Method for detecting bipolar plate coating of proton exchange membrane electrolytic cell

By introducing titanium sheets coated with bipolar plates into the electrolytic cell for cyclic activation and long-term operation tests, combined with scanning electron microscopy characterization, the accuracy and actual working conditions of bipolar plate coating evaluation in the prior art were solved. Simulating puzzles enables more efficient coating selection and electrolytic cell performance improvement.

CN118937798AActive Publication Date: 2024-11-12TAN KAH KEE INNOVATION LAB +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411110242.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-12
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

The prior art is difficult to accurately evaluate the life and surface conductivity of the bipolar plate coating of the proton exchange membrane electrolytic cell, and it is difficult to truly restore the corrosion environment under actual working conditions, resulting in coating selection deviations and poor performance.

Method used

The titanium sheet coated with bipolar plate coating was introduced into the electrolytic cell for cyclic activation and long-term operation tests, combined with a field emission scanning electron microscope for morphological characterization and contact resistance tests, and simulate actual working conditions to evaluate the coating. stability and corrosion degree.

Benefits of technology

It realizes accurate screening of suitable bipolar plate coating materials under actual operating conditions, evaluates the life of the coating and surface conductivity, reduces the cost of the electrolytic cell, and improves the efficiency and performance of the electrolytic cell.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118937798A_ABST
    Figure CN118937798A_ABST
Patent Text Reader

Abstract

The invention discloses a method for detecting a bipolar plate coating of a proton exchange membrane electrolytic bath, and relates to the technical field of proton exchange membrane electrolytic baths. The detection method comprises the following steps: assembling a titanium sheet with a bipolar plate coating in an electrolytic bath to obtain the electrolytic bath containing the titanium sheet; and the electrolytic cell containing the titanium sheet is firstly circularly activated under different current densities and then operates under a constant current density, and stability detection of the bipolar plate coating is carried out. A titanium sheet plated with a bipolar plate coating is introduced into the electrolytic bath, and a working condition test is carried out, so that the condition corrosion environment of the electrolytic bath is truly reduced; the method has the advantages that the method is simple and convenient to operate, a thin titanium sheet is used for testing very conveniently, meanwhile, the contact resistance between the coating and a gas diffusion layer of an electrolytic cell can be further evaluated, and morphology characterization such as a scanning electron microscope (SEM) can be performed, so that the service life and the surface conductivity of the bipolar plate coating can be more accurately and intuitively evaluated, and the corrosion degree of the surface of the coating can be evaluated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of proton exchange membrane electrolyzers, and in particular to a method for detecting a bipolar plate coating of a proton exchange membrane electrolyzer. Background Art

[0002] Proton exchange membrane (PEM) water electrolysis hydrogen production technology is regarded as an effective technical solution to the problem of renewable energy conversion and storage. However, the commercial application of this technology is limited by the high cost of electrolyzers. The key to this problem is that the high oxidation potential of the electrolyzer operating conditions requires the use of high-purity titanium metal as the anode bipolar plate material for the electrolyzer bipolar plates. However, the high oxidation potential to which the bipolar plates are subjected during operating conditions will still cause the bipolar plates to passivate and generate a TiO2 layer with poor electrical conductivity. This phenomenon increases the contact resistance at the interface between the bipolar plate and the diffusion layer, reducing the efficiency of the electrolyzer.

[0003] In order to prevent the passivation and corrosion of bipolar plates, it is usually necessary to apply a highly conductive and electrochemical corrosion-resistant coating on their surface. However, most of the current bipolar plate coating evaluation systems are divorced from actual working conditions, resulting in a deviation between the coating evaluation and the actual working conditions. This is not conducive to the research and development of bipolar plate coatings, making it difficult to screen out anti-corrosion coatings with excellent performance under real working conditions, and may also cause some excellent coatings that can withstand PEM water electrolysis conditions to be ignored.

[0004] In the prior art, there is a non-in-situ three-electrode method, with glassy carbon as the counter electrode (CE), saturated calomel as the reference electrode (RE), and the sample as the working electrode (WE). This study tested the corrosion current density of the coating under a simulated corrosion environment inside the PEM electrolyzer and continued at a constant potential of 2V for 100 hours, and then tested the surface conductivity of the coating. However, the actual PEM electrolyzer has a large water flow rate and the conductivity of ultrapure water is extremely low (18.25MΩ·cm), which makes the pH at the interface of the bipolar plate close to neutral.

[0005] Another in-situ three-electrode method also found that the electrochemical oxidation potential of the bipolar plate (about 1V@2A / cm 2 ) is much lower than the voltage of the entire electrolytic cell (about 1.8V@2A / cm 2 ). However, the electrochemical oxidation potential of the actual bipolar plate is related to the conductivity of the water sample and the operating conditions (such as current density, etc.). The complexity of the operating conditions and the difficulty in accurately detecting the corrosion environment at the bipolar plate make the non-in-situ three-electrode coating test method far from the actual operating conditions, making it difficult to accurately evaluate the life and surface conductivity of the bipolar plate coating.

