Construction and application of portable electrochemical detection device
By using prismatic rod-shaped tetra-metal Fe/Co/Ni/Cu MOF@PPy materials to construct a portable electrochemical detection device, the problem of interference and high cost of biological enzymes in the prior art is solved, and the problem of low Cost, high sensitivity detection and screening help the treatment of diabetes.
Patent Information
- Application Number
- CN202411091960.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-12
AI Technical Summary
The existing α-glucosidase activity detection and inhibitor screening methods are disturbed by color matrix and light illumination, and the biological enzyme preparation cost is high and the stability is poor, making it difficult to build a high-sensitivity electrochemical sensing system.
Using prismatic rod-shaped tetrametallic Fe/Co/Ni/Cu MOF@PPy material with low cost and many surfactant sites as bionic enzymes, a portable electrochemical detection device is constructed in combination with intelligent terminal devices for the detection of α-glucosidase activity and inhibitor screening in natural products.
The detection of α-glucosidase activity with low cost, high stability, portability and high sensitivity can be achieved, and natural substances with high enzyme activity inhibitory components can be quickly and accurately screened out, providing a portable and practical strategy for the clinical treatment of diabetes.
Smart Images

Figure CN118937434A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrochemical detection, and in particular relates to the construction and use of a portable electrochemical detection device. Background Art
[0002] Type 2 diabetes is a type of non-insulin-dependent diabetes that can be controlled by controlling blood sugar levels after meals. α-Glucosidase is not only a key enzyme for digesting carbohydrates, but also the main cause of type 2 diabetes. It can catalyze the hydrolysis of disaccharides / oligosaccharides into glucose, and α-glucosidase inhibitors inhibit the activity of α-glucosidase, thereby prolonging the digestion time of carbohydrates and delaying intestinal glucose absorption. Therefore, α-glucosidase inhibitors play an important role in controlling postprandial hyperglycemia in diabetic patients and maintaining blood sugar levels within a relatively normal range. Common inhibitor drugs include acarbose, voglibose, and miglitol, but these chemically synthesized drugs are prone to cause side effects such as flatulence and indigestion, while inhibitors extracted from natural substances are safer. Therefore, it is very necessary to develop a highly sensitive and easy-to-operate method to detect the activity of α-glucosidase and to screen α-glucosidase inhibitors from natural products.
[0003] At present, the commonly used methods for α-glucosidase activity detection and α-glucosidase inhibitor screening are ultraviolet spectrophotometry, fluorescence, and electrochemiluminescence. The principle is mainly to measure the product of α-glucosidase-catalyzed substrates, which is easily interfered by color matrix and light. The electrochemical method is not interfered by color matrix and light, which can make up for this defect.
[0004] In the process of constructing electrochemical sensing systems, signal probes play an important role in achieving specific recognition and in-situ catalysis of the analyte. However, the biological enzymes used to prepare signal probes are expensive, easily inactivated, and have poor stability, making them difficult to be directly used for electrode modification to construct sensing systems. In recent years, metal-organic framework materials (MOFs) have been widely used in sensor construction due to their advantages such as strong stability, simple preparation, and low preparation cost. However, the number of active sites on the surface of existing MOF biomimetic enzymes is limited, which affects their widespread application in electrochemical sensing sensitive analysis.
[0005] Therefore, it is crucial to use a MOF biomimetic enzyme with multiple active sites instead of biological enzymes to construct a low-cost, stable, and low-interference electrochemical sensor for the detection of α-glucosidase activity and the screening of α-glucosidase in natural products. Summary of the invention
[0006] In view of the above problems, the present invention prepares a low-cost bimetallic bionic enzyme with multiple surface active sites, constructs a portable electrochemical detection device, and uses it for detecting α-glucosidase activity and screening α-glucosidase inhibitors.
[0007] In order to achieve the above technical objectives, the specific steps of the present invention are as follows:
[0008] A method for preparing an electrochemical sensor, the steps are as follows:
[0009] Step 1: Preparation of sensing substrate:
[0010] Process 1: Weigh ferric chloride, cobalt nitrate, nickel nitrate, copper nitrate and 2-aminoterephthalic acid, disperse them in N,N-dimethylformamide to obtain a mixed solution and stir;
[0011] Process 2: The mixed solution obtained in process 1 is transferred into a reactor, and then placed in an oven for heating reaction. After the heating reaction is completed, a dark brown precipitate is obtained by centrifugation, which is washed with N,N-dimethylformamide and ethanol respectively, and then vacuum dried to obtain a prismatic rod-shaped four-metal Fe / Co / Ni / Cu MOF material;
[0012] Process three: Take pyrrole (PPy) in deionized water, add the prismatic rod-shaped tetrametallic Fe / Co / Ni / Cu MOF material prepared in process two under stirring, then carry out the first continuous stirring, add ferric chloride after stirring and carry out the second stirring; then the product obtained by centrifugation is washed with ethanol and deionized water respectively, and the powder obtained by vacuum drying is recorded as prismatic rod-shaped tetrametallic Fe / Co / Ni / Cu MOF@PPy material; finally, the obtained prismatic rod-shaped tetrametallic Fe / Co / Ni / CuMOF@PPy material is dispersed in deionized water to obtain a prismatic rod-shaped tetrametallic Fe / Co / Ni / Cu MOF@PPy aqueous solution.
[0013] Furthermore, the amounts of ferric chloride, cobalt nitrate, nickel nitrate, copper nitrate, 2-aminoterephthalic acid and N,N-dimethylformamide used in process 1 of step 1 are 0.1-0.5 mmol: 0.1-0.5 mmol: 0.1-0.5 mmol: 0.1-0.5 mmol: 30-80 mL.
[0014] Furthermore, in process 2 of step 1, the temperature of the heating reaction is 80-160°C, and the reaction time is 12-48 hours; the number of washing times is 3-5 times; the centrifugal conditions are: 5000-15000rpm, 5-15min; the temperature of the vacuum drying is 60-70°C, and the time is 12-14h.
[0015] Furthermore, in process three of step one, the dosage ratio of pyrrole to deionized water is 50 mg:30 mL; the mass ratio of pyrrole to prismatic rod-shaped tetrametallic Fe / Co / Ni / Cu MOF powder is 1:1-6; the first continuous stirring time is 30-70 min; the mass ratio of ferric chloride to pyrrole monomer is 1.04:1; the second stirring time is 4-6 h; the centrifugal conditions are: 5000-15000 rpm, 5-15 min; the vacuum drying temperature is 60-80°C; the concentration of the prismatic rod-shaped tetrametallic Fe / Co / Ni / Cu MOF@PPy aqueous solution is 0.5-3 mg / ml.
[0016] Step 2: Preparation of electrochemical sensor:
[0017] The screen-printed electrode was immersed in H2SO4 solution to activate the electrode. After activation, the H2SO4 solution on the surface was rinsed off with deionized water and dried at room temperature. After drying, it was recorded as screen-printed electrode A. Then, the prismatic rod-shaped four-metal Fe / Co / Ni / Cu MOF@PPy aqueous solution prepared in step 1 was dropped on the working electrode surface of screen-printed electrode A, and an electrochemical sensor was obtained after drying.
