Quick-drying type heat sublimation transfer paper and production process thereof
By using bleached coniferous wood pulp and broadleaf wood pulp in thermal sublimation transfer paper to mix with CTMP chemical mechanical pulp and the coordination of specific coatings, the problem of insufficient existing paper mechanics and antibacterial performance is solved, and faster Dry speed and longer service life meet the requirements of fast printing.
Patent Information
- Application Number
- CN202411220003.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-02
AI Technical Summary
The mechanical properties and antibacterial properties of existing fast-drying thermal sublimation transfer papers are insufficient, which affects its service life and quality, and the drying speed is not fast enough to meet the requirements of rapid printing.
Bleached coniferous wood pulp and broadleaf wood pulp are crushed and beaten and mixed with CTMP chemical mechanical pulp, add potassium aluminum sulfate dodecahydrate, wet strength agent, glue sizing agent and functional filler to prepare transfer base paper and on the paper surface Coated top and bottom coatings, combined with antibacterial agents and calcium silicate, improve the mechanical and antibacterial properties of the paper through specific process treatments, while accelerating moisture penetration to improve drying speed.
It significantly improves the mechanical properties and antibacterial properties of thermal sublimation transfer paper, extends the service life, and accelerates the drying speed through the coordinated cooperation of functional fillers and calcium silicate, and meets the needs of rapid printing.
Smart Images

Figure BDA0005022743910000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of transfer paper production, in particular to quick-drying thermal sublimation transfer paper and a production process thereof. Background Art
[0002] Thermal sublimation transfer is a new process that uses an inkjet printer equipped with thermal transfer ink to print portraits, landscapes, texts and other images on thermal sublimation transfer paper in a mirror-reversed manner, and then heats it to about 200°C through thermal transfer equipment. The thermal transfer ink on the thermal sublimation paper will penetrate into the substrate in the form of vaporization, thereby realistically transferring the color of the image on the paper to textiles, porcelain cups, porcelain plates, porcelain boards, metals and other materials.
[0003] In the patent document with application number "CN201710770251.1" and titled "A method for manufacturing fast-drying sublimation paper", a method for manufacturing fast-drying sublimation paper is disclosed, which relates to the manufacturing field of sublimation transfer paper, can solve the contradiction between the transfer rate and the drying speed of the transfer paper, and accelerate the drying speed. The present invention includes the following operating steps: select a base paper with strong water resistance, first apply a sublimation transfer ink-supporting coating on the front of the base paper; then apply a coating on the back of the base paper that is conducive to improving the water absorption of the paper, and the sizing material of the back coating is water + surfactant or water + starch + surfactant, wherein the mass percentage of the surfactant is 0.5%-5%, and the mass percentage of starch is 0.5%-3%.
[0004] Although the thermal sublimation paper manufactured by the above patent document has the advantage of fast drying speed, its mechanical properties and antibacterial properties are relatively insufficient, which shortens its service life to a certain extent and also affects its quality. Based on this, the present invention provides a quick-drying thermal sublimation transfer paper and its production process! Summary of the invention
[0005] The purpose of the present invention is to provide a quick-drying thermal sublimation transfer paper and a production process thereof. The produced thermal sublimation transfer paper not only has excellent mechanical properties but also has good antibacterial properties, and its service life is extended to a certain extent; furthermore, the use of functional fillers can accelerate the penetration of moisture into the interior of the thermal sublimation transfer paper, so that moisture can better pass through the thermal sublimation transfer base paper, thereby accelerating the drying speed of the thermal sublimation transfer base paper, and the functional fillers cooperate with calcium silicate to further improve the drying speed of the thermal sublimation transfer technology, and can better meet the requirements of fast printing.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] In a first aspect, the present invention provides a production process for quick-drying thermal sublimation transfer paper, comprising the following steps:
[0008] Step 1: Put the bleached coniferous wood pulp and the hardwood wood pulp into a pulper respectively, and crush them into bleached coniferous wood pulp and hardwood wood pulp with a concentration of 3-5wt%; then use a series double disc mill to beat them respectively; the bleached coniferous wood pulp and hardwood wood pulp obtained after beating are pumped into a mixing tank at a weight ratio of 1:2-3, and after fully mixing, CTMP chemical mechanical pulp is added, and the mixed pulp is obtained after mechanical mixing;
[0009] Step 2: Pump the mixed slurry into a stainless mixing tank, add potassium aluminum sulfate dodecahydrate, a wet strength agent, a sizing agent and a functional filler thereto in sequence, mix and stir evenly, and then process the obtained composite pulp through purification, screen-mounting, controlled screen dehydration, forming, pressing, surface sizing, drying and soft calendering finishing to obtain transfer base paper; wherein, the addition amounts of potassium aluminum sulfate dodecahydrate, wet strength agent, sizing agent and functional filler are 0.8-3%, 2-4%, 0.2-0.5% and 10-20% of the total mass of the absolute dry slurry, respectively;
[0010] Step 3, coating the front side of the transfer base paper prepared in step 2 with a top coating, and after coating, transferring it to a drying device for drying, and after drying, coating the other side of the transfer base paper with a bottom coating, and then transferring it to a drying device for drying; wherein the solid content of the top coating is 40-45%, and the solid content of the bottom coating is 10-15%;
[0011] The surface coating is made of the following raw materials in parts by weight: 500-600 parts of water, 60-70 parts of sodium carboxymethyl cellulose, 15-20 parts of starch and 10-15 parts of calcium silicate;
[0012] The primer is made of the following raw materials in parts by weight: 60-80 parts of water, 0.5-0.8 parts of antibacterial agent, 80-90 parts of nano zinc oxide, 25-35 parts of sodium carboxymethyl cellulose, and 0.5-1.0 parts of polyamide polyurea resin with a solid content of 40%;
[0013] The adhesive liquid used for adhesive treatment is made of the following raw materials in parts by weight: 90-100 parts of water, 0.5-1.0 parts of sodium carboxymethyl cellulose and 0.8-1.5 parts of antibacterial agent;
[0014] Step 4: convey the transfer paper after coating and drying in step 3 to the back gluing equipment, adjust the paper temperature after back gluing to balance the paper temperature; then go through soft calendering finishing and winding processes in sequence to finally obtain a quick-drying thermal sublimation transfer paper product.
[0015] Furthermore, the beating degrees of the bleached coniferous wood pulp and the hardwood wood pulp are 15-20°SR and 35-40°SR respectively.
[0016] Furthermore, the beating degree of the CTMP chemical mechanical pulp is 22-32°SR, and the dosage thereof is 2-6 times that of the bleached coniferous wood pulp.
[0017] Furthermore, the coniferous wood is any one of masson pine, larch, and spruce; the broad-leaved wood is any one of birch, maple, poplar, and basswood.
[0018] Furthermore, the wet strength agent is selected from any one of polyacrylamide resin, polyethyleneimine resin and epichlorohydrin.
[0019] Furthermore, the coating method is any one of roller coating, metering rod coating, air knife coating, blade coating, and curtain coating.
[0020] Furthermore, the sizing agent is selected from any one of cationic starch, carboxymethyl cellulose, alkyl ketene dimer, alkenyl succinic anhydride, and cationic rosin size.
[0021] Furthermore, the preparation method of the antibacterial agent is as follows: nano titanium dioxide is uniformly dispersed in an ethanol dispersion of 3-aminopropylmethyldioxysilane with a volume concentration of 30-40% at a weight ratio of 20-50 g / L, and then it is transferred to a high-speed disperser and mixed at a speed of 1000-1500 r / min for 10-15 minutes; after the mixing is completed, it is washed and dried in turn, and the obtained solid material is put into anhydrous ethanol at a solid-liquid ratio of 50-80 g / L, and then 3-methoxy-4-hydroxybenzaldehyde with a mass of 10-20% of the solid material is added, and the reaction is stirred at a temperature of 40-50° C. for 3-5 hours; after the reaction is completed, the obtained product components are filtered, washed and dried in turn, and the final product is the antibacterial agent.