[0006] In addition, there are reports in the prior art that TiN coating is directly sputtered on the bipolar plate of the actual electrolytic cell for working condition testing. However, since the area of ​​the bipolar plate is not the same as the actual electrochemical reaction area, and the oxidation degree of the bipolar plate flow channel groove ridge is not the same, it is difficult to directly test the contact resistance of the bipolar plate coating through the contact resistance equipment to evaluate the conductivity of the coating. At the same time, due to the large volume of the bipolar plate, it is difficult to characterize the morphology of the coating after the reaction through equipment such as scanning electron microscopes and evaluate the degree of corrosion on the coating surface.

[0007] Therefore, it is urgent to develop a method for evaluating bipolar plate coatings and optimize the selection of bipolar plate coating materials in order to more accurately evaluate the life and surface conductivity of the bipolar plate coatings and evaluate the degree of corrosion on the coating surface.

[0008] In view of this, the present invention is proposed. Summary of the invention

[0009] The purpose of the present invention is to provide a detection method for a proton exchange membrane electrolyzer bipolar plate coating. The detection method is suitable for an anti-corrosion coating screening method that meets the actual working conditions, which not only meets the test under the actual working conditions but also facilitates the post-characterization of the coating after a long-term test, and can accurately screen bipolar plate coating materials suitable for PEM water electrolysis conditions, and can more accurately evaluate the life and surface conductivity of the bipolar plate coating, as well as the degree of corrosion on the coating surface.

[0010] In a first aspect, the present invention provides a method for detecting a coating of a bipolar plate of a proton exchange membrane electrolyzer, the method comprising the following steps:

[0011] Assembling the titanium sheet with the bipolar plate coating in an electrolytic cell to obtain an electrolytic cell containing the titanium sheet;

[0012] The electrolytic cell containing the titanium sheet is first activated cyclically at different current densities and then operated at a constant current density to perform stability testing of the bipolar plate coating.

[0013] Furthermore, the electrolytic cell includes a cathode bipolar plate, a cathode diffusion layer, a cathode catalyst layer, a proton exchange membrane, an anode catalyst layer, an anode gas diffusion layer, a titanium sheet with a bipolar plate coating, and an anode bipolar plate stacked in sequence.

[0014] Furthermore, one side of the titanium sheet has a bipolar plate coating, and the bipolar plate coating is in contact with the anode gas diffusion layer.

[0015] Furthermore, the torque for assembling the electrolytic cell is greater than 3 N.m, preferably 4 N.m.

[0016] Furthermore, the compression rate of the anode gas diffusion layer in the thickness direction is less than 20%.

[0017] Furthermore, the thickness of the titanium sheet is 50-150 μm, preferably 100 μm.

[0018] Furthermore, the bipolar plate coating has a thickness of 0.01 to 1 μm.

[0019] Furthermore, the bipolar plate coating includes a metal coating and / or a metal nitride coating.

[0020] Furthermore, the metal in the metal coating includes any one of Ti, Zr, Cr or Pt, or a combination of at least two of them.

[0021] Furthermore, the metal nitride in the metal nitride coating includes any one of TiN, CrN or ZrN, or a combination of at least two of them.

[0022] Furthermore, the cyclic activation and operation of the electrolyzer containing the titanium sheet are carried out in a multi-channel proton exchange membrane electrolyzer test platform.

[0023] Furthermore, before the circulation activation, circulating water needs to be introduced and heated.

[0024] Preferably, the flow rate of the circulating water is 100-300 mL / min, preferably 200 mL / min.

[0025] Preferably, the temperature is raised to 75-85°C, preferably 80°C.

[0026] Furthermore, the cyclic activation at different current densities is specifically as follows:

[0027] 1~5A / cm 2 At least three current densities are selected within the current density range and the system is operated for at least 20 min in each of the selected current densities.

[0028] Furthermore, the operation under the constant current density is specifically as follows:

[0029] 1~5A / cm 2 A constant current density is selected within the current density range and the process is operated at the constant current density for at least 100 h.

[0030] Furthermore, the detection method further comprises the following steps:

[0031] Field emission scanning electron microscopy was used to characterize the morphology of the bipolar plate coating on the surface of the titanium sheet after operation at a constant current density.

[0032] Furthermore, the detection method further comprises the following steps:

[0033] The anode gas diffusion layer of the electrolytic cell is placed between two electrodes, pressure is applied on both sides of the electrodes, and the resistance value R1 under different pressure conditions is recorded;

[0034] After the anode gas diffusion layer of the electrolytic cell and the titanium sheet with the bipolar plate coating are combined, they are placed between two electrodes, pressure is applied on both sides of the electrodes, and the resistance value R2 under different pressure conditions is recorded; wherein the bipolar plate coating is in contact with the anode gas diffusion layer;

[0035] The contact resistance R between the anode gas diffusion layer and the bipolar plate coating of the electrolytic cell is calculated by the following formula I: contact ;

[0036]

[0037] Furthermore, the electrode is a gold-plated copper electrode.

[0038] Furthermore, the pressure range of the pressurizing is 0.1-2 MPa.

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] (1) The detection method of the present invention introduces a titanium sheet coated with a bipolar plate coating into an electrolytic cell and performs an operating condition test to truly restore the corrosion environment of the electrolytic cell.