[0018] Furthermore, the concentration of the H2SO4 solution in step 2 is 1 mol / L; the activation is performed by cyclic voltammetry, with 20 cycles; the volume of the prismatic rod-shaped four-metal Fe / Co / Ni / Cu MOF@PPy aqueous solution added is 6 to 10 μL; the drying temperature is 50°C and the drying time is 20 min.
[0019] A portable electrochemical detection device, comprising an electrochemical sensor prepared by the above method;
[0020] The portable electrochemical detection device is composed of a power supply, a Bluetooth module, a microcontroller, an electrical signal conversion module, an electrical signal acquisition module (potentiostat), an electrochemical sensor and an intelligent terminal; wherein the electrical signal conversion module includes an AD converter and a DA converter;
[0021] The intelligent terminal is electrically connected to the microcontroller via the Bluetooth module to achieve signal transmission and control; at the same time, the microcontroller is electrically connected to the AD converter and the DA converter respectively; the AD converter is connected to the electrical signal acquisition module; the electrochemical sensor is electrically connected to the DA converter and the electrical signal acquisition module (potentiostat) respectively;
[0022] The smart terminal is connected to the Bluetooth module and sends a detection command to the microcontroller. After receiving the detection command, the microcontroller converts the digital signal into an analog signal through the DA converter, and applies voltage to the electrochemical sensor through the electrical signal acquisition module (potentiostat). The electrochemical sensor is stimulated to generate a signal, and the analog signal is converted into a digital signal through the AD converter and then transmitted back to the microcontroller. The microcontroller then transmits the data to the smart terminal through the Bluetooth module;
[0023] Furthermore, the power supply is ZMV2405D, the Bluetooth module is nRF52840, and the microcontroller is STM32. The intelligent terminal includes a smart phone; the applied starting voltage is -0.8V, and the end voltage is 0.9V.
[0024] The portable electrochemical detection device is used for the detection of α-glucosidase activity, and the operation is as follows:
[0025] Process 1: First, a series of α-glucosidase solutions were prepared with PBS buffer, with concentrations of Q1, Q2, Q3, ..., Q n-1 , Q n , there are n concentration gradients in total, n is a positive integer;
[0026] Process 2: Mix the 4-nitrophenyl-α-D-pyranoglucoside solution and the α-glucosidase solution in process 1, incubate for a period of time, and then obtain a mixed solution for electrochemical detection;
[0027] Process 3: During the electrochemical detection process, the start and end voltages required for detection are output by the intelligent terminal, and the electrochemical sensor is used for detection. The microcontroller collects and stores the current response value generated by the electrochemical sensor. A linear regression model is established based on the correlation between the α-glucosidase concentration and the response current. The regression equation is y=ax+b, where x represents the concentration of α-glucosidase, y represents the current response value, and a and b are constants.
[0028] Process 4: Detection of α-glucosidase in serum:
[0029] The serum sample is centrifuged to remove the precipitate, and then diluted with deionized water to obtain a diluted serum sample; the diluted serum sample is mixed with a 4-nitrophenyl-α-D-pyranoglucoside solution, and electrochemical detection is performed after incubation for a period of time, and the obtained current value is substituted into the linear equation of process three to calculate the α-glucosidase concentration in the serum;
[0030] Furthermore, in process 1, the concentration of the PBS buffer is 0.1 mol / L, and the pH is 7.0; the concentration range of the α-glucosidase is 0.002 U / mL to 0.02 U / mL.
[0031] Furthermore, the concentration of the 4-nitrophenyl-α-D-pyranoglucoside solution in process 2 is 6 to 14 mmol / L, the volume ratio of the 4-nitrophenyl-α-D-pyranoglucoside solution to the α-glucosidase solution is 1 to 5:2 to 10; the concentration of the PBS buffer is 0.1 mol / L, and the pH is 7.0; the incubation temperature is 36 to 40°C, and the incubation time is 20 to 60 min.
[0032] Furthermore, the centrifugation conditions in process four are 4000 rpm, 5 to 10 min; the dilution multiple with deionized water is 100 times; the concentration of the 4-nitrophenyl-α-D-pyranoglucoside solution is 6 to 14 mmol / L, and the volume ratio of the 4-nitrophenyl-α-D-pyranoglucoside solution to the diluted serum sample is 1 to 5:2 to 10; the incubation temperature is 36 to 40°C, and the incubation time is 20 to 60 min.
[0033] The portable electrochemical detection device is used for screening α-glucosidase inhibitors, and the steps are as follows:
[0034] Process 1: Take the sample to be selected and place it in deionized water to obtain a mixed system, extract it by ultrasonication, centrifuge it and collect the supernatant;
[0035] Process 2: The supernatant was mixed with the α-glucosidase solution for the first incubation. After the incubation, 4-nitrophenyl-α-D-pyranoglucoside was added for the second incubation. After the incubation, electrochemical detection was performed to calculate the inhibition rate of the inhibitor and establish a linear regression equation. The inhibition rate was Where I1 is the current value measured in the presence of α-glucosidase and 4-nitrophenyl-α-D-pyranoglucoside, I x is the current value measured in the presence of only 4-nitrophenyl-α-D-pyranoglucoside, I0 is the current value measured in the presence of α-glucosidase, 4-nitrophenyl-α-D-pyranoglucoside and natural samples; then, based on the mass concentration of the sample in the mixed system and the corresponding inhibition rate, a regression equation of y1=a1x1+b1 is established, wherein x1 represents the concentration of the sample, y1 represents the inhibition rate, and a1 and b1 are constants; when the inhibition rate is 50%, the corresponding sample concentration is the half inhibition concentration (IC50), recorded as C-0;
[0036] Process 3: Identification: Replace the candidate sample with a commercial α-glucosidase inhibitor and follow the procedure of process 2 to obtain its corresponding half inhibition concentration, recorded as C-1; if the half inhibition concentration C-0 of the candidate sample is not higher than C-1, it can be selected as an inhibitor of α-glucosidase.
[0037] Furthermore, in process 1, the mass concentration of the sample in the mixed system is 0.1-2 mg / mL; the centrifugation condition is 8000 rpm, 5-10 min; the samples to be selected include but are not limited to tea, pepper, and wheat.
[0038] Furthermore, in process 2, the volume ratio of the supernatant to the α-glucosidase solution and 4-nitrophenyl-α-D-pyranoglucoside is 5:3:0.5-2.5, the concentration of the α-glucosidase solution is 0.05U / mL; the first incubation time is 30min, and the incubation temperature is 37°C; the concentration of the 4-nitrophenyl-α-D-pyranoglucoside is 6-14mmol / L; the second incubation temperature is 36-40°C, and the incubation time is 20-60min.
[0039] Furthermore, the commercial α-glucosidase inhibitors described in process three include acarbose, voglibose and miglitol.
[0040] Compared with the prior art, the present invention has the following beneficial effects:
[0041] (1) The prismatic rod-shaped tetrametallic Fe / Co / Ni / Cu MOF@PPy described in the present invention has the characteristics of low cost, high stability, and multiple surface active sites.
[0042] (2) The present invention combines electrochemical micro-nano electrodes with intelligent terminal devices, thereby improving the portability of electrochemical determination and the practicality of on-site detection.
