Negative photosensitive resin composition and method for producing cured relief pattern
By using a negative photosensitive resin composition, polyimide and urea bonding compound containing polymerizable functional groups, the problems of curing shrinkage and insufficient adhesion during low-temperature curing in the prior art are solved, and high performance is achieved Production of photosensitive resin composition and cured relief patterns thereof.
Patent Information
- Application Number
- CN202410568394.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-10
- Filing Date
- 2024-05-09
- Publication Date
- 2024-11-12
AI Technical Summary
The conventional photosensitive resin composition has problems of curing and shrinking under low temperature curing conditions, resulting in insufficient heat resistance and mechanical strength, and insufficient adhesion with copper and oxygen barrier properties.
Using a negative photosensitive resin composition, it comprises a polyimide having a polymerizable functional group at the end, a polymerizable compound having a urea bond, a photopolymerization initiator and other additives, such as a silane coupling agent and an organic titanium compound, A cured relief pattern is formed by specific processes such as coating, exposure, development and heating treatment.
It has achieved low curing shrinkage, excellent heat resistance, mechanical strength, copper adhesion and oxygen barrier properties, and is suitable for the manufacturing of semiconductor devices and multi-layer circuits.
Smart Images

Figure BDA0004830101500000061 
Figure BDA0004830101500000071 
Figure BDA0004830101500000081
Abstract
Description
Technical Field
[0001] The present application relates to a negative photosensitive resin composition and a method for producing a cured relief pattern. Background Art
[0002] In the past, polyimide resins, polybenzoxazole resins, phenolic resins, etc., which have excellent heat resistance, electrical properties, and mechanical properties, were used in insulating materials of electronic components and passivation films, surface protection films, and interlayer insulating films of semiconductor devices. Among these resins, the material provided in the form of a photosensitive resin composition can easily form a heat-resistant relief pattern coating through coating, exposure, development, and curing-based closed-loop treatment (imidization, benzoxazoleization), and thermal crosslinking of the composition. Therefore, it has the characteristic of greatly shortening the process compared with the previous non-photosensitive materials, and is used in the production of semiconductor devices.
[0003] In addition, semiconductor devices (hereinafter also referred to as "components") are mounted on printed circuit boards using various methods depending on the purpose. Conventional components are generally manufactured by wire bonding, which uses thin wires to connect the external terminals (pads) of the component to the lead frame. However, as components are becoming increasingly high-speed and the operating frequency has reached GHz, the difference in the wiring length of each terminal during installation has reached a level that affects the operation of the component. Therefore, in the installation of components for high-end applications, it is necessary to accurately control the length of the installation wiring, and it is difficult to meet this requirement through wire bonding.
[0004] Therefore, a flip chip mounting has been proposed, in which a rewiring layer is formed on the surface of a semiconductor chip, bumps (electrodes) are formed thereon, and then the chip is turned over (flipped) and mounted directly on a printed circuit board. This flip chip mounting is adopted in high-end components that process high-speed signals because it can accurately control the wiring distance, or in mobile phones and the like because of its small mounting size, and its demand is rapidly increasing.
[0005] Furthermore, a semiconductor chip mounting technology called fan-out wafer level packaging (FOWLP) has recently been proposed, in which a wafer that has completed the previous process is cut to produce individual chips, and then the individual chips are rebuilt on a support body and sealed with a molding resin. After the support body is peeled off, a rewiring layer is formed. FOWLP has the following advantages: since the rewiring layer is formed with a thin film thickness, the height of the package can be reduced, and high-speed transmission and low cost can be achieved.
[0006] Currently, the photosensitive polyimide precursor widely used in FOWLP requires an imidization step by heating.
[0007] On the other hand, in FOWLP, the package is easily warped by heating during the process due to thinning. From the viewpoint of suppressing the warping, the curing temperature of the photosensitive resin composition used in device production is desired to be lowered, preferably to 200° C. or lower.
[0008] For example, Patent Document 1 discloses that a polyimide precursor is cured at a low temperature of 200° C. or lower.
[0009] In addition, when the photosensitive resin composition is cured at a low temperature, it has low cure shrinkage and high heat resistance, which contributes to suppressing warping.
[0010] Furthermore, when a film is formed on a substrate using a photosensitive resin composition containing polyamide and the film is heated to ring-close the polyamide to form polyimide, the film may shrink due to the ring-closure reaction and dehydration accompanying the ring-closure reaction.
[0011] For example, Patent Document 2 discloses a photosensitive resin composition containing a solvent-soluble polyimide having an imide ring structure, from the viewpoint of eliminating the need for an imidization step by heating and suppressing cure shrinkage.
[0012] Furthermore, from the viewpoint of not only suppressing warpage but also improving reliability of the element, the photosensitive resin composition is required to have high adhesion to copper and high oxygen barrier properties.