[0041] (2) The detection method of the present invention is very convenient for testing by introducing a titanium sheet coated with a bipolar plate coating. At the same time, the contact resistance between the coating and the gas diffusion layer of the electrolytic cell can be evaluated, and morphological characterization such as scanning electron microscopy (SEM) can be performed. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0043] Figure 1 The figure is a schematic diagram of the assembly of the electrolytic cell of the present invention.

[0044] Among them, 1 is a cathode bipolar plate, 2 is a cathode diffusion layer, 3 is a cathode catalyst layer, 4 is a proton exchange membrane, 5 is an anode catalyst layer, 6 is an anode gas diffusion layer, 7 is a titanium sheet with a bipolar plate coating, and 8 is an anode bipolar plate.

[0045] Figure 2A This is a schematic diagram of the contact resistance test of the anode gas diffusion layer of the present invention.

[0046] Figure 2B The figure is a schematic diagram of the contact resistance test of the anode gas diffusion layer of the electrolytic cell of the present invention and the titanium sheet with the bipolar plate coating after being combined.

[0047] Among them, 101 is a power source, 102 is a current collector, 103 is a gold-plated copper electrode, 6 is an anode gas diffusion layer, 7 is a titanium sheet with a bipolar plate coating, and 71 is a bipolar plate coating.

[0048] Figure 3 Polarization curve diagram of the Pt and TiN coatings provided in Example 1 and Example 2 when applied in an electrolytic cell.

[0049] Figure 4 Polarization curve decoupling diagram of the Pt and TiN coatings provided in Example 1 and Example 2 applied in an electrolytic cell.

[0050] Figure 5 This is a diagram of the decay rates of the Pt and TiN coatings provided in Example 1 and Example 2 when applied in an electrolytic cell.

[0051] Figure 6 This is a contact resistance test diagram of the Pt and TiN coatings provided in Example 1 and Example 2 after stability testing in an electrolytic cell.

[0052] Fig. 7A This is a scanning electron microscope image of the TiN coating surface before reaction provided in Example 2.

[0053] Figure 7B This is a scanning electron microscope image of the TiN coating surface after the 400h operating condition test provided in Example 2.

[0054] Fig. 8A This is the surface picture of the TiN coating that was not tested.

[0055] Figure 8B This is a surface image of the TiN coating after the 400h operating condition test provided in Example 2 of the present invention.

[0056] Figure 8C Surface image of the TiN coating after the three-electrode method test provided in Comparative Example 1 of the present invention.

[0057] Fig. 9 This is a comparison chart of contact resistance after testing by the method provided in Example 2 of the present invention and the three-electrode method provided in Comparative Example 1.

[0058] Fig. 10A The operating condition diagram of the bipolar plate coating before and after the reaction provided for Comparative Example 2.

[0059] Fig. 10B The operating diagram for directly using a bipolar plate to test contact resistance is provided for Comparative Example 2. DETAILED DESCRIPTION

[0060] Unless otherwise defined herein, scientific and technical terms used in conjunction with the present invention shall have the meanings commonly understood by those of ordinary skill in the art. The meaning and scope of the terms should be clear, however, in the case of any potential ambiguity, the definitions provided herein take precedence over any dictionary or external definitions. In this application, unless otherwise stated, the use of "or" means "and / or". In addition, the use of the term "including" and other forms is non-limiting.

[0061] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0062] In addition, the technical features involved in different embodiments of the present application described below can be combined with each other as long as they do not conflict with each other.

[0063] In a first aspect, the present invention provides a method for detecting a coating of a bipolar plate of a proton exchange membrane electrolyzer, the method comprising the following steps:

[0064] Assembling the titanium sheet with the bipolar plate coating in an electrolytic cell to obtain an electrolytic cell containing the titanium sheet;

[0065] The electrolytic cell containing the titanium sheet is first activated cyclically at different current densities and then operated at a constant current density to perform stability testing of the bipolar plate coating.

[0066] In the detection method described in the present invention, a titanium sheet coated with a bipolar plate coating is introduced into the electrolytic cell, and an operating condition test is carried out to truly restore the corrosion environment of the electrolytic cell. It is very convenient to introduce a titanium sheet coated with a bipolar plate coating for testing, and the anti-corrosion coating screening method suitable for actual working conditions not only meets the test under actual working conditions, but also facilitates the post-characterization of the coating after a long period of testing. It can accurately screen bipolar plate coating materials suitable for PEM water electrolysis conditions, and can more accurately evaluate the life and surface conductivity of the bipolar plate coating, as well as evaluate the degree of corrosion on the coating surface.

[0067] As an optional embodiment of the present invention, Figure 1 As shown, the electrolytic cell includes a cathode bipolar plate 1, a cathode diffusion layer 2, a cathode catalyst layer 3, a proton exchange membrane 4, an anode catalyst layer 5, an anode gas diffusion layer 6, a titanium sheet 7 with a bipolar plate coating, and an anode bipolar plate 8 which are stacked in sequence.

[0068] In the present invention, before the stability test of the bipolar plate coating is carried out, the cathode bipolar plate 1, the cathode diffusion layer 2, the cathode catalyst layer 3, the proton exchange membrane 4, the anode catalyst layer 5, the anode gas diffusion layer 6, the titanium sheet 7 with the bipolar plate coating, and the anode bipolar plate 8 are assembled in order according to the positions of the positioning holes (that is, the titanium sheet 7 with the bipolar plate coating is assembled between the anode gas diffusion layer 6 and the anode bipolar plate 8). During the assembly process, the battery can be clamped using fastening bolts, nuts and a torque wrench.