[0022] Furthermore, the functional filler is compounded by montmorillonite, talcum powder, microcrystalline cellulose and chitosan in a mass ratio of 1:2-4:0.2-0.5:0.6-0.8.
[0023] In a second aspect, the present invention provides a quick-drying thermal sublimation transfer paper, which is produced by the production process described above.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1. The present invention adopts 3-aminopropylmethyldioxysilane to modify nano titanium dioxide so that the two are bonded by chemical bonds, and finally 3-aminopropylmethyldioxysilane is successfully grafted on the surface of nano titanium dioxide to obtain solid materials. The obtained solid materials are put into absolute ethanol, and then 3-methoxy-4-hydroxybenzaldehyde is added thereto, and the relevant active groups on the surface of 3-methoxy-4-hydroxybenzaldehyde and nano titanium dioxide are chemically reacted by stirring reaction, and finally 3-methoxy-4-hydroxybenzaldehyde is successfully grafted on the surface of nano titanium dioxide. Under the synergistic cooperation of nano titanium dioxide and 3-methoxy-4-hydroxybenzaldehyde, the prepared antibacterial agent has excellent antibacterial properties, and the use of the antibacterial agent can effectively improve the antibacterial properties of thermal sublimation transfer paper, and prolong its service life to a certain extent.
[0026] 2. The functional filler provided by the present invention can accelerate the penetration of moisture into the interior of the thermal sublimation transfer paper, allowing moisture to better pass through the thermal sublimation transfer base paper, thereby accelerating the drying speed of the thermal sublimation transfer base paper. It cooperates with calcium silicate to further improve the drying speed of the thermal sublimation transfer technology, and can better meet the requirements of fast printing. DETAILED DESCRIPTION
[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] Example 1
[0029] A production process for quick-drying thermal sublimation transfer paper comprises the following steps:
[0030] Step 1: Put the bleached coniferous wood pulp and the hardwood wood pulp into a pulper respectively, and crush them into bleached coniferous wood pulp and hardwood wood pulp with a concentration of 3wt%; then use a series double disc mill to beat them respectively; the bleached coniferous wood pulp and hardwood wood pulp obtained after beating are pumped into a mixing tank at a weight ratio of 1:2, and CTMP chemical mechanical pulp is added after being fully mixed, and mixed mechanically to obtain a mixed pulp;
[0031] The beating degrees of the bleached coniferous wood pulp and the hardwood wood pulp are 15°SR and 35°SR respectively.
[0032] The beating degree of CTMP chemical mechanical pulp is 22°SR, and its dosage is twice that of bleached softwood pulp; the softwood is masson pine; the hardwood is birch;
[0033] Step 2: Pump the mixed slurry into a stainless mixing tank, add potassium aluminum sulfate dodecahydrate, a wet strength agent, a sizing agent and a functional filler thereto in sequence, mix and stir evenly, and then process the obtained composite pulp through purification, screen-mounting, controlled screen dehydration, forming, pressing, surface sizing, drying and soft calendering finishing to obtain transfer base paper; wherein, the addition amounts of potassium aluminum sulfate dodecahydrate, wet strength agent, sizing agent and functional filler are 0.8%, 2%, 0.2% and 10% of the total mass of the absolute dry slurry, respectively;
[0034] The wet strength agent is polyacrylamide resin; the coating method is roller coating; the sizing agent is cationic starch; the functional filler is made of montmorillonite, talcum powder, microcrystalline cellulose and chitosan in a mass ratio of 1:2:0.2:0.6;
[0035] Step 3, coating the front side of the transfer base paper prepared in step 2 with a top coating, and after coating, transferring it to a drying device for drying, and after drying, coating the other side of the transfer base paper with a bottom coating, and then transferring it to a drying device for drying; wherein the solid content of the top coating is 40%, and the solid content of the bottom coating is 10%;
[0036] The surface coating is made of the following raw materials in parts by weight: 500 parts of water, 60 parts of sodium carboxymethyl cellulose, 15 parts of starch and 10 parts of calcium silicate;
[0037] The bottom coating is made of the following raw materials in parts by weight: 60 parts of water, 0.5 parts of antibacterial agent, 80 parts of nano zinc oxide, 25 parts of sodium carboxymethyl cellulose, and 0.5 parts of polyamide polyurea resin with a solid content of 40%;
[0038] The adhesive solution used for adhesive treatment is made of the following raw materials in parts by weight: 90 parts of water, 0.5 parts of sodium carboxymethyl cellulose and 0.8 parts of antibacterial agent;
[0039] Step 4: convey the transfer paper after coating and drying in step 3 to the back gluing equipment, adjust the paper temperature after back gluing to balance the paper temperature; then go through soft calendering finishing and winding processes in sequence to finally obtain a quick-drying thermal sublimation transfer paper product.