[0013] Prior art literature
[0014] Patent Literature
[0015] Patent Document 1: Japanese Patent Application Publication No. 2022-091355
[0016] Patent Document 2: Japanese Patent Application Publication No. 2021-162834 Summary of the invention
[0017] Problem that the invention aims to solve
[0018] Patent Document 1 has a problem that the side chain part volatilizes during imidization, so the curing shrinkage becomes large. Furthermore, imidization does not proceed sufficiently under low-temperature curing conditions, and heat resistance and mechanical strength (elongation of the cured film) are insufficient.
[0019] In addition, Patent Document 2 has a problem that important characteristics related to device reliability, namely, adhesion with copper and oxygen barrier properties are insufficient.
[0020] The object of the present invention is to provide a negative photosensitive resin composition having low cure shrinkage, excellent heat resistance, mechanical strength (elongation of the cured film), adhesion to copper and oxygen barrier properties among the film properties after low-temperature curing, and a method for producing a cured relief pattern.
[0021] Solutions for solving problems
[0022] That is, the present invention is as follows. [1]
[0024] A negative photosensitive resin composition comprising:
[0025] (A) a polyimide having a polymerizable functional group at the terminal,
[0026] (B) a polymerizable compound having a urea bond, and
[0027] (C) Photopolymerization initiator. [2]
[0029] The negative photosensitive resin composition according to [1], wherein the side chain of the polyimide (A) does not have a polymerizable functional group. [3]
[0031] The negative photosensitive resin composition according to [1] or [2], wherein the (A) polyimide and the (B) polymerizable compound have a structure derived from the same diamine. [4]
[0033] The negative photosensitive resin composition according to any one of [1] to [3], wherein the content of the polymerizable compound (B) is 0.1 to 50 parts by mass based on 100 parts by mass of the polyimide (A). [5]
[0035] The negative photosensitive resin composition according to any one of [1] to [4], wherein the weight average molecular weight Mw of the polyimide (A) is 3,000 or more and 30,000 or less. [6]
[0037] The negative photosensitive resin composition according to any one of [1] to [5], further comprising (D) a monomer having a polymerizable functional group which does not have a urea bond. [7]
[0039] The negative photosensitive resin composition according to any one of [1] to [6], further comprising (E) a silane coupling agent. [8]
[0041] The negative photosensitive resin composition according to any one of [1] to [7], further comprising (F) an organic titanium compound. [9]
[0043] The negative photosensitive resin composition according to any one of [1] to [8], further comprising (G) a thermal crosslinking agent.
[10]
[0045] The negative photosensitive resin composition according to any one of [1] to [9], further comprising (H) a rust inhibitor.
[11]
[0047] A method for manufacturing a solidified relief pattern, comprising the following steps:
[0048] (1) a step of applying the negative photosensitive resin composition described in any one of [1] to
[10] on a substrate to form a photosensitive resin layer on the substrate;
[0049] (2) exposing the photosensitive resin layer to light;
[0050] (3) a step of developing the exposed photosensitive resin layer to form a relief pattern; and
[0051] (4) A step of heating the relief pattern to form a cured relief pattern.
[12]
[0053] The negative photosensitive resin composition according to any one of [1] to
[10] , wherein the oxygen permeability (cc / m 2 ·24h·atm) is less than 1000.
[0054] Effects of the Invention
[0055] According to the present invention, a negative photosensitive resin composition having low cure shrinkage, excellent heat resistance, mechanical strength (elongation of the cured film), adhesion to copper and oxygen barrier properties after low-temperature curing, and a method for producing a cured relief pattern can be provided. DETAILED DESCRIPTION
[0056] Hereinafter, the embodiments of the present application will be described in detail. Throughout the present specification, when there are multiple structures represented by the same symbol in the general formula in a molecule, unless otherwise specified, they are independently selected and may be the same or different from each other.
[0057] Furthermore, structures represented by the same symbols in different general formulae are also independently selected unless otherwise specified, and may be the same as or different from each other.
[0058] In the following description, an upper limit value or a lower limit value in a numerical range described in a step format may be replaced with an upper limit value or a lower limit value in another numerical range described in a step format.
[0059] In the following description, the upper limit value or the lower limit value in a certain numerical range may be replaced by the value described in the Examples.
[0060] Furthermore, regarding the term "process" in the following description, an independent process is of course included in the term, and when it cannot be clearly distinguished from other processes, it is also included in the term as long as the function of the "process" can be achieved.
[0061] <Negative photosensitive resin composition>
[0062] The negative photosensitive resin composition of the present application (hereinafter referred to as “photosensitive resin composition”) contains (A) a polyimide having a polymerizable functional group at a terminal, (B) a polymerizable compound having a urea bond, and (C) a photopolymerization initiator.