[0069] As an optional embodiment of the present invention, one side of the titanium sheet 7 with a bipolar plate coating has a bipolar plate coating, and the bipolar plate coating is in contact with the anode gas diffusion layer 6 .

[0070] As an optional embodiment of the present invention, the torque for assembling the electrolytic cell is above 3 N.m, for example, it may be 3 N.m, 3.2 Nm, 3.4 Nm, 3.6 Nm, 3.8 Nm, 4 N.m, 4.2 Nm, 4.4 Nm, 4.5 Nm, etc.

[0071] As a preferred embodiment of the present invention, the torque for assembling the electrolytic cell is 4 N.m.

[0072] It should be noted that the present invention uses fastening bolts, nuts and torque wrenches to clamp the battery, and the battery assembly force should meet the following requirements: the torque is above 3 N.m, preferably 4 N.m, to ensure that the contact resistance between the gas diffusion layer and the bipolar plate is minimized.

[0073] As an optional embodiment of the present invention, the compression rate of the anode gas diffusion layer in the thickness direction is less than 20%, for example, it can be 19%, 18%, 17%, 16%, 15%, 14%, 13%, 12%, 11%, 10%, etc.

[0074] As an optional embodiment of the present invention, the thickness of the titanium sheet is 50 to 150 μm, for example, it can be 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 95 μm, 100 μm, 105 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, etc.

[0075] As a preferred embodiment of the present invention, the thickness of the titanium sheet is 100 μm.

[0076] As an optional embodiment of the present invention, the thickness of the bipolar plate coating is 0.01 to 1 μm, for example, 0.001 μm, 0.005 μm, 0.1 μm, 0.2 μm, 0.4 μm, 0.6 μm, 0.8 μm, 1 μm, etc.

[0077] As an optional embodiment of the present invention, the bipolar plate coating includes a metal coating and / or a metal nitride coating.

[0078] As an optional embodiment of the present invention, the metal in the metal coating includes any one of Ti, Zr, Cr or Pt, or a combination of at least two of them.

[0079] As an optional embodiment of the present invention, the metal nitride in the metal nitride coating includes any one of TiN, CrN or ZrN, or a combination of at least two of them.

[0080] As an optional embodiment of the present invention, the cyclic activation and operation of the electrolyzer containing the titanium sheet is carried out in a multi-channel proton exchange membrane electrolyzer test platform.

[0081] As an optional implementation mode of the present invention, circulating water needs to be introduced and heated before the cyclic activation.

[0082] More specifically, the steps of the stability test of the bipolar plate coating are as follows: the electrolytic cell containing the titanium sheet is installed on a multi-channel proton exchange membrane electrolytic cell test platform, circulating water is introduced and the temperature is increased, and then the bipolar plate coating is first activated under different current densities and then operated under a constant current density to perform a stability test on the bipolar plate coating.

[0083] As an optional embodiment of the present invention, the flow rate of the circulating water is 100-300 mL / min, for example, it can be 100 mL / min, 120 mL / min, 140 mL / min, 160 mL / min, 180 mL / min, 220 mL / min, 240 mL / min, 260 mL / min, 280 mL / min, 300 mL / min, etc.

[0084] As a preferred embodiment of the present invention, the flow rate of the circulating water is 200 mL / min.

[0085] As an optional embodiment of the present invention, the temperature is raised to 75-85, for example, it can be 75, 76, 77, 78, 79, 80, 81, 82, 83, 84, 85, etc.

[0086] As a preferred embodiment of the present invention, the temperature is raised to 80.degree.

[0087] As an optional embodiment of the present invention, the cyclic activation at different current densities specifically includes the following steps:

[0088] 1~5A / cm 2 At least three current densities are selected within the current density range and the system is operated for at least 20 min in each of the selected current densities.

[0089] As an optional embodiment of the present invention, the current density range is 1 to 5 A / cm 2 , for example, it can be 1A / cm 2 , 1.5A / cm 2 , 2A / cm 2 , 2.5A / cm 2 、3A / cm 2 、3.5A / cm 2 , 4A / cm 2 , 4.5A / cm 2 , 5A / cm 2 Select at least three current densities within the equation.

[0090] As an optional embodiment of the present invention, the operation is performed within the selected current density for at least 20 min, for example, 20 min, 22 min, 24 min, 26 min, 28 min, 30 min, 32 min, 34 min, 35 min, 40 min, etc.

[0091] As a preferred embodiment of the present invention, the cyclic activation at different current densities specifically includes the following steps:

[0092] At a current of 2A / cm 2 、3A / cm 2 , 4A / cm 2 Each run was for 30 min, and the cycle was repeated three times.

[0093] As an optional embodiment of the present invention, the operation under constant current density specifically includes the following steps:

[0094] 1~5A / cm 2 A constant current density is selected within the current density range and the process is operated at the constant current density for at least 100 h.

[0095] As an optional embodiment of the present invention, the current density range is 1 to 5 A / cm 2 , for example, it can be 1A / cm 2 , 1.5A / cm 2 , 2A / cm 2 , 2.5A / cm 2 、3A / cm 2 、3.5A / cm 2 , 4A / cm 2 , 4.5A / cm 2 , 5A / cm 2 A constant current density is selected.