[0040] The preparation method of the antibacterial agent is as follows: nano titanium dioxide is uniformly dispersed in an ethanol dispersion of 3-aminopropylmethyldioxysilane with a volume concentration of 30% at a weight ratio of 20g / L, and then it is transferred to a high-speed disperser and mixed at a speed of 1000r / min for 10min; after the mixing is completed, it is washed and dried in turn, the obtained solid material is put into anhydrous ethanol at a solid-liquid ratio of 50g / L, and then 3-methoxy-4-hydroxybenzaldehyde with a mass of 10% of the solid material is added, and the reaction is stirred at a temperature of 40°C for 3h; after the reaction is completed, the obtained product components are filtered, washed and dried in turn, and the final product is the antibacterial agent.
[0041] Example 2
[0042] A production process for quick-drying thermal sublimation transfer paper comprises the following steps:
[0043] Step 1: Put the bleached coniferous wood pulp and the hardwood wood pulp into a pulper respectively, and crush them into bleached coniferous wood pulp and hardwood wood pulp with a concentration of 4wt%; then use a series double disc mill to beat them respectively; the bleached coniferous wood pulp and hardwood wood pulp obtained after beating are pumped into a mixing tank at a weight ratio of 1:2.5, and after fully mixing, CTMP chemical mechanical pulp is added, and the mixed pulp is obtained after mechanical mixing;
[0044] The beating degrees of the bleached softwood pulp and hardwood pulp are 20°SR and 40°SR respectively;
[0045] The beating degree of CTMP chemical mechanical pulp is 28°SR, and its dosage is 4 times that of bleached softwood pulp; the softwood is larch; the hardwood is maple;
[0046] Step 2: Pump the mixed slurry into a stainless mixing tank, add potassium aluminum sulfate dodecahydrate, wet strength agent, sizing agent and functional filler thereto in sequence, mix and stir evenly, and then process the obtained composite pulp through purification, screen-mounting, controlled screen dehydration, forming, pressing, surface sizing, drying and soft calendering finishing to obtain transfer base paper; wherein, the addition amounts of potassium aluminum sulfate dodecahydrate, wet strength agent, sizing agent and functional filler are 2%, 3%, 0.4% and 15% of the total mass of the absolute dry slurry, respectively;
[0047] The wet strength agent is polyethyleneimine resin; the coating method is metering rod coating; the sizing agent is carboxymethyl cellulose; the functional filler is made of montmorillonite, talcum powder, microcrystalline cellulose and chitosan in a mass ratio of 1:3:0.4:0.7;
[0048] Step 3, coating the front side of the transfer base paper prepared in step 2 with a top coating, and after coating, transferring it to a drying device for drying, and after drying, coating the other side of the transfer base paper with a bottom coating, and then transferring it to a drying device for drying; wherein the solid content of the top coating is 40%, and the solid content of the bottom coating is 10%;
[0049] The surface coating is made of the following raw materials in parts by weight: 550 parts of water, 65 parts of sodium carboxymethyl cellulose, 15 parts of starch and 10 parts of calcium silicate;
[0050] The bottom coating is made of the following raw materials in parts by weight: 70 parts of water, 0.6 parts of antibacterial agent, 85 parts of nano zinc oxide, 30 parts of sodium carboxymethyl cellulose, and 0.8 parts of polyamide polyurea resin with a solid content of 40%;
[0051] The adhesive solution used for adhesive treatment is made of the following raw materials in parts by weight: 95 parts of water, 0.8 parts of sodium carboxymethyl cellulose and 1.2 parts of antibacterial agent;
[0052] Step 4: convey the transfer paper after coating and drying in step 3 to the back gluing equipment, adjust the paper temperature after back gluing to balance the paper temperature; then go through soft calendering finishing and winding processes in sequence to finally obtain a quick-drying thermal sublimation transfer paper product.
