Characterization method of asphalt-aggregate interface fatigue performance

Through the direct tensile test method, the dynamic modulus and phase angle are calculated, and the fatigue life of the asphalt-aggregate interface is iteratively calculated, which solves the problem of insufficient fatigue performance characterization in the prior art, and improves the accuracy and reliability of the test. Suitable for practical engineering applications.

CN118937067APending Publication Date: 2024-11-12SOUTHEAST UNIV
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411028036.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is difficult to effectively characterize the fatigue performance of the asphalt-aggregate interface, resulting in poor accuracy of the test results and lack of reliable evaluation methods and indicators, making it difficult to refer to in actual engineering.

Method used

Using a method based on direct tensile test, the asphalt-aggregate test is prepared, the device is fixed and loaded, fatigue test is performed, dynamic modulus and phase angle are calculated, and the fatigue life is iteratively calculated as a characterization index of the interface tensile strength.

Benefits of technology

It improves the fatigue performance characterization effect of the asphalt-aggregate interface, provides reliable quantitative indicators, enhances the repeatability and prediction accuracy of the experiment, conforms to the real load form, and makes up for the gap in the existing technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118937067A_ABST
    Figure CN118937067A_ABST
Patent Text Reader

Abstract

The invention discloses a characterization method of asphalt-aggregate interface fatigue performance. The characterization method comprises the following steps: S1, preparing an asphalt-aggregate test piece; s2, fixing the asphalt-aggregate test piece; s3, asphalt-aggregate interface fatigue performance testing is carried out, brake displacement data, tension sensor data and phase angle data are collected in real time according to a data collection period, and stress and strain of an asphalt film are calculated; and S4, calculating the dynamic modulus, and iteratively solving the fatigue life of the asphalt film based on the crack propagation speed and the relationship between the dynamic modulus and the phase angle, thereby completing the asphalt-aggregate interface tensile strength test. Therefore, by taking the basic attributes of the asphalt material such as the dynamic modulus and the phase angle as a starting point, a fatigue performance quantitative characterization index, namely the fatigue life of the asphalt-aggregate interface, is provided, the fatigue performance of the interface can be reflected most intuitively, and the tensile strength characterization effect of the asphalt-aggregate interface is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of indoor testing of asphalt pavement interface adhesion fatigue performance, and in particular to a method for characterizing asphalt-aggregate interface fatigue performance. Background Art

[0002] Expressways are the lifeline of transportation throughout the country. Compared with gravel and cement concrete pavements, asphalt pavements have the characteristics of good shock absorption, high safety, low noise, and simple maintenance. They are widely used in the construction of high-grade roads.

[0003] During the construction and maintenance process, cracking, looseness and potholes are the main defects that lead to structural or functional degradation of asphalt pavements and pose a serious threat to driver safety. Most cracks in asphalt pavements originate from micro-damage in the asphalt-aggregate interface area, which is the part most susceptible to failure. Further studies have shown that cracking of asphalt mixtures may occur at the asphalt-aggregate interface or within the asphalt film, leading to debonding. In fact, asphalt debonding occurs mainly due to repeated loads. Under repeated loads less than the tensile strength of the interface, fatigue damage occurs at the asphalt-aggregate interface, which slowly develops into cracks and finally presents itself in the form of cracking, looseness, slippage and other defects.

[0004] There have been many studies on the adhesion performance between asphalt and aggregate interfaces, but there is a lack of research on the fatigue performance of asphalt-aggregate interfaces. Many standard tests are used to evaluate the adhesion / debonding behavior between asphalt and aggregate, including direct tensile tests, surface energy tests, water boiling tests, immersion tests, etc. For fatigue performance tests, the majority of the research objects are asphalt mixtures or individual asphalt materials, usually using mechanical strength such as tensile strength and shear strength or energy such as surface energy and binding energy as indicators. Such as direct tensile tests, dynamic shear tests, indirect tensile fatigue tests, and surface free energy tests, most of the above tests characterize fatigue performance by applying simple forms of cyclic loads, such as triangular cyclic waves, or based on indirect indicators such as energy.