[0096] As an optional embodiment of the present invention, the running time is at least 100 hours, for example, it can be 100 hours, 150 hours, 200 hours, 250 hours, 300 hours, 350 hours, 400 hours, 450 hours, 500 hours, 550 hours, 600 hours, etc.

[0097] As a preferred embodiment of the present invention, the operation under constant current density specifically comprises the following steps:

[0098] After the cycle activation is completed, the electrolytic cell containing the titanium sheet is heated at 2A / cm 2 The battery was operated for 400 h at a current density range of 200 ℃ and 800 ℃.

[0099] In the present invention, the stability detection of the bipolar plate coating includes but is not limited to: drawing of polarization curves, decoupling of polarization curves and calculation of voltage decay rate.

[0100] The drawing of the polarization curve refers to: a curve representing the relationship between the electrode potential and the polarization current or polarization current density, that is, recording the corresponding voltage at different current densities, and drawing the polarization curve with the current density as the horizontal coordinate and the voltage as the vertical coordinate.

[0101] The decoupling of the polarization curves refers to: ηOER refers to the OER overpotential of the electrolytic cell performance; ηohm refers to the ohmic overpotential of the electrolytic cell performance; ηmt refers to the mass transfer overpotential of the electrolytic cell performance. 2 -0.1A / cm 2 The Tafel curve of the electrolyzer device can be calculated from the polarization curve within the current density range, and thus the OER overpotential under the entire current density can be calculated; the ohmic overpotential of the electrolyzer device can be calculated by testing the high-frequency resistance of the electrolyzer (ηohm=I×R); the mass transfer overpotential ηmt can be obtained by subtracting the OER overpotential and the ohmic overpotential from the total overpotential of the electrolyzer.

[0102] The calculation of the voltage decay rate refers to: running for a long time under a constant current density range, and counting the voltage values ​​at different times, drawing a curve graph, and calculating the decay rate of the device.

[0103] As an optional embodiment of the present invention, the detection method further comprises the following steps:

[0104] Field emission scanning electron microscopy was used to characterize the morphology of the bipolar plate coating on the surface of the titanium sheet after operation at a constant current density.

[0105] In the present invention, a field emission scanning electron microscope (SEM) is further used to characterize the surface morphology of the coating after the working condition test (i.e., the bipolar plate coating on the surface of the titanium sheet after long-term operation under constant current density). After a long period of working condition operation, the surface of the bipolar plate coating is observed to see if there is corrosion, so as to more intuitively and accurately detect whether the bipolar plate coating can withstand the corrosive environment of the bipolar plate.

[0106] As an optional embodiment of the present invention, the detection method further comprises the following steps (such as Figure 2A and Figure 2B shown):

[0107] The anode gas diffusion layer of the electrolytic cell is placed between two electrodes, pressure is applied on both sides of the electrodes, and the resistance value R1 under different pressure conditions is recorded;

[0108] After the anode gas diffusion layer of the electrolytic cell and the titanium sheet with the bipolar plate coating are combined, they are placed between two electrodes, and pressure is applied on both sides of the electrodes to record the resistance value R2 under different pressure conditions; wherein the bipolar plate coating 71 is in contact with the anode gas diffusion layer 6;

[0109] The contact resistance R between the anode gas diffusion layer and the bipolar plate coating of the electrolytic cell is calculated by the following formula I: contact ;

[0110]

[0111] In the present invention, the above steps are further used to perform a contact resistance test on the coating after the operating condition test (i.e., the bipolar plate coating on the surface of the titanium sheet after long-term operation under a constant current density) to more intuitively and accurately detect whether the bipolar plate coating still maintains good conductivity after long-term operation.

[0112] As an optional implementation manner of the present invention, the electrode is a gold-plated copper electrode 103 .

[0113] As an optional embodiment of the present invention, the pressure range of the applied pressure is 0.1-2 MPa, for example, it can be 0.1 MPa, 0.2 MPa, 0.4 MPa, 0.6 MPa, 0.8 MPa, 1 MPa, 1.2 MPa, 1.4 MPa, 1.6 MPa, 1.8 MPa, 2 MPa, etc.

[0114] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0115] Example 1

[0116] This embodiment provides a method for detecting a coating of a bipolar plate of a proton exchange membrane electrolyzer, the method comprising the following steps:

[0117] S1. Working condition bipolar plate coating test method:

[0118] According to the position of the positioning holes, the cathode bipolar plate, cathode diffusion layer, cathode catalyst layer, proton exchange membrane, anode catalyst layer, anode gas diffusion layer, titanium sheet with bipolar plate coating (the titanium sheet thickness is 100 μm, and the bipolar plate coating is Pt coating with a thickness of 0.3 μm), and anode bipolar plate are assembled in order (the titanium sheet of the anode bipolar plate is cut into 20 mm*20 mm, and the double corners are cut off to allow the anode circulating water to flow in), and the battery is clamped using fastening bolts, nuts and a torque wrench. The battery assembly force should meet the following requirements: the torque is 4 N.m to ensure that the contact resistance between the gas diffusion layer and the bipolar plate is minimized, and the compression rate of the cathode diffusion layer in the thickness direction is <20%.