[0053] The preparation method of the antibacterial agent is as follows: nano titanium dioxide is uniformly dispersed in an ethanol dispersion of 3-aminopropylmethyldioxysilane with a volume concentration of 35% at a weight ratio of 40g / L, and then it is transferred to a high-speed disperser and mixed at a speed of 1200r / min for 15min; after the mixing is completed, it is washed and dried in turn, the obtained solid material is put into anhydrous ethanol at a solid-liquid ratio of 60g / L, and then 3-methoxy-4-hydroxybenzaldehyde with a mass of 15% of the solid material is added, and the reaction is stirred at a temperature of 45°C for 4h; after the reaction is completed, the obtained product components are filtered, washed and dried in turn, and the final product is the antibacterial agent.
[0054] Example 3
[0055] A production process for quick-drying thermal sublimation transfer paper comprises the following steps:
[0056] Step 1: Put the bleached coniferous wood pulp and the hardwood wood pulp into a pulper respectively, and crush them into bleached coniferous wood pulp and hardwood wood pulp with a concentration of 5wt%; then use a series double disc mill to beat them respectively; the bleached coniferous wood pulp and hardwood wood pulp obtained after beating are pumped into a mixing tank at a weight ratio of 1:3, and after fully mixing, CTMP chemical mechanical pulp is added, and the mixed pulp is obtained after mechanical mixing;
[0057] The beating degrees of the bleached coniferous wood pulp and the hardwood wood pulp are 20°SR and 40°SR respectively.
[0058] The beating degree of CTMP chemical mechanical pulp is 32°SR, and its dosage is 6 times that of bleached softwood pulp; the softwood is spruce; the hardwood is poplar;
[0059] Step 2: Pump the mixed slurry into a stainless mixing tank, add potassium aluminum sulfate dodecahydrate, wet strength agent, sizing agent and functional filler thereto in sequence, mix and stir evenly, and then process the obtained composite pulp through purification, screen-mounting, controlled screen dehydration, forming, pressing, surface sizing, drying and soft calendering finishing to obtain transfer base paper; wherein, the addition amounts of potassium aluminum sulfate dodecahydrate, wet strength agent, sizing agent and functional filler are 3%, 4%, 0.5% and 20% of the total mass of the absolute dry slurry respectively;
[0060] Among them, epichlorohydrin is used as wet strength agent; air knife coating is used as coating method; alkyl ketene dimer is used as sizing agent; functional filler is compounded by montmorillonite, talcum powder, microcrystalline cellulose and chitosan in a mass ratio of 1:4:0.5:0.8;
[0061] Step 3, coating the front side of the transfer base paper prepared in step 2 with a top coating, and after coating, transferring it to a drying device for drying, and after drying, coating the other side of the transfer base paper with a bottom coating, and then transferring it to a drying device for drying; wherein the solid content of the top coating is 45%, and the solid content of the bottom coating is 15%;
[0062] The surface coating is made of the following raw materials in parts by weight: 600 parts of water, 70 parts of sodium carboxymethyl cellulose, 20 parts of starch and 15 parts of calcium silicate;
[0063] The primer is made of the following raw materials in parts by weight: 80 parts of water, 0.8 parts of antibacterial agent, 90 parts of nano zinc oxide, 35 parts of sodium carboxymethyl cellulose, and 1.0 parts of polyamide polyurea resin with a solid content of 40%;
[0064] The adhesive solution used for adhesive treatment is made of the following raw materials in parts by weight: 100 parts of water, 1.0 parts of sodium carboxymethyl cellulose and 1.5 parts of antibacterial agent;
[0065] Step 4: convey the transfer paper after coating and drying in step 3 to the back gluing equipment, adjust the paper temperature after back gluing to balance the paper temperature; then go through soft calendering finishing and winding processes in sequence to finally obtain a quick-drying thermal sublimation transfer paper product.