[0063] The negative photosensitive resin composition of the present application may contain, in addition to the above-mentioned components, additives selected from (D) a monomer having a polymerizable functional group without a urea bond, (E) a silane coupling agent, (F) an organic titanium compound, (G) a thermal crosslinking agent, (H) a rust inhibitor, and other components as desired.
[0064] (A) Polyimide having a polymerizable functional group at the end
[0065] The polyimide (A) having a polymerizable functional group at a terminal of the present application preferably includes a structure represented by the following formula (1).
[0066]
[0067] {In formula (1), X1 is a tetravalent organic group, Y1 is a divalent organic group, and n is an integer of 2 to 150.}
[0068] From the viewpoint of low cure shrinkage and heat resistance, the polyimide of the present application preferably does not substantially contain a polyamic acid or polyamic acid ester structure.
[0069] In the present application, “substantially containing no” polyamic acid or polyamic acid ester structure means, for example, that the imidization rate of polyimide is 90% or more, preferably 95% or more.
[0070] The imidization rate of polyimide can be measured by a known method, for example, it can be calculated by the following method. First, the infrared absorption spectrum of polyimide is measured to confirm the presence of an absorption peak of the imide structure (1780 cm -1 Nearby, 1377cm -1 Then, the polyimide was heat treated at 350°C for 1 hour, and the infrared absorption spectrum of the heat-treated polyimide was measured. -1The imidization ratio of the polyimide can be calculated by comparing the peak intensity near the region with the intensity of the polyimide before the heat treatment.
[0071] The structure of X1 in the formula (1) is not particularly limited as long as it is a known structure derived from tetracarboxylic dianhydride, and examples thereof include a structure derived from tetracarboxylic dianhydride represented by the following formula (2).
[0072]
[0073] From the viewpoint of heat resistance of the cured film obtained from the negative photosensitive resin composition of the present application and solvent solubility of the polyimide, it is preferred that the structure derived from tetracarboxylic dianhydride of X1 has an alicyclic structure. In addition, from the viewpoint of elongation of the cured film, it is preferred that the structure derived from tetracarboxylic dianhydride of X1 has an aromatic structure.
[0074] The structure of Y1 in the formula (1) is not particularly limited as long as it is a known structure derived from a diamine, and examples thereof include structures derived from a diamine represented by the following formulas (3) and (4).
[0075]
[0076]
[0077] In addition, from the viewpoint of the elongation of the cured film obtained from the negative photosensitive resin composition of the present application and the solvent solubility of the polyimide, among the diamine-derived structures of formulas (3) to (4), the diamine-derived structures represented by the following formulas (5) to (11) are preferred, and from the viewpoint of the heat resistance of the cured film, the diamine-derived structures represented by the following formulas (12) to (15) are preferred.
[0078]
[0079]
[0080] The polymerizable functional group of the present application is a radical polymerizable functional group in one embodiment, and is typically a carbon-carbon double bond site. The polymerizable functional group is not particularly limited, but a functional group having an ethylenically unsaturated bond is preferred.
[0081] The (A) polyimide having a polymerizable functional group at the terminal preferably has a polymerizable functional group at the terminal of the main chain or the side chain, and more preferably has a polymerizable functional group at the terminal of the main chain. The negative photosensitive resin composition of the present application has excellent adhesion to copper and can improve oxygen barrier properties by including the (A) polyimide having a polymerizable functional group at the terminal.
[0082] The polyimide (A) having a polymerizable functional group at a terminal may have a polymerizable functional group at a terminal of a side chain, but preferably has no polymerizable functional group at a terminal of a side chain from the viewpoint of elongation and storage stability of a cured film.
[0083] Specific examples of the polymerizable functional group include polymerizable functional groups represented by the following formulae (16) to (18).
[0084]
[0085] (R1 and R2 are each independently selected from a hydrogen atom and a monovalent organic group having 1 to 3 carbon atoms, R3 is an organic group having 1 to 20 carbon atoms which may contain a heteroatom, k is an integer of 1 to 2. R4 is a hydrogen atom and an organic group having 1 to 4 carbon atoms, and * represents a bonding site to the terminal of the polyimide (A).)
[0086] In the present application, an organic group refers to a group having 1 or more carbon atoms.
[0087]
[0088] (In the formula, R5 and R6 are each independently a hydrogen atom and a monovalent organic group having 1 to 3 carbon atoms. In addition, * represents a bonding site to the terminal of the polyimide (A).)
[0089]
[0090] (In the formula, R7, R8 and R9 are each independently a hydrogen atom or a monovalent organic group having 1 to 3 carbon atoms, and j is an integer of 2 to 10. In addition, * represents a bonding site to the terminal of the polyimide (A).)
[0091] More specific examples of the structure represented by formula (16) include structures represented by the following formulae (19) to (22).