[0005] However, the current direct tensile test research object is the asphalt mixture as a whole, and it is impossible to characterize the fatigue performance of the asphalt-aggregate interface. Since the physical scale of the asphalt-aggregate interface is small and difficult to observe, it is often confused in the asphalt mixture, and the actual load form of the vehicle is difficult to reproduce. There is a problem of ignoring the performance characterization of the asphalt-aggregate interface, which is the most prone to failure, and the problem of difficult to control the load form; on the other hand, tests such as dynamic shear tests and surface free energy methods are limited by complex operations, and the preparation of asphalt mixture specimens cannot be completely consistent every time, resulting in poor prediction results. Inaccuracy, lack of quantitative indicators of fatigue performance, lack of reliable methods and indicators for evaluating the fatigue performance of the asphalt-aggregate interface, make the test results difficult to be referenced by actual projects. Summary of the invention

[0006] The purpose of the present invention is to solve the problem of insufficient characterization of fatigue performance of asphalt-aggregate interface indoors, and to provide a method and index for characterizing fatigue performance of asphalt-aggregate interface based on direct tensile test.

[0007] In order to achieve the above technical objectives, the present invention will adopt the following technical solutions:

[0008] A method for characterizing fatigue performance of asphalt-aggregate interface comprises the following steps:

[0009] Step S1: asphalt-aggregate specimen preparation;

[0010] After the aggregate specimen is prepared, the area to be tested is marked on the surface of the aggregate specimen, and an asphalt coating area is set within the area to be tested, and then cold asphalt is evenly coated on the asphalt coating area to the target asphalt film thickness, so that an asphalt-aggregate specimen that meets the requirements can be prepared;

[0011] Step S2: asphalt-aggregate specimen fixing;

[0012] Loading the asphalt-aggregate specimen prepared in step S1 into an asphalt-aggregate interface fatigue test fixing and loading device;

[0013] The asphalt-aggregate interface fatigue test fixing and loading device comprises a fixture table, a lifting platform, a pull rod and a stainless steel metal pressure head; the fixture table is installed above the lifting platform in a liftable manner, and the stainless steel metal pressure head is suspended above the fixture table through the pull rod; the stainless steel metal pressure head can move toward / away from the fixture table under the drive of the pull rod;

[0014] The asphalt-aggregate specimen is loaded through a fixture table, and the area to be tested on the asphalt-aggregate specimen is located directly below the stainless steel metal pressure head;

[0015] Step S3: asphalt-aggregate interface fatigue performance test;

[0016] After the asphalt-aggregate specimens are cured at 20°C for a period of time, the asphalt-aggregate interface fatigue test fixing and loading device is started, and according to the preset direct tensile fatigue program, the asphalt-aggregate interface fatigue performance test is carried out by driving the stainless steel metal pressure head to repeatedly stretch and restore the test area of ​​the asphalt-aggregate specimen, and the brake displacement data, tension sensor data, and phase angle data are collected in real time according to the data collection cycle, and the stress and strain of the asphalt film are calculated respectively according to the collected brake displacement data and tension sensor data;

[0017] Step S4: characterization of fatigue performance of asphalt-aggregate interface;

[0018] According to the stress and strain of the asphalt film calculated in step S3, the dynamic modulus is calculated. Then, based on the relationship between the crack growth rate, dynamic modulus and phase angle, the fatigue life Nf of the asphalt film can be iteratively calculated, thereby completing the asphalt-aggregate interface tensile strength test.

[0019] Preferably, in step S2, the fixture table has a specimen accommodating cavity; the outer dimensions of the asphalt-aggregate specimen match the inner wall shape of the specimen accommodating cavity; the asphalt-aggregate specimen is placed in the specimen accommodating cavity and is locked by fixing bolts configured on the cavity wall of the specimen accommodating cavity.

[0020] Preferably, in step S1, the area to be tested and the asphalt coating area are both circular and overlap each other, and the size of the stainless steel metal pressure head is equal to the size of the asphalt coating area.

