Preparation method of fluorescent dye for superfine fiber composite material
The fluorescent dye prepared by segmented vacuum heating, crushing, ultrasonication and distillation treatment solves the problem of light color in dyeing of microfiber composites, achieves the improvement of the brightness and color fastness of the material, and uses green and environmentally friendly chemical reagents. Ensure environmental friendliness of production.
Patent Information
- Application Number
- CN202410860003.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During the dyeing process, due to the complementary color luminescence and fiber scattering of existing dyes, the final product has a light and inconspicuous color, which affects the performance and grade of use.
A fluorescent dye preparation method including steps is adopted: firstly, the semi-finished product of the fluorescent dye is obtained by segmented vacuum heating treatment, then pulverized and dispersed in anhydrous ethanol for ultrasonic treatment and centrifugation, and finally, the solvent is removed by distillation to obtain an aqueous solution of the fluorescent dye. and lyophilized to prepare fluorescent dye. The ratio of carbon-containing raw materials and foaming agents used in this method is reasonable to ensure the fluorescent properties of the dye and its binding properties with fibers.
The prepared fluorescent dye has photoluminescent properties and good bonding properties, making the microfiber synthetic material high brightness, bright colors and high color fastness. The whole process uses green and environmentally friendly chemical reagents, making the production process clean and friendly.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of dyeing ultrafine fiber composite materials, and in particular to a method for preparing a fluorescent dye for ultrafine fiber composite materials. Background Art
[0002] Ultrafine fiber composite materials are made of ultrafine fibers with similar structure and properties to the bundled collagen fibers in natural leather, which are made into high-density non-woven fabrics with a three-dimensional mesh structure, and then filled with polyurethane with excellent open microporous structure, and then processed. This ultrafine fiber composite material has the hygienic properties inherent in ultrafine fiber composite natural leather, so it can be comparable to high-grade natural leather in terms of internal microstructure, appearance texture, physical properties and wearing comfort. In addition, ultrafine fiber synthetic leather is superior to natural leather in chemical resistance, quality uniformity, production and processing adaptability, and waterproof and mildew-proof properties. It is used to make bags, clothing, shoes and automotive interiors, etc., and has broad development prospects.
[0003] Due to the fineness of ultrafine fiber composite materials, although the color yield is high during the dyeing process, the existing dyes emit complementary colors and the fibers scatter severely, resulting in the final product being light and dull in color, affecting the performance and grade of the final product. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a method for preparing a fluorescent dye for ultrafine fiber composite materials. The prepared dye has fluorescent properties and can photoluminesce, and the dye has good bonding with the ultrafine fiber composite material, so that the ultrafine fiber synthetic material has high brightness and bright colors.
[0005] The technical solution adopted by the present invention is:
[0006] A method for preparing a fluorescent dye for ultrafine fiber composite materials comprises the following steps:
[0007] (1) weighing a carbon-containing raw material, urea and a foaming agent in proportion, adding distilled water, stirring and dissolving, and mixing uniformly to obtain a reaction raw material solution, placing the solution in a sealed container for segmented vacuum heating treatment to obtain a semi-finished product containing a fluorescent dye;
[0008] (2) crushing the semi-finished product containing the fluorescent dye obtained in step (1), wherein the particle size of the semi-finished product after crushing is less than 10 μm;
[0009] (3) dispersing the semi-finished product containing the fluorescent dye after the pulverization in step (2) in anhydrous ethanol to obtain a suspension, subjecting the suspension to ultrasonic treatment for 10 to 25 minutes, and then subjecting the suspension to centrifugation, and collecting the supernatant after centrifugation to obtain a fluorescent dye ethanol solution;
[0010] (4) placing the fluorescent dye ethanol solution obtained in step (3) into distilled water, stirring sufficiently, and then distilling off the ethanol to obtain a fluorescent dye aqueous solution;
[0011] (5) freeze-drying the fluorescent dye aqueous solution obtained in step (4) to obtain a fluorescent dye for ultrafine fiber composite materials.
[0012] Furthermore, the carbon-containing raw material in step (1) is at least one of tartaric acid, oxalic acid, malic acid and citric acid.
[0013] Furthermore, in step (1), the foaming agent is at least one of calcium chloride, sodium silicate and sodium polyphosphate.
[0014] Furthermore, in the step (1), the mass ratio of the carbon-containing raw material, urea and foaming agent is 1:1-2:0.5-1.