[0119] S2. Electrolyzer bipolar plate coating stability test:

[0120] The electrolyzer was installed on the multi-channel proton exchange membrane electrolyzer test platform, and circulating water (flow rate 200 ml / min) was introduced. After the temperature rose to 80°C, the current was 2A / cm 2 、3A / cm 2 , 4A / cm 2 The activation process was completed and the electrolytic cell was maintained at 2A / cm 2 The system was operated for 400 h at a current density of ; the polarization curve, polarization curve decoupling diagram, and attenuation rate diagram in the electrolytic cell were drawn respectively.

[0121] S3. Contact resistance test of bipolar plate coating and gas diffusion layer:

[0122] The anode gas diffusion layer of the electrolytic cell is placed between two electrodes, pressure (0.1-2.0 MPa) is applied to both sides of the electrodes, and the resistance value R1 under different pressure conditions is recorded;

[0123] After the anode gas diffusion layer of the electrolytic cell and the titanium sheet with the bipolar plate coating are combined, they are placed between two electrodes, and pressure (0.1-2.0 MPa) is applied on both sides of the electrodes, and the resistance value R2 under different pressure conditions is recorded; wherein the bipolar plate coating is in contact with the anode gas diffusion layer; the bipolar plate coating is the bipolar plate coating on the surface of the titanium sheet after running for 400 hours at a constant current density;

[0124] The contact resistance R between the anode gas diffusion layer and the bipolar plate coating of the electrolytic cell is calculated by the following formula I: contact ;

[0125]

[0126] S4. Scanning electron microscope observation:

[0127] Field emission scanning electron microscopy was used to characterize the morphology of the bipolar plate coating on the surface of the titanium sheet after running at a constant current density for 400 hours.

[0128] Example 2

[0129] This embodiment provides a method for detecting a coating of a bipolar plate of a proton exchange membrane electrolyzer, the method comprising the following steps:

[0130] S1. Working condition bipolar plate coating test method:

[0131] According to the position of the positioning holes, the cathode bipolar plate, cathode diffusion layer, cathode catalyst layer, proton exchange membrane, anode catalyst layer, anode gas diffusion layer, titanium sheet with bipolar plate coating (the titanium sheet thickness is 100 μm, and the bipolar plate coating is TiN coating with a thickness of 0.3 μm), and anode bipolar plate are assembled in order (the titanium sheet of the anode bipolar plate is cut into 20 mm*20 mm, and the double corners are cut off to allow the anode circulating water to flow in), and the battery is clamped using fastening bolts, nuts and a torque wrench. The battery assembly force should meet the following requirements: the torque is 4 N.m to ensure that the contact resistance between the gas diffusion layer and the bipolar plate is minimized, and the compression rate of the cathode diffusion layer in the thickness direction is <20%.

[0132] S2. Electrolyzer bipolar plate coating stability test:

[0133] The electrolyzer was installed on the multi-channel proton exchange membrane electrolyzer test platform, and circulating water (flow rate 200 mL / min) was introduced. After the temperature rose to 80°C, the current was 2 A / cm 2 、3A / cm 2 , 4A / cm 2 The activation process was completed and the electrolytic cell was maintained at 2A / cm 2 The system was operated for 400 h at a current density of ; the polarization curve, polarization curve decoupling diagram, and attenuation rate diagram in the electrolytic cell were drawn respectively.

[0134] S3. Contact resistance test of bipolar plate coating and gas diffusion layer:

[0135] The anode gas diffusion layer of the electrolytic cell is placed between two electrodes, pressure (0.1-2.0 MPa) is applied to both sides of the electrodes, and the resistance value R1 under different pressure conditions is recorded;

[0136] After the anode gas diffusion layer of the electrolytic cell and the titanium sheet with the bipolar plate coating are combined, they are placed between two electrodes, and pressure (0.1-2.0 MPa) is applied on both sides of the electrodes, and the resistance value R2 under different pressure conditions is recorded; wherein the bipolar plate coating is in contact with the anode gas diffusion layer; the bipolar plate coating is the bipolar plate coating on the surface of the titanium sheet after running for 400 hours at a constant current density;

[0137] The contact resistance R between the anode gas diffusion layer and the bipolar plate coating of the electrolytic cell is calculated by the following formula I: contact ;

[0138]

[0139] S4. Scanning electron microscope observation:

[0140] Field emission scanning electron microscopy was used to characterize the morphology of the bipolar plate coating on the surface of the titanium sheet after running at a constant current density for 400 hours.

[0141] The test results of the steps of the above-mentioned embodiment 1 and embodiment 2 are as follows:

[0142] Figure 3 Polarization curves of the Pt and TiN coatings provided in Examples 1 and 2 when applied to an electrolytic cell. Figure 3 As shown, sputtering Pt coating and TiN coating on the surface of the titanium sheet improves the performance of the overall electrolytic cell.

[0143] Figure 4 The Pt and TiN coatings provided in Example 1 and Example 2 are applied to the polarization curve decoupling diagram in the electrolytic cell. Figure 4 As shown in the figure, through the overpotential decomposition of the polarization curve, it can be seen that the improvement in the performance of the electrolyzer is mainly reflected in the reduction of the ohmic overpotential. This shows that the application of Pt coating and TiN coating reduces the contact resistance at the interface between the titanium bipolar plate and the diffusion layer, and improves the performance of the electrolyzer and the electrolysis efficiency. After using highly conductive Pt coating and TiN coating as the titanium bipolar plate coating, the stability of the overall device has been improved.