[0043] (3) In addition to being able to detect α-glucosidase activity in a portable manner, the present invention can also quickly and accurately screen out natural substances with high levels of enzyme activity inhibitory components, safety and low cost, providing a more portable and practical strategy for the screening of α-glucosidase inhibitors, which is helpful for the clinical treatment of diabetes. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 This is a scanning electron microscope image of the prismatic rod-shaped four-metal Fe / Co / Ni / Cu MOF.
[0045] Figure 2 This is a scanning electron microscope image of the prismatic rod-shaped four-metal Fe / Co / Ni / Cu MOF@PPy.
[0046] Figure 3 Block diagram of a portable device that assists a smartphone. DETAILED DESCRIPTION
[0047] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0048] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0049] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0050] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0051] The tea leaves used in this example were purchased from Jimailong Supermarket in Zhenjiang City. The serum samples were calf serum samples purchased from Kewei Biotechnology Co., Ltd.
[0052] Embodiment 1:
[0053] Step 1: Preparation of sensing substrate:
[0054] Process 1: Weigh 0.1 mmol of ferric chloride, 0.1 mmol of cobalt nitrate, 0.1 mmol of nickel nitrate, 0.1 mmol of copper nitrate and 0.1 mmol of 2-aminoterephthalic acid and disperse them in 30 mL of N,N-dimethylformamide to obtain a mixed solution and stir for 40 min;
[0055] Process 2: The mixed solution obtained in process 1 was transferred into a reactor, and then placed in an oven and heated at 80°C for 12 hours. After the heating reaction was completed, a dark brown precipitate was obtained by centrifugation (5000 rpm, 15 min). The precipitate was washed by centrifugation with N,N-dimethylformamide and ethanol respectively, and then dried in vacuum at 60°C for 12 hours to obtain a prismatic rod-shaped four-metal Fe / Co / Ni / Cu MOF material.
[0056] Process three: Take 50 mg of pyrrole (PPy) and dissolve it in 30 ml of deionized water. Add 50 mg of prismatic rod-shaped tetrametallic Fe / Co / Ni / Cu MOF powder under stirring. After continuous stirring for 30 minutes, add 52 mg of ferric chloride and continue stirring for 4 hours. Then, the product obtained by centrifugation (5000 rpm, 15 minutes) was washed with ethanol and deionized water respectively, and then dried in vacuo at 60°C to obtain a powder recorded as prismatic rod-shaped tetrametallic Fe / Co / Ni / Cu MOF@PPy material. Finally, the obtained prismatic rod-shaped tetrametallic Fe / Co / Ni / Cu MOF@PPy material was dispersed in deionized water to obtain a 0.5 mg / mL prismatic rod-shaped tetrametallic Fe / Co / Ni / Cu MOF@PPy aqueous solution.
[0057] Figure 1 This is a scanning electron microscope image of a prismatic rod-shaped four-metal Fe / Co / Ni / Cu MOF material. From the image, it can be seen that the surface of the four-metal Fe / Co / Ni / Cu MOF material is smooth and presents a prismatic rod-shaped structure.
[0058] Figure 2 This is a scanning electron microscope image of the prismatic rod-shaped tetrametallic Fe / Co / Ni / Cu MOF@PPy material. From the figure, it can be seen that the surface of the tetrametallic Fe / Co / Ni / Cu MOF@PPy material is rough, but it still presents a prismatic rod-shaped structure, indicating that the modification of PPy does not change the morphology of the prismatic rod-shaped tetrametallic Fe / Co / Ni / Cu MOF.
[0059] Step 2: Preparation of electrochemical sensor:
[0060] The screen-printed electrode was immersed in 5 mL of 1 mol / L H2SO4 solution, and the electrode was activated by cyclic voltammetry. The number of activation cycles was 20. After the activation was completed, the H2SO4 solution on the surface was rinsed off with deionized water and dried at room temperature. The screen-printed electrode obtained after drying was recorded as screen-printed electrode A. Then, 6 μL of the prismatic rod-shaped four-metal Fe / Co / Ni / Cu MOF@PPy aqueous solution prepared in step 1 was dropped on the working electrode surface of screen-printed electrode A, and dried in an oven at 50°C for 20 min to obtain an electrochemical sensor.
[0061] Step 3: Construction of portable electrochemical detection device:
[0062] The portable electrochemical detection device consists of a power supply (ZMV2405D), a Bluetooth module (nRF52840), a microcontroller (STM32), an electrical signal conversion module (AD converter and DA converter), an electrical signal acquisition module (using a constant potential instrument), an electrochemical sensor and a smart phone; the smart phone is electrically connected to the microcontroller through the Bluetooth module to achieve signal transmission and control; at the same time, the microcontroller is electrically connected to the AD converter and the DA converter respectively; the AD converter is connected to the constant potential instrument; the electrochemical sensor is electrically connected to the DA converter and the constant potential instrument respectively;
[0063] Connect the smartphone to the Bluetooth module and send a detection command to the microcontroller. After receiving the detection command, the microcontroller converts the digital signal into an analog signal through the DA converter, and applies a starting voltage of -0.8V and a termination voltage of 0.9V to the electrochemical sensor through the electrical signal acquisition module (potentiostat). The electrochemical sensor receives the stimulus and generates a signal, which is converted into a digital signal through the AD converter and then transmitted back to the microcontroller. The microcontroller then sends the analyzed data to the smartphone through the Bluetooth module (such as Figure 3 shown);
[0064] Application 1: Portable electrochemical detection device is used for the activity detection of α-glucosidase:
[0065] Process 1: First, a series of α-glucosidase solutions were prepared with PBS buffer (0.1 mol / L, pH 7.0), including 0 U / mL, 0.002 U / mL, 0.004 U / mL, 0.006 U / mL, 0.008 U / mL, 0.01 U / mL, 0.012 U / mL, 0.014 U / mL, 0.016 U / mL, 0.018 U / mL, and 0.02 U / mL, with a total of 11 concentration gradients;
[0066] Process 2: 50 μL of 6 mmol / L 4-nitrophenyl-α-D-pyranoglucoside solution, 100 μL of α-glucosidase solution in process 1 and 100 μL of PBS buffer (0.1 mol / L, pH 7.0) were mixed, incubated at 36°C for 60 min, and the mixed solution was subjected to electrochemical detection;
[0067] Process 3: Before detection, the mixed solution is dripped onto the surface of the electrochemical sensor; the smartphone is connected to the microcontroller via the Bluetooth module and sends a detection command to the microcontroller. The smartphone outputs the starting voltage of -0.8V and the ending voltage of 0.9V required for detection. After receiving the detection command, the microcontroller converts the digital signal into an analog signal through the DA converter, and applies voltage to the electrochemical sensor through the electrical signal acquisition module. The electrochemical sensor is stimulated to generate a signal, and the analog signal is converted into a digital signal through the AD converter and then transmitted back to the microcontroller. The microcontroller then transmits the data to the smartphone via the Bluetooth module to obtain the current response value generated by the electrochemical sensor; a linear regression model is established based on the correlation between the α-glucosidase concentration and the response current, and the regression equation is y=95.352x+0.260(R 2 =0.9980), where x represents the concentration of α-glucosidase and y represents the response current value;
[0068] Process 4: Detection of α-glucosidase in serum:
[0069] 1 mL of serum sample was centrifuged (4000 rpm, 5 min) to remove the precipitate, then diluted 100 times with deionized water, 100 μL of the diluted serum sample, 50 μL of 6 mmol / L 4-nitrophenyl-α-D-pyranoglucoside solution and 100 μL of PBS buffer (0.1 mol / L, pH 7.0) were mixed, incubated at 36°C for 60 min, and then electrochemical detection was performed. The obtained current value was substituted into the linear equation of process three. The results showed that the concentration of α-glucosidase in the serum was 0.00542 U / mL.