[0021] Preferably, in step S1, the asphalt-aggregate specimen is prepared by:

[0022] Step S1.1, preparing aggregate specimens and determining target asphalt film thickness:

[0023] The rock is cored and cut to obtain cylindrical aggregate specimens, and the mass of cold asphalt required for the test is calculated and weighed according to the determined target asphalt film thickness:

[0024] m=πr 2 hρ(T)

[0025] Where: m-bitumen weight; r-bitumen film radius; h-bitumen film thickness; ρ(T)-bitumen density; T-test temperature;

[0026] Step S1.2, washing the surface of the polished aggregate specimen with distilled water to remove dust and impurities;

[0027] Step S1.3, marking the area to be tested on the surface of the aggregate specimen to match the circular bottom surface of the stainless steel metal indenter;

[0028] Step S1.4, drying the moisture on the surface of the aggregate specimen and maintaining the surface temperature of the aggregate specimen;

[0029] Step S1.5: At the middle position of the test area marked on the surface of the aggregate specimen, select an area with a radius of r as the asphalt coating area, and use a stainless steel metal press to evenly apply asphalt with a weight of m on the asphalt coating area to obtain an asphalt-aggregate specimen with a target asphalt film thickness.

[0030] Preferably, in step S2, the asphalt-aggregate specimen is fixed by the following steps:

[0031] Step S2.1, assembling the stainless steel metal pressing head under the pulling rod;

[0032] Step S2.2, raising the lifting platform to drive the fixture table to rise, so that the fixing bolts arranged around the fixture table are aligned with the middle position of the asphalt-aggregate specimen;

[0033] Step S2.3, tighten the fixing bolts in diagonal order to lock the asphalt-aggregate specimen;

[0034] Step S2.4, zeroing the pressure sensor of the lifting platform.

[0035] Preferably, in step S2, the asphalt-aggregate interface fatigue test fixing and loading device used is a DTS-30 servo hydraulic dynamic testing system.

[0036] Preferably, in step S3, the asphalt-aggregate interface fatigue performance test specifically includes the following steps:

[0037] Step S3.1, maintaining the operating box temperature of the DTS-30 servo hydraulic dynamic testing system at 20°C to cure the asphalt-aggregate specimen for 40 minutes to ensure that the interface forms a stable strength;

[0038] Step S3.2, setting a direct tensile fatigue program, setting the control strain form to a half-haversine waveform, optionally, the waveform amplitude is 5% of the asphalt film thickness, the loading width is 1000 ms, the frequency is 1 Hz, and the stop condition is reaching 5% of the peak load;

[0039] Step S3.3, collecting brake displacement data, tension sensor data, and phase angle data;

[0040] Step S3.4, processing test data:

[0041] The strain of the asphalt film was calculated according to the following formula:

[0042]

[0043] ε-strain of asphalt film; ΔL-displacement of brake; h-thickness of asphalt film;

[0044] The stress of the asphalt membrane is calculated according to the following formula:

[0045]

[0046] σ-stress, MPa; c-bitumen film radius; F-tension.

[0047] The method for characterizing fatigue performance of asphalt-aggregate interface according to claim 1 is characterized in that, in step S4, the characterization of fatigue performance of asphalt-aggregate interface is specifically obtained by the following steps:

[0048] S4.1: Based on the stress and strain data, take the ratio and plot the dynamic modulus The dynamic modulus of the first cycle is taken as the initial modulus.

[0049] S4.2: Draw the phase angle according to the phase angle data output by DTS-30 The curve with the number of loading times, the phase angle of the first cycle is taken as the initial phase angle

[0050] S4.3: According to the energy balance principle of the entire volume of the cylindrical specimen, in the Nth loading cycle, the dissipated strain energy DSE based on the damage configuration is A and the dissipated strain energy DSE of the undamaged configuration T Equivalently, the calculation formula for the crack length under the tensile load mode is derived:

[0051]

[0052] S4.4: Based on the Paris law of fracture mechanics, establish the power function relationship between crack growth rate and stress intensity factor;

[0053] S4.5. Based on the relationship between crack growth rate, dynamic modulus and phase angle, using mathematical processing software, the integral of both sides of the formula is as follows:

[0054]

[0055] By iterative solution, the fatigue life Nf of the asphalt-aggregate interface is obtained, which is the characterization index of the fatigue performance of the asphalt-aggregate interface.

