl cellulose is 0.1-100 g / L, and the volume ratio of ethanol / deionized water is 1:1-10:

1.

7. The preparation method according to claim 1, characterized in that: Step S3 specifically includes: The pretreated fabric obtained in step S2 is immersed in a polydimethylsiloxane solution for hydrophobic treatment, and the super-hydrophobic fabric after the fabric drying treatment is taken out, wherein the concentration of the polydimethylsiloxane is 0.1 to 100 g / L, and the immersion time is 1 minute to 48 hours.

8. The preparation method according to claim 1, characterized in that: The fabric is one or more of cotton fabric, wool fabric, silk fabric, pure linen fabric, polyester fabric and nylon fabric.

9. A super hydrophobic fabric, characterized in that: It is prepared by the preparation method according to any one of claims 1 to 8.