[0070] Process 5: α-glucosidase spike recovery method determination:
[0071] 1 mL of serum sample was centrifuged (4000 rpm, 5 min) to remove the precipitate and then diluted 100 times with deionized water. 100 μL of the diluted serum sample, 100 μL of α-glucosidase solution and 50 μL of 6 mmol / L 4-nitrophenyl-α-D-pyranoglucoside solution were mixed and incubated at 36 °C for 60 min before spike recovery.
[0072] Table 1 Spike recovery test results
[0073] sample Spiked amount (U / mL) Detection amount (U / mL) Relative error (%) Recovery rate (%) 1 0 0.00542 2.5 - 2 0.004 0.00966 1.9 106.0 3 0.008 0.01363 1.7 102.6 4 0.120 0.12544 2.8 100.0
[0074] Application 2: The portable electrochemical detection device is used to screen α-glucosidase inhibitors in selected samples; the selected sample is Lapsang Souchong (black tea);
[0075] Process 1: Add tea leaves to deionized water to obtain a tea-water mixture system; the corresponding mass concentrations are 0.1 mg / mL, 0.2 mg / mL, 0.4 mg / mL, 0.6 mg / mL, 0.8 mg / mL, 1 mg / mL, 1.2 mg / mL, 1.4 mg / mL, 1.6 mg / mL, 1.8 mg / mL, and 2 mg / mL, with a total of 11 concentration gradients. Ultrasonic extraction is performed for 5 minutes, followed by centrifugation (8000 rpm, 5 minutes) and the supernatant is collected as a tea sample;
[0076] Process 2: 100 μL of tea sample supernatant corresponding to different mass concentrations were mixed with 100 μL 0.05U / mL α-glucosidase solution, incubated at 37°C for 30 min, and then 50 μL 6mmol / L 4-nitrophenyl-α-D-pyranoglucoside was added. The mixture was incubated at 36°C for 60 min before electrochemical detection. The detection process was as follows: before detection, the mixed solution was dripped onto the surface of the electrochemical sensor; the smartphone was connected to the microcontroller via the Bluetooth module and sent a detection instruction to the microcontroller. The smartphone output the starting voltage of -0.8V and the ending voltage of 0.9V required for detection. After receiving the detection command, the microcontroller converted the digital signal into an analog signal through the DA converter, and applied voltage to the electrochemical sensor through the electrical signal acquisition module. The electrochemical sensor was stimulated to generate a signal, and the analog signal was converted into a digital signal through the AD converter and then transmitted back to the microcontroller. The microcontroller then transmitted the data to the smartphone through the Bluetooth module to obtain the current response value generated by the electrochemical sensor. The inhibition rate of the inhibitor was calculated according to the correlation between the tea sample concentration and the response current, and a linear regression equation was established.
[0077] The inhibition rate is Where I1 is the current value measured in the presence of α-glucosidase and 4-nitrophenyl-α-D-pyranoglucoside, I x is the current value measured when only 4-nitrophenyl-α-D-pyranoglucoside is present, and I0 is the current value measured when α-glucosidase, 4-nitrophenyl-α-D-pyranoglucoside and the sample are present. The regression equation established based on the mass concentration of tea leaves and the corresponding inhibition rate is y1=35.372x1+18.620(R 2 =0.9920); when the inhibition rate is 50%, that is, y1=50, the half inhibition concentration is calculated to be 0.887 mg / mL;
[0078] Process 3: Dissolve the commercial α-glucosidase inhibitor acarbose in deionized water, and its mass concentrations are 0.1mg / mL, 0.2mg / mL, 0.4mg / mL, 0.6mg / mL, 0.8mg / mL, 1mg / mL, 1.2mg / mL, 1.4mg / mL, 1.6mg / mL, 1.8mg / mL, 2mg / mL, a total of 11 concentration gradients. Use it to replace the tea sample, and establish a linear regression equation according to the operation of process 2. The regression equation is y2=34.385x2+16.820(R 2 =0.9916); when the inhibition rate is 50%, that is, y2=50, the half inhibition concentration is calculated to be 0.965 mg / mL by substituting it into the regression equation;
[0079] From the above results, it can be seen that the components in tea samples that have an inhibitory effect on α-glucosidase have a better inhibitory effect than acarbose and can be used as inhibitors of α-glucosidase.
[0080] Embodiment 2:
[0081] Step 1: Preparation of sensing substrate:
[0082] Process 1: Weigh 0.3 mmol of ferric chloride, 0.3 mmol of cobalt nitrate, 0.3 mmol of nickel nitrate, 0.3 mmol of copper nitrate and 0.3 mmol of 2-aminoterephthalic acid and disperse them in 50 mL of N,N-dimethylformamide to obtain a mixed solution and stir for 40 min;
[0083] Process 2: The mixed solution obtained in process 1 was transferred into a reactor, and then placed in an oven and heated at 120°C for 24 hours. After the heating reaction was completed, a dark brown precipitate was obtained by centrifugation (10000 rpm, 10 min). After centrifugation and washing with N,N-dimethylformamide and ethanol, the precipitate was vacuum dried at 65°C for 13 hours to obtain a prismatic rod-shaped four-metal Fe / Co / Ni / Cu MOF material.
[0084] Process three: Take 50 mg of pyrrole (PPy) and dissolve it in 30 ml of deionized water. Add 150 mg of prismatic rod-shaped tetrametallic Fe / Co / Ni / Cu MOF powder under stirring. After continuous stirring for 50 min, add 52 mg of ferric chloride and continue stirring for 5 h. Then, the product obtained by centrifugation (10000 rpm, 10 min) was washed with ethanol and deionized water respectively, and then dried in vacuo at 70 ° C. The powder obtained was recorded as prismatic rod-shaped tetrametallic Fe / Co / Ni / Cu MOF@PPy material. Finally, the obtained prismatic rod-shaped tetrametallic Fe / Co / Ni / Cu MOF@PPy material was dispersed in deionized water to obtain a 2 mg / mL prismatic rod-shaped tetrametallic Fe / Co / Ni / Cu MOF@PPy aqueous solution.
[0085] Step 2: Preparation of electrochemical sensor:
[0086] The screen-printed electrode was immersed in 5 mL of 1 mol / L H2SO4 solution, and the electrode was activated by cyclic voltammetry. The number of activation cycles was 20. After the activation was completed, the H2SO4 solution on the surface was rinsed off with deionized water and dried at room temperature to obtain a screen-printed electrode A. Then, 8 μL of the prismatic rod-shaped four-metal Fe / Co / Ni / Cu MOF@PPy aqueous solution prepared in step 1 was dropped on the working electrode surface of the screen-printed electrode A, and dried in an oven at 50°C for 20 min to obtain an electrochemical sensor.