[0056] Based on the above technical objectives, the present invention has the following advantages over the prior art:

[0057] 1. The characterization method of fatigue performance of asphalt-aggregate interface proposed in the present invention focuses on fatigue debonding, the weakest link in asphalt mixture, i.e. fatigue debonding failure of asphalt-aggregate interface. Different from the existing fatigue research of asphalt materials which mainly focuses on tensile or shear fatigue failure of asphalt or asphalt mixture, the fatigue performance characterization method of interface failure is proposed, which fills the existing gap.

[0058] 2. The characterization method of fatigue performance of asphalt-aggregate interface proposed in the present invention is based on the basic properties of asphalt materials such as dynamic modulus and phase angle, and proposes a quantitative characterization index of fatigue performance based on the dissipated strain energy balance, namely, the fatigue life of asphalt-aggregate interface, which can most intuitively reflect the fatigue performance of the interface and improve the tensile strength characterization effect of asphalt-aggregate interface. It is different from the traditional tensile or shear fatigue test, which lasts until failure and lacks mechanism analysis;

[0059] 3. The characterization method of fatigue performance of asphalt-aggregate interface proposed in the present invention can control the thickness of asphalt film only by controlling the quality of asphalt. The test has high repeatability and low relative error. Compared with fatigue test, the prediction effect is good and it can basically reflect the fatigue performance of the real asphalt-aggregate interface.

[0060] 4. The method for characterizing fatigue performance of asphalt-aggregate interface proposed in the present invention is simple to operate, and the loading form for controlling strain is easy to control. In particular, the half-positive vector wave is more consistent with the form of actual vehicle load acting on the road surface. BRIEF DESCRIPTION OF THE DRAWINGS

[0061] Figure 1 Flow chart of the method for characterizing fatigue performance of asphalt-aggregate interface;

[0062] Figure 2 It is a fixing and loading device for asphalt-aggregate interface fatigue test in the present invention;

[0063] Among them are: A. Pull rod; B. Stainless steel metal pressure head; C. Asphalt membrane; D. Aggregate; E. Clamp table; F. Fixing bolts; G. Lifting platform.

[0064] Figure 3 is the curve of dynamic modulus changing with loading times;

[0065] Figure 4 is the curve of phase angle changing with loading times;

[0066] Figure 5 This is the curve showing the variation of crack length with loading times. DETAILED DESCRIPTION

[0067] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means any limitation to the present invention and its application or use. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise specified, the relative arrangement, expressions and numerical values ​​of the components and steps described in these embodiments do not limit the scope of the present invention. The techniques, methods and equipment known to ordinary technicians in the relevant fields may not be discussed in detail, but in appropriate cases, the techniques, methods and equipment should be regarded as part of the specification. In all examples shown and discussed here, any specific value should be interpreted as merely exemplary, rather than as a limitation. Therefore, other examples of the exemplary embodiments may have different values.

[0068] Embodiment 1

[0069] See also Figure 1 According to the process of the embodiment of the invention, the method includes the following steps:

[0070] 1. Preparation of asphalt-aggregate specimens;

[0071] 2. Fixing of asphalt-aggregate specimens;

[0072] 3. Asphalt-aggregate interface fatigue performance test;

[0073] 4. Characterization of fatigue performance of asphalt-aggregate interface;

[0074] See also Figure 2 , the asphalt-aggregate specimen fixing process according to the embodiment of the present invention is the main test device.

[0075] See also Figure 3 , during the characterization of fatigue performance of the asphalt-aggregate interface according to an embodiment of the present invention, a functional relationship between the dynamic modulus and the number of loading times is obtained.

[0076] See also Figure 4 , according to the asphalt-aggregate interface fatigue performance characterization process of an embodiment of the present invention, the functional relationship between the phase angle and the number of loading times is obtained.

[0077] See also Figure 5 , during the characterization of fatigue performance of the asphalt-aggregate interface according to an embodiment of the present invention, a functional relationship between crack length and loading times is obtained.