[0144] Figure 5 The attenuation rate diagram of the Pt and TiN coatings provided in Example 1 and Example 2 when applied in an electrolytic cell. Figure 5 As shown, the decay rate of the uncoated bipolar plate is 65.2μV / h, while the decay rates of the device after using the corrosion-resistant and highly conductive TiN and Pt coatings are 32.6μV / h and 37.8μV / h, and the stability is improved compared to the uncoated titanium bipolar plate.

[0145] Figure 6The contact resistance test diagram of the Pt and TiN coatings provided in Example 1 and Example 2 after stability test in the electrolytic cell. Figure 6 As shown, the contact resistance test was carried out on the Pt coating and the TiN coating after 400 hours of the operating condition test. The TiN coating and the Pt coating still maintained good conductivity after the 400 hours of operating condition stability test.

[0146] Fig. 7A This is a scanning electron microscope image of the TiN coating surface before reaction provided in Example 2. Figure 7B This is a scanning electron microscope image of the TiN coating surface after the 400h operating condition test provided in Example 2. Fig. 7A and Figure 7B From the comparison, it can be seen that after a long period of 400 hours of operation, there is no obvious corrosion on the surface of the TiN coating, which indicates that the TiN coating can withstand the corrosive environment of the bipolar plate.

[0147] In summary, in order to prevent oxidation and corrosion of the bipolar plates during long-term operation of the electrolyzer, corrosion-resistant and highly conductive coatings are needed to improve the performance and electrolysis efficiency of the electrolyzer. Pt and TiN are key materials that can be used in bipolar plate coatings for PEM electrolyzers in the future.

[0148] Comparative Example 1

[0149] This comparative example provides a three-electrode testing method, which specifically includes the following steps:

[0150] The coating to be tested is used as the working electrode, mercurous sulfate or reversible hydrogen electrode is used as the reference electrode, and carbon rod is used as the counter electrode to test in an H-type electrolytic cell. Air or oxygen is introduced into the electrolyte solution of H2SO4 at a temperature of 80°C, F-content of 0.1 mg / L, pH=3 at a flow rate of 20 mL / min to simulate the anode environment of the electrolytic cell. A potential of 2 V (vs. RHE) is applied to the sample in the simulated anode environment and maintained for at least 100 h.

[0151] The comparison results of the above-mentioned Example 2 and Comparative Example 1 are as follows:

[0152] Fig. 8A This is the surface image of the TiN coating that has not been tested. Fig. 8A As shown, the initial TiN coating surface appears golden yellow.

[0153] Figure 8B This is a surface image of the TiN coating after a 400h working condition test provided in Example 2 of the present invention. Figure 8B As shown, after 400 hours of testing using the working condition detection method of the present invention, the TiN coating on the surface of the titanium sheet becomes slightly darker and is only partially oxidized.

[0154] Figure 8C The surface image of the TiN coating after the three-electrode method test provided in Comparative Example 1 of the present invention. Figure 8C As shown, after only 24 hours of testing using the traditional three-electrode method, the TiN coating had completely fallen off and a light yellow TiO2 layer was generated on the surface of the titanium sheet.

[0155] Fig. 9 This is a comparison chart of the contact resistance after testing by the method provided in Example 2 of the present invention and the three-electrode method provided in Comparative Example 1. Fig. 9 As shown, after 24 hours of testing using the traditional three-electrode method, the contact resistance on the titanium sheet surface is much greater than the contact resistance after testing using the operating condition detection method.

[0156] In summary, the traditional three-electrode test method provided in Comparative Example 1 is significantly different from the actual working conditions, seriously overestimates the corrosion environment of the bipolar plate in the PEM electrolyzer, and is difficult to accurately screen the bipolar plate coating.

[0157] Comparative Example 2

[0158] This comparative example provides a conventional bipolar plate operating condition detection method, which specifically includes the following steps:

[0159] The coating to be tested is deposited on the surface of the bipolar plate of the electrolyzer by electroplating or magnetron sputtering. The electrolyzer is installed on the multi-channel proton exchange membrane electrolyzer test platform, and circulating water is passed through at a constant current density (such as 2A / cm 2 The stability test was carried out with the current density of 10000 Ω.

[0160] The comparison results of the above-mentioned Example 2 and Comparative Example 2 are as follows:

[0161] Fig. 10A The working condition diagram of the bipolar plate coating before and after the reaction provided for Comparative Example 2. Fig. 10A As shown, the coating is directly sputtered onto the bipolar plate for operating condition testing. Since the tight packaging of the PEM water electrolysis device requires bolt positioning holes, the area of ​​the bipolar plate is larger than the actual reaction active area. Therefore, this method is difficult to accurately quantify key properties such as the conductivity of the surface coating after the actual reaction.

[0162] Fig. 10B The working condition diagram of directly using the bipolar plate to test the contact resistance provided in Comparative Example 2. Fig. 10B As shown, the bipolar plates are thick and large in area, requiring large equipment to analyze the surface coating, which makes it very inconvenient to characterize the surface morphology of the coating after operating condition testing.