[0087] Step 3: Construction of electrochemical detection device:
[0088] The portable detection device consists of a power supply (ZMV2405D), a Bluetooth module (nRF52840), a microcontroller (STM32), an electrical signal conversion module (AD converter and DA converter), an electrical signal acquisition module (potentiostat), an electrochemical sensor and a smart phone; the smart phone is electrically connected to the microcontroller through the Bluetooth module to achieve signal transmission and control; at the same time, the microcontroller is electrically connected to the AD converter and the DA converter respectively; the AD converter is connected to the potentiostat; the electrochemical sensor is electrically connected to the DA converter and the potentiostat respectively;
[0089] Connect the smartphone to the Bluetooth module and send a detection command to the microcontroller. After receiving the detection command, the microcontroller converts the digital signal into an analog signal through the DA converter, and applies a starting voltage of -0.8V and a termination voltage of 0.9V to the electrochemical sensor through the electrical signal acquisition module (potentiostat). The electrochemical sensor receives the stimulation and generates a signal, which is converted into a digital signal through the AD converter and then transmitted back to the microcontroller. The microcontroller then sends the analyzed and processed data to the smartphone through the Bluetooth module.
[0090] Application 1: Portable electrochemical detection device is used for the activity detection of α-glucosidase:
[0091] Process 1: First, a series of α-glucosidase solutions were prepared with PBS buffer (0.1 mol / L pH 7.0), including 0 U / mL, 0.002 U / mL, 0.004 U / mL, 0.006 U / mL, 0.008 U / mL, 0.01 U / mL, 0.012 U / mL, 0.014 U / mL, 0.016 U / mL, 0.018 U / mL, and 0.02 U / mL, with a total of 11 concentration gradients;
[0092] Process 2: 150 μL of 10 mmol / L 4-nitrophenyl-α-D-pyranoglucoside solution, 100 μL of α-glucosidase solution in process 1, and 100 μL of PBS buffer (0.1 mol / L pH 7.0) were mixed, incubated at 38°C for 40 min, and the mixed solution was subjected to electrochemical detection;
[0093] Process 3: Before detection, the mixed solution is dripped onto the surface of the electrochemical sensor; the smartphone is connected to the microcontroller via the Bluetooth module and sends a detection command to the microcontroller. The smartphone outputs the starting voltage of -0.8V and the ending voltage of 0.9V required for detection. After receiving the detection command, the microcontroller converts the digital signal into an analog signal through the DA converter, and applies voltage to the electrochemical sensor through the electrical signal acquisition module. The electrochemical sensor is stimulated to generate a signal, and the analog signal is converted into a digital signal through the AD converter and then transmitted back to the microcontroller. The microcontroller then transmits the data to the smartphone via the Bluetooth module to obtain the current response value generated by the electrochemical sensor; a linear regression model is established based on the correlation between the α-glucosidase concentration and the response current, and the regression equation is y=95.388x+0.246(R 2 =0.9985), where x represents the concentration of α-glucosidase and y represents the response current value;
[0094] Process 4: Detection of α-glucosidase in serum:
[0095] The serum sample was centrifuged (4000 rpm, 5 min) to remove the precipitate, and then diluted 100 times with deionized water. 100 μL of the diluted serum sample, 150 μL of 10 mmol / L 4-nitrophenyl-α-D-pyranoglucoside solution and 100 μL of PBS buffer (0.1 mol / L pH 7.0) were mixed, and electrochemical detection was performed after incubation at 38°C for 40 min. The obtained current value was substituted into the linear equation of process three. The results showed that the concentration of α-glucosidase in the serum was 0.00738 U / mL;
[0096] Process 5: α-glucosidase spike recovery method determination:
[0097] 1 mL of serum sample was centrifuged (4000 rpm, 5 min) to remove the precipitate, then diluted 100 times with deionized water, 100 μL of the diluted serum sample, 100 μL of α-glucosidase solution and 150 μL of 10 mmol / L 4-nitrophenyl-α-D-pyranoglucoside solution were mixed, and spiked and recovered after incubation at 38 °C for 40 min.
[0098] Table 2 Spike recovery test results
[0099] sample Spiked amount (U / mL) Detection amount (U / mL) Relative error (%) Recovery rate (%) 1 0 0.00738 2.3 - 2 0.004 0.01138 2.8 100.0 3 0.008 0.01546 1.9 101.0 4 0.120 0.12738 2.6 100.0
[0100] Application 2: The portable electrochemical detection device is used to screen α-glucosidase inhibitors in selected samples; the selected sample is early spring snail green tea;
[0101] Process 1: Add tea leaves to deionized water to obtain a tea-water mixture system; the corresponding mass concentrations are 0.1 mg / mL, 0.2 mg / mL, 0.4 mg / mL, 0.6 mg / mL, 0.8 mg / mL, 1 mg / mL, 1.2 mg / mL, 1.4 mg / mL, 1.6 mg / mL, 1.8 mg / mL, and 2 mg / mL, with a total of 11 concentration gradients. Ultrasonic extraction is performed for 5 minutes, followed by centrifugation (8000 rpm, 8 minutes) and the supernatant is collected;
[0102] Process 2: 100 μL of tea sample supernatant corresponding to different mass concentrations were mixed with 100 μL 0.05U / mL α-glucosidase respectively, incubated at 37°C for 30 min, and then 150 μL 10mmol / L 4-nitrophenyl-α-D-pyranoglucoside was added. After incubation at 38°C for 40 min, electrochemical detection was performed. The detection process is as follows: before detection, the mixed solution was dripped onto the surface of the electrochemical sensor; the smartphone was connected to the microcontroller via the Bluetooth module and sent a detection instruction to the microcontroller. The smartphone output the starting voltage of -0.8V and the ending voltage of 0.9V required for detection. After receiving the detection command, the microcontroller converted the digital signal into an analog signal through the DA converter, and applied voltage to the electrochemical sensor through the electrical signal acquisition module. The electrochemical sensor was stimulated to generate a signal, and the analog signal was converted into a digital signal through the AD converter and then transmitted back to the microcontroller. The microcontroller then transmitted the data to the smartphone through the Bluetooth module to obtain the current response value generated by the electrochemical sensor. The inhibition rate of the inhibitor was calculated according to the correlation between the tea sample concentration and the response current, and a linear regression equation was established.
[0103] The inhibition rate is Where I1 is the current value measured in the presence of α-glucosidase and 4-nitrophenyl-α-D-pyranoglucoside, I x is the current value measured in the presence of only 4-nitrophenyl-α-D-pyranoglucoside, and I0 is the current value measured in the presence of α-glucosidase, 4-nitrophenyl-α-D-pyranoglucoside and natural samples. The regression equation based on the mass concentration of tea leaves and the corresponding inhibition rate is y1=45.523x1+29.086(R 2 =0.9975); when the inhibition rate is 50%, that is, y1=50, the half inhibition concentration is calculated to be 0.459 mg / mL;
[0104] Process 3: Dissolve the commercial α-glucosidase inhibitor voglibose in deionized water, and its mass concentrations are 0.1mg / mL, 0.2mg / mL, 0.4mg / mL, 0.6mg / mL, 0.8mg / mL, 1mg / mL, 1.2mg / mL, 1.4mg / mL, 1.6mg / mL, 1.8mg / mL, 2mg / mL, a total of 11 concentration gradients. Use it to replace the tea sample, and establish a linear regression equation according to the operation of process 2. The regression equation is y2=36.853x2+18.260(R 2 =0.9964); when the inhibition rate is 50%, that is, y2=50, the half inhibition concentration is calculated to be 0.861 mg / mL by substituting it into the regression equation;
[0105] From the above results, it can be seen that the components in tea samples that have an inhibitory effect on α-glucosidase have a better inhibitory effect than acarbose and can be used as inhibitors of α-glucosidase.