[0015] Furthermore, in step (1), the mass ratio of the total mass of the carbon-containing raw material, urea and foaming agent to the mass ratio of distilled water is 1:3-5.
[0016] Furthermore, the segmented vacuum heating treatment in step (2) is specifically as follows: the heating temperature of the first segment is 80-120°C, and the reaction time is 1-3h; the heating temperature of the second segment is 130-180°C, and the reaction time is 1-3h; the heating temperature of the third segment is 200-260°C, and the reaction time is 1-3h.
[0017] Furthermore, the vacuum degree of the segmented vacuum heating treatment in step (2) is ≤-20 kPa.
[0018] Furthermore, in the step (3), the mass ratio of the semi-finished product containing fluorescent dye to anhydrous ethanol is 1:4-8.
[0019] Furthermore, in step (3), the centrifugal speed is 6000-8000 r / min, and the centrifugal time is 3-10 min.
[0020] Furthermore, in step (4), the distillation temperature is 80-90° C., and the distillation time is 20-30 min.
[0021] The beneficial effects of the present invention are:
[0022] The present invention provides a method for preparing a fluorescent dye for an ultrafine fiber composite material. The prepared dye has fluorescent properties and can emit photoluminescence, and the dye has good binding properties with the ultrafine fiber composite material, so that the ultrafine fiber synthetic material has not only high brightness and bright colors, but also high color fastness. Moreover, the preparation method of the present invention adopts green and environmentally friendly chemical reagents for synthesis, and the entire production process is clean, green and environmentally friendly. DETAILED DESCRIPTION
[0023] The present invention provides a method for preparing a fluorescent dye for an ultrafine fiber composite material. To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0024] Example 1
[0025] This embodiment provides a method for preparing a fluorescent dye for ultrafine fiber composite materials, and the preparation process is as follows:
[0026] (1) Weigh 100 g of tartaric acid, 100 g of urea, and 50 g of calcium chloride, put them into 750 mL of distilled water to prepare a solution, put them into a sealed container for staged vacuum heating treatment, the first stage heating temperature is 80° C., the reaction time is 3 h, the second stage heating temperature is 130° C., the reaction time is 3 h, the third stage heating temperature is 200° C., the reaction time is 3 h, and the vacuum degree is set to -20 kPa during the above three stages of heating treatment to obtain a semi-finished product containing a fluorescent dye;
[0027] (2) collecting and crushing the obtained semi-finished product containing the fluorescent dye, and controlling the crushed particle size to be less than 10 μm;
[0028] (3) dispersing the crushed semi-finished product in anhydrous ethanol to obtain a suspension, wherein the mass ratio of the semi-finished product to the anhydrous ethanol is 1:4, subjecting the suspension to ultrasonic treatment for 25 minutes, and then centrifuging the suspension after ultrasonic treatment in a centrifuge at a centrifugal speed of 6000 r / min for 3 minutes, and collecting the supernatant after centrifugation to obtain a fluorescent dye ethanol solution;
[0029] (4) placing the fluorescent dye ethanol solution into distilled water, stirring thoroughly, and then distilling away the ethanol at a distillation temperature of 90° C. for 30 min to obtain a fluorescent dye aqueous solution;
[0030] (5) Freeze-drying the fluorescent dye aqueous solution to obtain the fluorescent dye for ultrafine fiber composite material.
[0031] After testing, the purity of the fluorescent dye is 95%.
[0032] The ultrafine fiber composite material is dyed with the fluorescent dye. The dyed ultrafine fiber composite material has high brightness and bright color, and its water washing color fastness can reach about level 3.