[0078] The above scheme of the present invention is based on an asphalt film thickness of 0.2 mm, a semi-haver waveform, a waveform amplitude of 0.01 mm, a loading width of 1000 ms, a frequency of 1 Hz, an ambient temperature of 20 ° C, an aggregate type of limestone, a stop condition of 5% of the peak load, and a circular stainless steel metal pressure head with a diameter of 27 mm. When used, the following steps are specifically included:

[0079] S1: Prepare asphalt-aggregate specimens. Take the required initial cylindrical aggregate specimens from the rock core and cut them;

[0080] The target asphalt film thickness is determined to be 0.2 mm, using the formula

[0081] m=πr 2 hρ(T)

[0082] Where, m is the weight of asphalt, g; r is the radius of asphalt film, cm; h is the thickness of asphalt film, cm; ρ(T) is the density of asphalt, which is 1.037 g / cm 3; T-test temperature, 20℃;

[0083] Calculate and weigh the required mass of #70 base asphalt, which is 118 mg;

[0084] Rinse the polished aggregate surface with distilled water to remove dust and impurities from the surface;

[0085] A circular area with a diameter of 27 mm was marked on the surface of the processed aggregate specimen to accommodate the circular bottom surface of the stainless steel metal indenter;

[0086] Place the marked aggregate specimens in a 150°C oven for 1 hour to dry the moisture on the limestone surface and maintain the temperature of the specimen surface to ensure smooth application of cold asphalt;

[0087] Use a stainless steel metal indenter to evenly apply 118 mg of cold asphalt to the marked circular area with a radius of 13.5 mm, and place the asphalt-aggregate specimen in a 20°C operating box. Based on the formula

[0088]

[0089] Where m is the weight of asphalt, 118 mg; r is the radius of the asphalt film, 13.5 mm; h is the thickness of the asphalt film, 0.2 mm; ρ(T) is the density of asphalt, 1.037 g / cm 3 ; T-test temperature, 20℃;

[0090] The target asphalt film thickness was 0.2 mm.

[0091] S2: Fix the asphalt-aggregate specimens, such as Figure 2 As shown, the stainless steel metal head screw B on the above specimen is screwed into the pull rod A;

[0092] Raise the G lifting platform until the F fixing bolts on the E fixture platform reach the middle of the D cylindrical aggregate, then stop;

[0093] Tighten the bolts in diagonal order until the F fixing bolts cannot be inserted into the threads;

[0094] Manually zero the pressure sensor of the G lift.

[0095] S3: Perform fatigue performance test on asphalt-aggregate interface, maintain the servo hydraulic dynamic test system operating box at 20°C, and cure the asphalt-aggregate specimen for 40 minutes to ensure stable strength of the interface;

[0096] The control strain form is set to have a half-haversine waveform, with a waveform amplitude of 0.01 mm, a loading width of 1000 ms, a frequency of 1 Hz, and a stop condition of reaching 5% of the peak load;

[0097] Collect brake displacement data, tension sensor data, and phase angle data;

[0098] Processing experimental data, according to the displacement of the brake, based on the formula

[0099]

[0100] ε-strain of asphalt film; ΔL-displacement of brake, mm; h-thickness of asphalt film, mm;

[0101] Calculate the strain of the asphalt membrane based on the formula

[0102]

[0103] σ-stress, MPa; S-area of ​​circular region, mm 2 ; r-radius of circular area, mm; F-tension, N;

[0104] Calculate stress and strain during stretching and make dynamic modulus and phase angle Curves, such as Figure 4-5 , complete the asphalt-aggregate interface tensile strength test.

[0105] S4: Characterize the fatigue performance of the asphalt-aggregate interface, take the ratio based on the stress and strain data, and draw the dynamic modulus The dynamic modulus of the first cycle is taken as the initial modulus.

[0106] According to the phase angle data output by DTS-30, draw the phase angle The curve with the number of loading times, the phase angle of the first cycle is taken as the initial phase angle

[0107] According to the energy balance principle of the entire volume of the cylindrical specimen, in the Nth loading cycle, the dissipated strain energy DSE of the damage configuration is A and the dissipated strain energy DSE of the undamaged configuration T Equivalent, based on the formula

[0108]

[0109] Where, ε0-amplitude of the haversine waveform, 0.01 mm; - Dynamic modulus, MPa; -phase angle, deg; a-radius of the circular area of ​​the specimen, 13.5 mm; t-thickness of the asphalt film, 0.2 mm; c-crack length, mm; - Initial modulus, 1.76 MPa; - Initial phase angle, 40°;