[0106] Embodiment 3:
[0107] Step 1: Preparation of sensing substrate:
[0108] Process 1: Weigh 0.5 mmol of ferric chloride, 0.5 mmol of cobalt nitrate, 0.5 mmol of nickel nitrate, 0.5 mmol of copper nitrate and 0.5 mmol of 2-aminoterephthalic acid and disperse them in 80 mL of N,N-dimethylformamide to obtain a mixed solution and stir for 40 min;
[0109] Process 2: The mixed solution obtained in process 1 was transferred into a reactor, and then placed in an oven and heated at 160°C for 48 hours. After the heating reaction was completed, a dark brown precipitate was obtained by centrifugation (15000rpm, 5min). The precipitate was washed by centrifugation with N,N-dimethylformamide and ethanol respectively, and then dried in vacuum at 70°C for 14 hours to obtain a prismatic rod-shaped four-metal Fe / Co / Ni / Cu MOF material.
[0110] Process three: Take 50 mg of pyrrole (PPy) and dissolve it in 30 ml of deionized water. Add 300 mg of prismatic rod-shaped tetrametallic Fe / Co / Ni / Cu MOF powder under stirring. After continuous stirring for 70 min, add 52 mg of ferric chloride and continue stirring for 6 h. Then, the product obtained by centrifugation (15000 rpm, 5 min) was washed with ethanol and deionized water respectively, and then vacuum dried at 80 ° C to obtain a powder recorded as prismatic rod-shaped tetrametallic Fe / Co / Ni / Cu MOF@PPy material. Finally, the obtained prismatic rod-shaped tetrametallic Fe / Co / Ni / Cu MOF@PPy material was dispersed in deionized water to obtain a 3 mg / mL prismatic rod-shaped tetrametallic Fe / Co / Ni / Cu MOF@PPy aqueous solution.
[0111] Step 2: Preparation of electrochemical sensor:
[0112] The screen-printed electrode was immersed in 5 mL of 1 mol / L H2SO4 solution, and the electrode was activated by cyclic voltammetry. The number of activation cycles was 20. After the activation was completed, the H2SO4 solution on the surface was rinsed off with deionized water and dried at room temperature to obtain a screen-printed electrode A. Then, 10 μL of the prismatic rod-shaped four-metal Fe / Co / Ni / Cu MOF@PPy aqueous solution prepared in step 1 was dropped on the working electrode surface of the screen-printed electrode A, and dried in an oven at 50°C for 20 min to obtain an electrochemical sensor.
[0113] Step 3: Construction of electrochemical detection device:
[0114] The portable electrochemical detection device consists of a power supply (ZMV2405D), a Bluetooth module (nRF52840), a microcontroller (STM32), an electrical signal conversion module (AD converter and DA converter), an electrical signal acquisition module (using a constant potential instrument), an electrochemical sensor and a smart phone; the smart phone is electrically connected to the microcontroller through the Bluetooth module to achieve signal transmission and control; at the same time, the microcontroller is electrically connected to the AD converter and the DA converter respectively; the AD converter is connected to the constant potential instrument; the electrochemical sensor is electrically connected to the DA converter and the constant potential instrument respectively;
[0115] Connect the smartphone to the Bluetooth module and send a detection command to the microcontroller. After receiving the detection command, the microcontroller converts the digital signal into an analog signal through the DA converter, and applies a starting voltage of -0.8V and a termination voltage of 0.9V to the electrochemical sensor through the electrical signal acquisition module (potentiostat). The electrochemical sensor receives the stimulation and generates a signal, which is converted into a digital signal through the AD converter and then transmitted back to the microcontroller. The microcontroller then sends the analyzed and processed data to the smartphone through the Bluetooth module.
[0116] Application 1: Portable electrochemical detection device is used for the activity detection of α-glucosidase:
[0117] Process 1: First, a series of α-glucosidase solutions were prepared with PBS buffer (0.1 mol / L pH 7.0), including 0 U / mL, 0.002 U / mL, 0.004 U / mL, 0.006 U / mL, 0.008 U / mL, 0.01 U / mL, 0.012 U / mL, 0.014 U / mL, 0.016 U / mL, 0.018 U / mL, and 0.02 U / mL, with a total of 11 concentration gradients;
[0118] Process 2: 250 μL of 14 mmol / L 4-nitrophenyl-α-D-pyranoglucoside solution, 100 μL of α-glucosidase solution in process 1 and 100 μL of PBS buffer (0.1 mol / L pH 7.0) were mixed, incubated at 40°C for 20 min, and the mixed solution was subjected to electrochemical detection;
[0119] Process 3: Before detection, the mixed solution is dripped onto the surface of the electrochemical sensor; the smartphone is connected to the microcontroller via the Bluetooth module and sends a detection command to the microcontroller. The smartphone outputs the starting voltage of -0.8V and the ending voltage of 0.9V required for detection. After receiving the detection command, the microcontroller converts the digital signal into an analog signal through the DA converter, and applies voltage to the electrochemical sensor through the electrical signal acquisition module. The electrochemical sensor is stimulated to generate a signal, and the analog signal is converted into a digital signal through the AD converter and then transmitted back to the microcontroller. The microcontroller then transmits the data to the smartphone via the Bluetooth module to obtain the current response value generated by the electrochemical sensor; a linear regression model is established based on the correlation between the α-glucosidase concentration and the response current, and the regression equation is y=95.180x+0.196(R 2 =0.9982), where x represents the concentration of α-glucosidase and y represents the response current value;
[0120] Process 4: Detection of α-glucosidase in serum:
[0121] 1 mL of serum sample was centrifuged (4000 rpm, 5 min) to remove the precipitate, then diluted 100 times with deionized water, 100 μL of the diluted serum sample, 250 μL of 14 mmol / L 4-nitrophenyl-α-D-pyranoglucoside solution and 100 μL of PBS buffer (0.1 mol / L pH 7.0) were mixed, incubated at 40 °C for 20 min, and then electrochemical detection was performed. The obtained current value was substituted into the linear equation of process three, and the results showed that the concentration of α-glucosidase in serum was 0.00666 U / mL;
[0122] Process 5: α-glucosidase spike recovery method determination:
[0123] 1 mL of serum sample was centrifuged (4000 rpm, 5 min) to remove the precipitate, then diluted 100 times with deionized water, 100 μL of the diluted serum sample, 100 μL of α-glucosidase solution and 250 μL of 14 mmol / L 4-nitrophenyl-α-D-pyranoglucoside solution were mixed, incubated at 40 °C for 20 min, and then spiked and recovered.