[0033] Example 2
[0034] This embodiment provides a method for preparing a fluorescent dye for ultrafine fiber composite materials, and the preparation process is as follows:
[0035] (1) Weigh 100 g of oxalic acid, 100 g of urea, and 100 g of sodium silicate, put them into 1200 mL of distilled water to prepare a solution, put them into a sealed container for vacuum heating treatment, the first stage heating temperature is 100° C., the reaction time is 2 h, the second stage heating temperature is 150° C., the reaction time is 2 h, the third stage heating temperature is 220° C., the reaction time is 2 h, and the vacuum degree is set to -30 kPa during the above three stages of heating treatment to obtain a semi-finished product containing a fluorescent dye;
[0036] (2) collecting and crushing the obtained semi-finished product containing the fluorescent dye, and controlling the crushed particle size to be less than 10 μm;
[0037] (3) dispersing the crushed semi-finished product in anhydrous ethanol to obtain a suspension, wherein the mass ratio of the semi-finished product to the anhydrous ethanol is 1:5, subjecting the suspension to ultrasonic treatment for 25 minutes, and then centrifuging the suspension after ultrasonic treatment in a centrifuge at a centrifugal speed of 7000 r / min for 8 minutes, and collecting the supernatant after centrifugation to obtain a fluorescent dye ethanol solution;
[0038] (4) placing the fluorescent dye ethanol solution into distilled water, stirring thoroughly, and then distilling away the ethanol at a distillation temperature of 80° C. for 30 min to obtain a fluorescent dye aqueous solution;
[0039] (5) Freeze-drying the fluorescent dye aqueous solution to obtain the fluorescent dye for ultrafine fiber composite material.
[0040] After testing, the purity of the fluorescent dye is above 95%.
[0041] The ultrafine fiber composite material is dyed with the fluorescent dye. The dyed ultrafine fiber composite material has high brightness and bright color, and its water washing color fastness can reach about level 3.
[0042] Example 3
[0043] This embodiment provides a method for preparing a fluorescent dye for ultrafine fiber composite materials, and the preparation process is as follows:
[0044] (1) Weigh 100 g of malic acid, 200 g of urea, and 100 g of sodium silicate, put them into 1200 mL of distilled water to prepare a solution, put them into a sealed container for vacuum heating treatment, the first stage heating temperature is 110° C., the reaction time is 2 h, the second stage heating temperature is 160° C., the reaction time is 2 h, the third stage heating temperature is 260° C., the reaction time is 1 h, and the vacuum degree is set to -35 kPa during the above three stages of heating treatment to obtain a semi-finished product containing a fluorescent dye;
[0045] (2) collecting and crushing the obtained semi-finished product containing the fluorescent dye, and controlling the crushed particle size to be less than 10 μm;
[0046] (3) dispersing the crushed semi-finished product in anhydrous ethanol to obtain a suspension, the mass ratio of the semi-finished product to anhydrous ethanol being 1:8, subjecting the suspension to ultrasonic treatment for 15 minutes, and then centrifuging the suspension after ultrasonic treatment in a centrifuge at a centrifugal speed of 8000 r / min for 10 minutes, and collecting the supernatant after centrifugation to obtain a fluorescent dye ethanol solution;
[0047] (4) placing the fluorescent dye ethanol solution into distilled water, stirring thoroughly, and then distilling away the ethanol at a distillation temperature of 85° C. for 20 min to obtain a fluorescent dye aqueous solution;
[0048] (5) Freeze-drying the fluorescent dye aqueous solution to obtain the fluorescent dye for ultrafine fiber composite material.
[0049] After testing, the purity of the fluorescent dye is above 95%.
[0050] Example 4
[0051] This embodiment provides a method for preparing a fluorescent dye for ultrafine fiber composite materials, and the preparation process is as follows:
[0052] (1) Weigh 80 g of citric acid, 20 g of oxalic acid, 200 g of urea, 50 g of sodium silicate and 50 g of calcium chloride, put them into 1200 mL of distilled water to prepare a solution, put them into a sealed container for vacuum heating treatment, the first stage heating temperature is 120° C., the reaction time is 2 h, the second stage heating temperature is 180° C., the reaction time is 2 h, the third stage heating temperature is 260° C., the reaction time is 1 h, and the vacuum degree is set to -35 kPa during the three-stage heating treatment to obtain a semi-finished product containing a fluorescent dye;
[0053] (2) collecting and crushing the obtained semi-finished product containing the fluorescent dye, and controlling the crushed particle size to be less than 10 μm;
[0054] (3) dispersing the crushed semi-finished product in anhydrous ethanol to obtain a suspension, the mass ratio of the semi-finished product to anhydrous ethanol being 1:8, subjecting the suspension to ultrasonic treatment for 25 minutes, and then centrifuging the suspension after ultrasonic treatment in a centrifuge at a centrifugal speed of 7000 r / min for 9 minutes, and collecting the supernatant after centrifugation to obtain a fluorescent dye ethanol solution;
[0055] (4) placing the fluorescent dye ethanol solution into distilled water, stirring thoroughly, and then distilling away the ethanol at a distillation temperature of 90° C. for 20 min to obtain a fluorescent dye aqueous solution;
[0056] (5) Freeze-drying the fluorescent dye aqueous solution to obtain the fluorescent dye for ultrafine fiber composite material.