[0066] The preparation method of the antibacterial agent is as follows: nano titanium dioxide is uniformly dispersed in an ethanol dispersion of 3-aminopropylmethyldioxysilane with a volume concentration of 40% at a weight ratio of 50g / L, and then the dispersion is transferred to a high-speed disperser and mixed at a speed of 1500r / min for 15min; after the mixing is completed, the dispersion is washed and dried in turn, the obtained solid material is put into anhydrous ethanol at a solid-liquid ratio of 80g / L, and then 3-methoxy-4-hydroxybenzaldehyde with a mass of 20% of the solid material is added, and the reaction is stirred at a temperature of 50°C for 5h; after the reaction is completed, the obtained product components are filtered, washed and dried in turn, and the final product is the antibacterial agent.
[0067] Performance test: The relevant properties (including mechanical properties, transfer properties and antibacterial properties) of the thermal sublimation transfer paper samples provided in Examples 1 to 3 were tested respectively, and the test data obtained were recorded in the following table:
[0068]
[0069] By comparing and analyzing the relevant data in the table, it can be seen that the thermal sublimation transfer paper produced by the present invention not only has excellent mechanical properties but also has good antibacterial properties, which prolongs its service life to a certain extent; furthermore, the use of functional fillers can accelerate the penetration of moisture into the interior of the thermal sublimation transfer paper, so that moisture can better pass through the thermal sublimation transfer base paper, thereby accelerating the drying speed of the thermal sublimation transfer base paper, and it cooperates with calcium silicate to further improve the drying speed of the thermal sublimation transfer technology, which can better meet the requirements of fast printing. This shows that the quick-drying thermal sublimation transfer paper and its production process provided by the present invention have a broader market prospect and are more suitable for promotion.
[0070] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0071] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A production process for quick-drying thermal sublimation transfer paper, characterized in that: The following steps are involved: Step 1: Put the bleached coniferous wood pulp and the hardwood wood pulp into a pulper respectively, and crush them into bleached coniferous wood pulp and hardwood wood pulp with a concentration of 3-5wt%; then use a series double disc mill to beat them respectively; the bleached coniferous wood pulp and hardwood wood pulp obtained after beating are pumped into a mixing tank at a weight ratio of 1:2-3, and after fully mixing, CTMP chemical mechanical pulp is added, and the mixed pulp is obtained after mechanical mixing; Step 2: Pump the mixed slurry into a stainless mixing tank, add potassium aluminum sulfate dodecahydrate, a wet strength agent, a sizing agent and a functional filler thereto in sequence, mix and stir evenly, and then process the obtained composite pulp through purification, screen-mounting, controlled screen dehydration, forming, pressing, surface sizing, drying and soft calendering finishing to obtain transfer base paper; wherein, the addition amounts of potassium aluminum sulfate dodecahydrate, wet strength agent, sizing agent and functional filler are 0.8-3%, 2-4%, 0.2-0.5% and 10-20% of the total mass of the absolute dry slurry, respectively; Step 3, coating the front side of the transfer base paper prepared in step 2 with a top coating, and after coating, transferring it to a drying device for drying, and after drying, coating the other side of the transfer base paper with a bottom coating, and then transferring it to a drying device for drying; wherein the solid content of the top coating is 40-45%, and the solid content of the bottom coating is 10-15%; The surface coating is made of the following raw materials in parts by weight: 500-600 parts of water, 60-70 parts of sodium carboxymethyl cellulose, 15-20 parts of starch and 10-15 parts of calcium silicate; The primer is made of the following raw materials in parts by weight: 60-80 parts of water, 0.5-0.8 parts of antibacterial agent, 80-90 parts of nano zinc oxide, 25-35 parts of sodium carboxymethyl cellulose, and 0.5-1.0 parts of polyamide polyurea resin with a solid content of 40%; The adhesive liquid used for adhesive treatment is made of the following raw materials in parts by weight: 90-100 parts of water, 0.5-1.0 parts of sodium carboxymethyl cellulose and 0.8-1.5 parts of antibacterial agent; Step 4: convey the transfer paper after coating and drying in step 3 to the back gluing equipment, adjust the paper temperature after back gluing to balance the paper temperature; then go through soft calendering finishing and winding processes in sequence to finally obtain a quick-drying thermal sublimation transfer paper product.