[0124] Table 3 Spike recovery test results
[0125] sample Spiked amount (U / mL) Detection amount (U / mL) Relative error (%) Recovery rate (%) 1 0 0.00666 2.6 - 2 0.004 0.01065 2.0 99.8 3 0.008 0.01478 1.7 101.5 4 0.120 0.12666 2.7 100.0
[0126] Application 2: The portable electrochemical detection device is used for screening α-glucosidase inhibitors in the selected samples; the sample is Gongmei white tea;
[0127] Process 1: Add tea leaves into deionized water to obtain a tea-water mixture system; the corresponding mass concentrations are 0.1 mg / mL, 0.2 mg / mL, 0.4 mg / mL, 0.6 mg / mL, 0.8 mg / mL, 1 mg / mL, 1.2 mg / mL, 1.4 mg / mL, 1.6 mg / mL, 1.8 mg / mL, and 2 mg / mL, with a total of 11 concentration gradients. After ultrasonic extraction for 5 minutes, centrifuge (8000 rpm, 10 min) and collect the supernatant as a tea sample.
[0128] Process 2: 100 μL of tea sample supernatant corresponding to different mass concentrations were mixed with 100 μL 0.05U / mL α-glucosidase, incubated at 37°C for 30 min, and then 250 μL 14mmol / L 4-nitrophenyl-α-D-pyranoglucoside was added. The mixture was incubated at 40°C for 20 min before electrochemical detection. The detection process was as follows: before detection, the mixed solution was dripped onto the surface of the electrochemical sensor; the smartphone was connected to the microcontroller via the Bluetooth module and sent a detection instruction to the microcontroller. The smartphone output the starting voltage of -0.8V and the ending voltage of 0.9V required for detection. After receiving the detection command, the microcontroller converted the digital signal into an analog signal through the DA converter, and applied voltage to the electrochemical sensor through the electrical signal acquisition module. The electrochemical sensor was stimulated to generate a signal, and the analog signal was converted into a digital signal through the AD converter and then transmitted back to the microcontroller. The microcontroller then transmitted the data to the smartphone through the Bluetooth module to obtain the current response value generated by the electrochemical sensor. The inhibition rate of the inhibitor was calculated according to the correlation between the tea sample concentration and the response current, and a linear regression equation was established. The inhibition rate is Where I1 is the current value measured in the presence of α-glucosidase and 4-nitrophenyl-α-D-pyranoglucoside, I x is the current value measured in the presence of only 4-nitrophenyl-α-D-pyranoglucoside, and I0 is the current value measured in the presence of α-glucosidase, 4-nitrophenyl-α-D-pyranoglucoside and natural samples. The regression equation based on the mass concentration of tea leaves and the corresponding inhibition rate is y1=50.211x1+22.736(R 2 =0.9968), when the inhibition rate is 50%, that is, when y1=50, the half inhibition concentration is calculated to be 0.543 mg / mL;
[0129] Process 3: Add the commercial α-glucosidase inhibitor Miglitol into deionized water, and its concentration is 0.1mg / mL, 0.2mg / mL, 0.4mg / mL, 0.6mg / mL, 0.8mg / mL, 1mg / mL, 1.2mg / mL, 1.4mg / mL, 1.6mg / mL, 1.8mg / mL, 2mg / mL, a total of 11 concentration gradients. And use it to replace the tea sample, and establish a linear regression equation according to the operation of process 2. The regression equation is y2=33.863x2+26.180(R 2 =0.9964); when the inhibition rate is 50%, that is, y2=50, the half inhibition concentration is calculated to be 0.703 mg / mL by substituting it into the regression equation;
[0130] From the above results, it can be seen that the components in the tea samples that have an inhibitory effect on α-glucosidase have a better inhibitory effect than miglitol and can be used as inhibitors of α-glucosidase.
[0131] In summary, the present invention is a highly sensitive and highly specific portable electrochemical sensor based on a prismatic rod-shaped four-metal Fe / Co / Ni / Cu MOF@PPy material as a bionic catalyst, which is combined with a smartphone for the detection of α-glucosidase in serum and the screening of α-glucosidase inhibitors from natural products. This detection technology is easy to operate, overcomes the shortcomings of other detection technologies that are easily interfered by color matrix and light, and can achieve timely on-site detection, quickly and accurately screen out green, low-cost natural products with high content of enzyme activity inhibitors, which is conducive to the further development and application of hypoglycemic food resources, and also provides new ideas for food intervention for type 2 diabetes, reducing the burden on diabetic patients and the national medical system, and contributing to the healthy development of society.
[0132] The series of detailed descriptions listed above are only specific descriptions of feasible embodiments of the present invention. They are not intended to limit the scope of protection of the present invention. All equivalent embodiments or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preparing an electrochemical sensor, characterized in that: Here are the steps: Step 1: Preparation of sensing substrate: Process 1: Weigh ferric chloride, cobalt nitrate, nickel nitrate, copper nitrate and 2-aminoterephthalic acid, disperse them in N,N-dimethylformamide to obtain a mixed solution and stir; Process 2: The mixed solution obtained in process 1 is transferred into a reactor, and then placed in an oven for heating reaction. After the heating reaction is completed, a dark brown precipitate is obtained by centrifugation, which is washed with N,N-dimethylformamide and ethanol respectively, and then vacuum dried to obtain a prismatic rod-shaped four-metal Fe / Co / Ni / Cu MOF material; Process 3: Take pyrrole in deionized water, add the prismatic rod-shaped tetrametallic Fe / Co / Ni / Cu MOF material prepared in process 2 under stirring, then perform the first continuous stirring, add ferric chloride after stirring and perform the second stirring; then the product obtained by centrifugation is washed with ethanol and deionized water respectively, and the powder obtained by vacuum drying is recorded as prismatic rod-shaped tetrametallic Fe / Co / Ni / Cu MOF@PPy material; finally, the obtained prismatic rod-shaped tetrametallic Fe / Co / Ni / Cu MOF@PPy material is dispersed in deionized water to obtain a prismatic rod-shaped tetrametallic Fe / Co / Ni / Cu MOF@PPy aqueous solution; Step 2: Preparation of electrochemical sensor: The screen-printed electrode was immersed in H2SO4 solution to activate the electrode. After activation, the H2SO4 solution on the surface was rinsed off with deionized water and dried at room temperature. After drying, it was recorded as screen-printed electrode A. Then, the prismatic rod-shaped four-metal Fe / Co / Ni / Cu MOF@PPy aqueous solution prepared in step 1 was dropped on the working electrode surface of screen-printed electrode A, and an electrochemical sensor was obtained after drying.
2. The method for preparing an electrochemical sensor according to claim 1, characterized in that: The amounts of ferric chloride, cobalt nitrate, nickel nitrate, copper nitrate, 2-aminoterephthalic acid and N,N-dimethylformamide used in process 1 of step 1 are 0.1-0.5 mmol: 0.1-0.5 mmol: 0.1-0.5 mmol: 0.1-0.5 mmol: 30-80 mL.
3. The method for preparing an electrochemical sensor according to claim 1, characterized in that: In process 2 of step 1, the temperature of the heating reaction is 80-160°C, and the reaction time is 12-48h; the number of cleanings is 3-5 times; the centrifugal conditions are: 5000-15000rpm, 5-15min; the temperature of the vacuum drying is 60-70°C, and the time is 12-14h.