[0163] In summary, the bipolar plate working condition detection method proposed in the present invention not only truly restores the actual working condition test environment of the bipolar plate in the PEM electrolyzer, but also improves the convenience of characterizing the key properties of the coating. The method has a high degree of accuracy, can effectively solve the problem of bipolar plate coating detection, optimize the selection of coating materials, and thus reduce the cost of the entire electrolyzer.

[0164] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for detecting a coating of a bipolar plate of a proton exchange membrane electrolyzer, characterized in that: The detection method comprises the following steps: Assembling the titanium sheet with the bipolar plate coating in an electrolytic cell to obtain an electrolytic cell containing the titanium sheet; The electrolytic cell containing the titanium sheet is first activated cyclically at different current densities and then operated at a constant current density to perform stability testing of the bipolar plate coating.

2. The method for detecting the coating of the bipolar plate of a proton exchange membrane electrolyzer according to claim 1, characterized in that: The electrolytic cell comprises a cathode bipolar plate, a cathode diffusion layer, a cathode catalyst layer, a proton exchange membrane, an anode catalyst layer, an anode gas diffusion layer, a titanium sheet with a bipolar plate coating, and an anode bipolar plate which are stacked in sequence.

3. The method for detecting the coating of the bipolar plate of a proton exchange membrane electrolyzer according to claim 1 or 2, characterized in that: One side of the titanium sheet has a bipolar plate coating, and the bipolar plate coating is in contact with the anode gas diffusion layer; and / or, the torque for assembling the electrolytic cell is 3 N.m or more, preferably 4 N.m; And / or, the compression ratio of the anode gas diffusion layer in the thickness direction is less than 20%.

4. The method for detecting the coating of the bipolar plate of a proton exchange membrane electrolyzer according to claim 1 or 2, characterized in that: The thickness of the titanium sheet is 50 to 150 μm, preferably 100 μm; and / or, the bipolar plate coating has a thickness of 0.01 to 1 μm; and / or, the bipolar plate coating comprises a metal coating and / or a metal nitride coating; And / or, the metal in the metal coating includes any one of Ti, Zr, Cr or Pt or a combination of at least two thereof; And / or, the metal nitride in the metal nitride coating includes any one of TiN, CrN or ZrN, or a combination of at least two of them.

5. The method for detecting the coating of the bipolar plate of a proton exchange membrane electrolyzer according to claim 1, characterized in that: The cyclic activation and operation of the electrolyzer containing the titanium sheet are carried out in a multi-channel proton exchange membrane electrolyzer test platform.

6. The method for detecting the coating of the bipolar plate of a proton exchange membrane electrolyzer according to claim 1, characterized in that: Before the cycle activation, circulating water needs to be introduced and heated; Preferably, the flow rate of the circulating water is 100 to 300 mL / min, preferably 200 mL / min; Preferably, the temperature is raised to 75-85°C, preferably 80°C.

7. The method for detecting the coating of the bipolar plate of a proton exchange membrane electrolyzer according to claim 1, characterized in that: The cyclic activation at different current densities is specifically as follows: 1~5A / cm 2 Select at least three current densities within the current density range and run each of the selected current densities for at least 20 min; And / or, the operation under the constant current density is specifically: 1~5A / cm 2 A constant current density is selected within the current density range and the process is operated at the constant current density for at least 100 h.

8. The method for detecting the coating of the bipolar plate of a proton exchange membrane electrolyzer according to claim 1, characterized in that: The detection method further comprises the following steps: Field emission scanning electron microscopy was used to characterize the morphology of the bipolar plate coating on the surface of the titanium sheet after operation at a constant current density.

9. The method for detecting the coating of the bipolar plate of a proton exchange membrane electrolyzer according to claim 1 or 2, characterized in that: The detection method further comprises the following steps: The anode gas diffusion layer of the electrolytic cell is placed between two electrodes, pressure is applied on both sides of the electrodes, and the resistance value R1 under different pressure conditions is recorded; After combining the anode gas diffusion layer of the electrolytic cell and the titanium sheet with the bipolar plate coating, the two electrodes are placed between each other, and pressure is applied on both sides of the electrodes to record the resistance value R2 under different pressure conditions; wherein the bipolar plate coating is in contact with the anode gas diffusion layer; The contact resistance R between the anode gas diffusion layer and the bipolar plate coating of the electrolytic cell is calculated by the following formula I: contact ; 10. The method for detecting the coating of the bipolar plate of a proton exchange membrane electrolyzer according to claim 9, characterized in that: The electrode is a gold-plated copper electrode; And / or, the pressure range of the pressurizing is 0.1-2 MPa.

Citation Information

Patent Citations

  • Metal-based bipolar plate used for PEMFC and preparation method thereof

    CN110061257A

  • On-site rapid spot check method for coating quality of metal bipolar plate

    CN112285013A

  • System and method for testing corrosion resistance of metal bipolar plate and coating of hydrogen fuel cell for automobile

    CN114976135A

  • Cathode bipolar plate of proton exchange membrane electrolytic cell and preparation method of cathode bipolar plate

    CN117165987A

  • Field monitoring electrochemical method for anticorrosion performance of organic coatings in seawater environment