2. The production process of a quick-drying thermal sublimation transfer paper according to claim 1, characterized in that: The beating degrees of the bleached coniferous wood pulp and the broadleaved wood pulp are 15-20°SR and 35-40°SR respectively.
3. The production process of a quick-drying thermal sublimation transfer paper according to claim 1, characterized in that: The beating degree of the CTMP chemical mechanical pulp is 22-32°SR, and the dosage thereof is 2-6 times that of the bleached coniferous wood pulp.
4. The production process of a quick-drying thermal sublimation transfer paper according to claim 1, characterized in that: The coniferous wood is any one of masson pine, larch and spruce; the broad-leaved wood is any one of birch, maple, poplar and basswood.
5. The production process of a quick-drying thermal sublimation transfer paper according to claim 1, characterized in that: The wet strength agent is selected from any one of polyacrylamide resin, polyethyleneimine resin and epichlorohydrin.
6. The production process of a quick-drying thermal sublimation transfer paper according to claim 1, characterized in that: The coating method can be any one of roller coating, metering rod coating, air knife coating, blade coating and curtain coating.
7. The production process of a quick-drying thermal sublimation transfer paper according to claim 1, characterized in that: The sizing agent is selected from any one of cationic starch, carboxymethyl cellulose, alkyl ketene dimer, alkenyl succinic anhydride and cationic rosin size.
8. The production process of a quick-drying thermal sublimation transfer paper according to claim 1, characterized in that: The preparation method of the antibacterial agent is as follows: nano titanium dioxide is uniformly dispersed in an ethanol dispersion of 3-aminopropylmethyldioxysilane with a volume concentration of 30-40% at a weight ratio of 20-50 g / L, and then the dispersion is transferred into a high-speed disperser and mixed at a speed of 1000-1500 r / min for 10-15 minutes; after the mixing is completed, the dispersion is washed and dried in sequence, the obtained solid material is put into anhydrous ethanol at a solid-liquid ratio of 50-80 g / L, and then 3-methoxy-4-hydroxybenzaldehyde with a mass of 10-20% of the solid material is added, and the reaction is stirred at a temperature of 40-50°C for 3-5 hours; after the reaction is completed, the obtained product components are filtered, washed and dried in sequence, and the final product is the antibacterial agent.
9. The production process of a quick-drying thermal sublimation transfer paper according to claim 1, characterized in that: The functional filler is prepared by compounding montmorillonite, talcum powder, microcrystalline cellulose and chitosan in a mass ratio of 1:2-4:0.2-0.5:0.6-0.
8.
10. A quick-drying thermal sublimation transfer paper, characterized in that: The quick-drying thermal sublimation transfer paper is prepared by the production process of any one of claims 1 to 9.
Citation Information
Patent Citations
Method for making raw paper of heat sublimation transfer printing paper
CN102767120A
Quick-drying type digital thermal dye sublimation transfer paper
CN106626856A
Coating-free ink jet heat sublimation transfer paper and preparation method thereof
CN106758513A
Thermal dye sublimation transfer paper suitable for on-line high-speed production
CN108894053A
Thermal dye sublimation transfer paper and production process thereof
CN114737413A