4. The method for preparing an electrochemical sensor according to claim 1, characterized in that: In process three of step one, the dosage ratio of pyrrole to deionized water is 50 mg:30 mL; the mass ratio of pyrrole to prismatic rod-shaped four-metal Fe / Co / Ni / Cu MOF powder is 1:1-6; the first continuous stirring time is 30-70 min; the mass ratio of ferric chloride to pyrrole monomer is 1.04:1; the second stirring time is 4-6 h; the centrifugal conditions are: 5000-15000 rpm, 5-15 min; the vacuum drying temperature is 60-80°C; the concentration of the prismatic rod-shaped four-metal Fe / Co / Ni / Cu MOF@PPy aqueous solution is 0.5-3 mg / ml.
5. The method for preparing an electrochemical sensor according to claim 1, characterized in that: The concentration of the H2SO4 solution in step 2 is 1 mol / L; the activation is performed by cyclic voltammetry with 20 cycles; the volume of the prismatic rod-shaped four-metal Fe / Co / Ni / Cu MOF@PPy aqueous solution added is 6 to 10 μL; the drying temperature is 50°C and the drying time is 20 min.
6. A portable electrochemical detection device, characterized in that: An electrochemical sensor prepared by the method according to any one of claims 1-5.
7. A portable electrochemical detection device according to claim 6, characterized in that: The portable electrochemical detection device is composed of a power supply, a Bluetooth module, a microcontroller, an electrical signal conversion module, an electrical signal acquisition module, an electrochemical sensor and an intelligent terminal; The electrical signal conversion module includes an AD converter and a DA converter; The smart terminal is electrically connected to the microcontroller via the Bluetooth module to achieve signal transmission and control; at the same time, the microcontroller is electrically connected to the AD converter and the DA converter respectively; the AD converter is connected to the electrical signal acquisition module; the electrochemical sensor is electrically connected to the DA converter and the electrical signal acquisition module respectively; Use the smart terminal to connect the Bluetooth module and send detection instructions to the microcontroller. After receiving the detection command, the microcontroller converts the digital signal into an analog signal through the DA converter, and applies voltage to the electrochemical sensor through the electrical signal acquisition module. The electrochemical sensor is stimulated to generate a signal, and the analog signal is converted into a digital signal through the AD converter and transmitted back to the microcontroller. The microcontroller then transmits the data to the smart terminal through the Bluetooth module.
8. A portable electrochemical detection device according to claim 7, characterized in that: The power supply is ZMV2405D, the Bluetooth module is nRF52840, and the microcontroller is STM32; the intelligent terminal includes a smart phone; the applied starting voltage is -0.8V and the ending voltage is 0.9V.
9. Use of the portable electrochemical detection device according to any one of claims 6 to 8 for detecting α-glucosidase activity, characterized in that: Here are the steps: Process 1: First, a series of α-glucosidase solutions were prepared with PBS buffer, with concentrations of Q1, Q2, Q3, ..., Q n-1 , Q n , there are n concentration gradients in total, n is a positive integer; Process 2: Mix the 4-nitrophenyl-α-D-pyranoglucoside solution and the α-glucosidase solution in process 1, incubate for a period of time, and then obtain a mixed solution for electrochemical detection; Process 3: During the electrochemical detection process, the intelligent terminal is used to output the start and end voltages required for detection, and the electrochemical sensor is used for detection. The microcontroller collects and stores the current response value generated by the electrochemical sensor; A linear regression model was established based on the correlation between the α-glucosidase concentration and the response current, and the regression equation was y=ax+b, where x represented the α-glucosidase concentration, y represented the current response value, and a and b were constants; Process 4: Detection of α-glucosidase in serum: The serum sample is centrifuged to remove the precipitate, and then diluted with deionized water to obtain a diluted serum sample; the diluted serum sample is mixed with a 4-nitrophenyl-α-D-pyranoglucoside solution, and electrochemical detection is performed after incubation for a period of time, and the obtained current value is substituted into the linear equation of process three to calculate the α-glucosidase concentration in the serum.
10. The use according to claim 9, characterized in that In process 1, the concentration of the PBS buffer is 0.1 mol / L, and the pH is 7.0; the concentration range of the α-glucosidase is 0.002 U / mL to 0.02 U / mL.
11. The use according to claim 9, characterized in that The concentration of the 4-nitrophenyl-α-D-pyranoglucoside solution in process 2 is 6 to 14 mmol / L, and the volume ratio of the 4-nitrophenyl-α-D-pyranoglucoside solution to the α-glucosidase solution is 1 to 5:2 to 10; the concentration of the PBS buffer is 0.1 mol / L, and the pH is 7.0; the incubation temperature is 36 to 40° C., and the incubation time is 20 to 60 min.
12. The use according to claim 9, characterized in that The centrifugation conditions of process four are 4000 rpm, 5 to 10 min; the dilution multiple with deionized water is 100 times; the concentration of the 4-nitrophenyl-α-D-pyranoglucoside solution is 6 to 14 mmol / L, and the volume ratio of the 4-nitrophenyl-α-D-pyranoglucoside solution to the diluted serum sample is 1 to 5:2 to 10; the incubation temperature is 36 to 40°C, and the incubation time is 20 to 60 min.
13. Use of the portable electrochemical detection device according to any one of claims 6 to 8 for screening α-glucosidase inhibitors, characterized in that: Here are the steps: Process 1: Take the sample to be selected and place it in deionized water to obtain a mixed system, extract it by ultrasonication, centrifuge it and collect the supernatant; Process 2: The supernatant was mixed with the α-glucosidase solution for the first incubation. After the incubation, 4-nitrophenyl-α-D-pyranoglucoside was added for the second incubation. After the incubation, electrochemical detection was performed to calculate the inhibition rate of the inhibitor and establish a linear regression equation. The inhibition rate was Where I1 is the current value measured in the presence of α-glucosidase and 4-nitrophenyl-α-D-pyranoglucoside, I x is the current value measured in the presence of only 4-nitrophenyl-α-D-pyranoglucoside, I0 is the current value measured in the presence of α-glucosidase, 4-nitrophenyl-α-D-pyranoglucoside and natural samples; then, based on the mass concentration of the sample in the mixed system and the corresponding inhibition rate, a regression equation is established as y1=a1x1+b1, wherein x1 represents the concentration of the sample, y1 represents the inhibition rate, and a1 and b1 are constants; when the inhibition rate is 50%, the corresponding sample concentration is the half inhibition concentration, recorded as C-0; Process 3: Discrimination: Substitute the candidate sample with the commercial α-glucosidase inhibitor and follow the operation of process 2 to obtain its corresponding half inhibition concentration, recorded as C-1; If the half inhibition concentration of the candidate sample is not higher than C-1, it can be selected as an inhibitor of α-glucosidase.
14. The use according to claim 13, characterized in that Process 1: The mass concentration of the sample in the mixed system is 0.1-2 mg / mL; the centrifugation condition is 8000 rpm, 5-10 min; the samples to be selected include but are not limited to tea, pepper, and wheat.
15. The use according to claim 13, wherein the volume ratio of the supernatant to the α-glucosidase solution and 4-nitrophenyl-α-D-pyranoglucoside in process 2 is 5:3:0.5-2.5, the concentration of the α-glucosidase solution is 0.05U / mL; the first incubation time is 30min, and the incubation temperature is 37°C; the concentration of the 4-nitrophenyl-α-D-pyranoglucoside is 6-14mmol / L; the second incubation temperature is 36-40°C, and the incubation time is 20-60min.
16. The use according to claim 13, wherein the commercial α-glucosidase inhibitors in process 3 include acarbose, voglibose and miglitol.