[0057] After testing, the purity of the fluorescent dye is above 95%.
[0058] It should be noted that some parts not described in the present invention can be implemented by adopting or drawing on existing technologies.
[0059] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by technicians in this technical field within the essential scope of the present invention should also fall within the protection scope of the present invention.
Claims
1. A method for preparing a fluorescent dye for ultrafine fiber composite materials, characterized in that: Includes steps: (1) weighing a carbon-containing raw material, urea and a foaming agent in proportion, adding distilled water, stirring and dissolving, and mixing uniformly to obtain a reaction raw material solution, placing the solution in a sealed container for segmented vacuum heating treatment to obtain a semi-finished product containing a fluorescent dye; (2) crushing the semi-finished product containing the fluorescent dye obtained in step (1), wherein the particle size of the semi-finished product after crushing is less than 10 μm; (3) dispersing the semi-finished product containing the fluorescent dye after the pulverization in step (2) in anhydrous ethanol to obtain a suspension, subjecting the suspension to ultrasonic treatment for 10 to 25 minutes, and then subjecting the suspension to centrifugation, and collecting the supernatant after centrifugation to obtain a fluorescent dye ethanol solution; (4) placing the fluorescent dye ethanol solution obtained in step (3) into distilled water, stirring sufficiently, and then distilling off the ethanol to obtain a fluorescent dye aqueous solution; (5) freeze-drying the fluorescent dye aqueous solution obtained in step (4) to obtain a fluorescent dye for ultrafine fiber composite materials.
2. The method for preparing a fluorescent dye for ultrafine fiber composite material according to claim 1, characterized in that: The carbon-containing raw material in step (1) is at least one of tartaric acid, oxalic acid, malic acid and citric acid.
3. The method for preparing a fluorescent dye for ultrafine fiber composite material according to claim 1, characterized in that: In the step (1), the foaming agent is at least one of calcium chloride, sodium silicate and sodium polyphosphate.
4. The method for preparing a fluorescent dye for ultrafine fiber composite material according to claim 1, characterized in that: In the step (1), the mass ratio of the carbon-containing raw material, urea and foaming agent is 1:1-2:0.5-1.
5. The method for preparing a fluorescent dye for ultrafine fiber composite material according to claim 1, characterized in that: In the step (1), the mass ratio of the total mass of the carbon-containing raw material, urea and foaming agent to the mass ratio of distilled water is 1:3-5.
6. The method for preparing a fluorescent dye for ultrafine fiber composite material according to claim 1, characterized in that: The specific staged vacuum heating treatment in step (2) is as follows: the heating temperature of the first stage is 80-120°C, and the reaction time is 1-3h; the heating temperature of the second stage is 130-180°C, and the reaction time is 1-3h; the heating temperature of the third stage is 200-260°C, and the reaction time is 1-3h.
7. The method for preparing a fluorescent dye for ultrafine fiber composite material according to claim 1, characterized in that: The vacuum degree of the segmented vacuum heating treatment in step (2) is ≤-20 kPa.
8. The method for preparing a fluorescent dye for ultrafine fiber composite material according to claim 1, characterized in that: In the step (3), the mass ratio of the semi-finished product containing fluorescent dye to anhydrous ethanol is 1:4-8.
9. The method for preparing a fluorescent dye for ultrafine fiber composite material according to claim 1, characterized in that: In the step (3), the centrifugal speed is 6000-8000 r / min, and the centrifugal time is 3-10 min.
10. The method for preparing a fluorescent dye for ultrafine fiber composite material according to claim 1, characterized in that: In the step (4), the distillation temperature is 80-90° C. and the distillation time is 20-30 min.
Citation Information
Patent Citations
Method for preparing water-soluble fluorescent carbon dots
CN103834397A
Method for selectively detecting concentration of 2,4-DNP in solution system by phosphorus-doped fluorescent carbon dots synthesized through hydrothermal method
CN110174385A
Method for massively preparing panchromatic fluorescent carbon dots and panchromatic fluorescent carbon dots prepared thereof
CN112830475A
Aluminum functionalized fluorescent carbon dot and preparation method and application thereof
CN113150778A
Preparation method of single-matrix white light emitting carbon dot fluorescent powder