[0110] After derivation, the calculation formula for the crack length under the tensile load mode is

[0111]

[0112] The curve of crack length versus loading times is obtained, such as Figure 5 As shown;

[0113] Based on the Pseudo J-integral law of fracture mechanics:

[0114]

[0115] Where, c-crack length, mm; dc / dN-crack growth rate, mm / time; ΔK-stress intensity factor; A and n-fracture coefficient;

[0116] Based on the data of loading times, dynamic modulus and phase angle, the power function relationship between crack growth rate and stress intensity factor is established through planning and solving, where A = 1.26*E-9, n = 1.47;

[0117] After derivation, we get

[0118]

[0119] Finally, based on the relationship between crack growth rate and dynamic modulus and phase angle, Matlab software was used;

[0120] Integrate both sides of the formula

[0121]

[0122] The iterative solution yields the fatigue life Nf = 5717 times, which is the fatigue performance characterization index of the asphalt-aggregate interface.

Claims

1. A method for characterizing fatigue performance of asphalt-aggregate interface, It is characterized in that The steps include: Step S1: asphalt-aggregate specimen preparation; After the aggregate specimen is prepared, the area to be tested is marked on the surface of the aggregate specimen, and an asphalt coating area is set within the area to be tested, and then cold asphalt is evenly coated on the asphalt coating area to the target asphalt film thickness, so that an asphalt-aggregate specimen that meets the requirements can be prepared; Step S2: asphalt-aggregate specimen fixing; Loading the asphalt-aggregate specimen prepared in step S1 into an asphalt-aggregate interface fatigue test fixing and loading device; The asphalt-aggregate interface fatigue test fixing and loading device comprises a fixture table, a lifting platform, a pull rod and a stainless steel metal pressure head; the fixture table is installed above the lifting platform in a liftable manner, and the stainless steel metal pressure head is suspended above the fixture table through the pull rod; the stainless steel metal pressure head can move toward / away from the fixture table under the drive of the pull rod; The asphalt-aggregate specimen is loaded through a fixture table, and the area to be tested on the asphalt-aggregate specimen is located directly below the stainless steel metal pressure head; Step S3: asphalt-aggregate interface fatigue performance test; After the asphalt-aggregate specimens are cured at 20°C for a period of time, the asphalt-aggregate interface fatigue test fixing and loading device is started, and according to the preset direct tensile fatigue program, the asphalt-aggregate interface fatigue performance test is carried out by driving the stainless steel metal pressure head to repeatedly stretch and restore the test area of ​​the asphalt-aggregate specimen, and the brake displacement data, tension sensor data, and phase angle data are collected in real time according to the data collection cycle, and the stress and strain of the asphalt film are calculated respectively according to the collected brake displacement data and tension sensor data; Step S4: characterization of fatigue performance of asphalt-aggregate interface; According to the stress and strain of the asphalt film calculated in step S3, the dynamic modulus is calculated. Then, based on the relationship between the crack growth rate, dynamic modulus and phase angle, the fatigue life Nf of the asphalt film can be iteratively calculated, thereby completing the asphalt-aggregate interface tensile strength test.

2. The method for characterizing fatigue performance of asphalt-aggregate interface according to claim 1, It is characterized in that In step S2, the fixture table has a specimen accommodating cavity; the outer dimensions of the asphalt-aggregate specimen match the inner wall shape of the specimen accommodating cavity; the asphalt-aggregate specimen is placed in the specimen accommodating cavity and is locked by fixing bolts configured on the cavity wall of the specimen accommodating cavity.

3. The method for characterizing fatigue performance of asphalt-aggregate interface according to claim 1, It is characterized in that In step S1, the area to be tested and the asphalt coating area are both circular and overlapped as a whole, and the size of the stainless steel metal pressure head is equal to the size of the asphalt coating area.

4. The method for characterizing fatigue performance of asphalt-aggregate interface according to claim 1, It is characterized in that In step S1, the asphalt-aggregate specimen is prepared specifically by: Step S1.1, preparing aggregate specimens and determining target asphalt film thickness: The rock is cored and cut to obtain cylindrical aggregate specimens, and the mass of cold asphalt required for the test is calculated and weighed according to the determined target asphalt film thickness: m=πr 2 hρ(T) Where: m-bitumen weight; r-bitumen film radius; h-bitumen film thickness; ρ(T)-bitumen density; T-test temperature; Step S1.2, washing the surface of the polished aggregate specimen with distilled water to remove dust and impurities; Step S1.3, marking the area to be tested on the surface of the aggregate specimen to match the circular bottom surface of the stainless steel metal indenter; Step S1.4, drying the moisture on the surface of the aggregate specimen and maintaining the surface temperature of the aggregate specimen; Step S1.5: At the middle position of the test area marked on the surface of the aggregate specimen, select an area with a radius of r as the asphalt coating area, and evenly apply asphalt with a weight of m on the asphalt coating area to obtain an asphalt-aggregate specimen with a target asphalt film thickness.

5. The method for characterizing fatigue performance of asphalt-aggregate interface according to claim 4, It is characterized in that In step S2, the asphalt-aggregate specimen is fixed specifically by the following steps: Step S2.1, assembling the stainless steel metal pressing head under the pulling rod; Step S2.2, raising the lifting platform to drive the fixture table to rise, so that the fixing bolts arranged around the fixture table are aligned with the middle position of the asphalt-aggregate specimen; Step S2.3, tighten the fixing bolts in diagonal order to lock the asphalt-aggregate specimen; Step S2.4, zeroing the pressure sensor of the lifting platform.

6. The method for characterizing fatigue performance of asphalt-aggregate interface according to claim 5, It is characterized in that In step S2, the asphalt-aggregate interface fatigue test fixing and loading device used is a DTS-30 servo hydraulic dynamic test system.

7. The method for characterizing fatigue performance of asphalt-aggregate interface according to claim 6, It is characterized in that In step S3, the asphalt-aggregate interface fatigue performance test specifically includes the following steps: Step S3.1, maintaining the operating box temperature of the DTS-30 servo hydraulic dynamic testing system at 20°C to cure the asphalt-aggregate specimen for 40 minutes to ensure that the interface forms a stable strength; Step S3.2, setting a direct tensile fatigue program, setting the control strain form to a half-haversine waveform, optionally, the waveform amplitude is 5% of the asphalt film thickness, the loading width is 1000 ms, the frequency is 1 Hz, and the stop condition is reaching 5% of the peak load; Step S3.3, collecting brake displacement data, tension sensor data, and phase angle data; Step S3.4, processing test data: The strain of the asphalt film was calculated according to the following formula: ε-strain of asphalt film; ΔL-displacement of brake; h-thickness of asphalt film; The stress of the asphalt membrane is calculated according to the following formula: σ-stress, MPa; r-radius of asphalt film; F-tension.

8. The method for characterizing fatigue performance of asphalt-aggregate interface according to claim 1, It is characterized in that In step S4, the fatigue performance characterization of the asphalt-aggregate interface is specifically obtained by the following steps: S4.1: Based on the stress and strain data, take the ratio and plot the dynamic modulus The dynamic modulus of the first cycle is taken as the initial modulus. S4.2: Draw the phase angle according to the phase angle data output by DTS-30 The curve with the number of loading times, the phase angle of the first cycle is taken as the initial phase angle S4.3: According to the energy balance principle of the entire volume of the cylindrical specimen, in the Nth loading cycle, the dissipated strain energy DSE based on the damage configuration is A and the dissipated strain energy DSE of the undamaged configuration T Equivalently, the calculation formula for the crack length under the tensile load mode is derived: S4.4: Based on the Paris law of fracture mechanics, establish the power function relationship between crack growth rate and stress intensity factor; S4.

5. Based on the relationship between crack growth rate, dynamic modulus and phase angle, using mathematical processing software, the integral of both sides of the formula is as follows: By iterative solution, the fatigue life Nf of the asphalt-aggregate interface is obtained, which is the characterization index of the fatigue performance of the asphalt-aggregate interface.

Citation Information

Cited By

  • Analysis method of composite interface cohesive mechanical behavior

    CN120831321A

  • An analysis method for mechanical behavior of composite interface bonding

    CN120831321B

  • Asphalt-aggregate interface bonding fatigue testing device and testing method