[0092]
[0093] (* in formulas (19) to (22) represents a bonding site to the terminal of the polyimide (A).)
[0094] More specific examples of the structure represented by formula (17) include structures represented by the following formulas (23) and (24).
[0095]
[0096] (* in formulas (23) to (24) represents a bonding site to the terminal of the polyimide (A).)
[0097] More specific examples of the structure represented by formula (18) include structures represented by the following formulae (25) to (28).
[0098]
[0099] (* in formulas (25) to (28) represents a bonding site to the terminal of the polyimide (A).)
[0100] From the viewpoint of oxygen barrier properties, the polymerizable functional group at the end of the polyimide preferably has a urea bond as a connecting group to the polymer. Specific examples include the structures represented by the above formulae (19) to (22).
[0101] The molecular weight distribution (Mw / Mn) of the (A) polyimide is preferably 1.0 or more and 1.9 or less. From the viewpoint of manufacturing efficiency, the lower limit of the molecular weight distribution of the (A) polyimide is more preferably 1.15 or more, and further preferably 1.25 or more. Regarding the upper limit of the molecular weight distribution of the (A) polyimide, from the viewpoint of resolution, the upper limit is more preferably 1.6 or less, and further preferably 1.5 or less.
[0102] The weight average molecular weight (Mw) of the polyimide (A) is not particularly limited as long as the polyimide (A) is soluble in the solvent (I) described later, but is preferably 3,000 or more and 30,000 or less from the viewpoint of copper adhesion and heat resistance of a cured film obtained from the negative photosensitive resin composition of the present application.
[0103] From the viewpoint of the elongation of the cured film, the lower limit of the weight average molecular weight of the polyimide (A) is more preferably 4,000 or more, and further preferably 5,000 or more. From the viewpoint of the solubility of the polyimide in a solvent, the upper limit of the weight average molecular weight of the polyimide (A) is more preferably 25,000 or less, and particularly preferably 20,000 or less.
[0104] (A) The weight average molecular weight of the polyimide can be measured by the method described in Examples described below, for example.
[0105] <Method for producing polyimide having a polymerizable functional group at the terminal>
[0106] (A) A polyimide having a polymerizable functional group at the end can be obtained, for example, as follows: a polyamic acid obtained by reacting tetracarboxylic dianhydride with a diamine is subjected to a dehydration ring-closure treatment by heat treatment to obtain a polyimide having a reactive group at the end of the main chain of the polyimide, and then a compound having a polymerizable functional group at the end is reacted with the polyimide having a reactive group at the end of the main chain to obtain the polyimide.
[0107] In the present application, the reactive group refers to a carboxyl group or an acid anhydride group derived from tetracarboxylic dianhydride at the main chain terminal of the polyimide, or an amino group derived from diamine at the main chain terminal of the polyimide.
[0108] In addition, the modification rate of the terminal of a polyimide (A) is measured by the method described in an Example.
[0109] The temperature for dehydration ring-closing of the polyamic acid by heat treatment is not particularly limited. If it is too low, the ring-closing reaction cannot be completed, so the lower limit is preferably 150° C. or higher, more preferably 160° C. or higher. On the other hand, if it is too high, the side reaction will proceed, so the upper limit is preferably 200° C. or lower, more preferably 180° C.
[0110] The tetracarboxylic dianhydride is not particularly limited, and specific examples thereof include bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride (BCD), 4,4'-oxydiphthalic anhydride (ODPA), 3,3',4,4'-biphenyltetracarboxylic dianhydride, 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride (BPADA), 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, and 4,4'-(hexafluoroisopropylidene)diphthalic anhydride.
[0111] The diamine is not particularly limited, and specific examples thereof include 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 1,3-bis(3-aminophenoxy)benzene (APB), 1,4-bis(4-aminophenoxy)benzene (TPE-Q), 6-(4-aminophenoxy)[1,1'-biphenyl]-3-amine (PDPE), 4,4'-bis(4-aminophenoxy)biphenyl, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(4-aminophenoxy)phenyl]sulfone (BAPS), 9,9-bis(4-aminophenyl)fluorene (BAFL), 2,2'-dimethylbenzidine, 2,2'-bis(trifluoromethyl)benzidine (TFMB), and 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane (HFBAPP).
[0112] The compound having a polymerizable functional group at a terminal is preferably at least one compound selected from the group consisting of isocyanate compounds, chloride compounds, and alcohol compounds.
[0113] Specific examples of the isocyanate compound include 2-methacryloyloxyethyl isocyanate, 2-acryloyloxyethyl isocyanate, 1,1-(bisacryloyloxymethyl)ethyl isocyanate, and 2-(2-methacryloyloxyethoxy)ethyl isocyanate.
[0114] Specific examples of chloride-based compounds include acryloyl chloride and methylpropionyl chloride;
[0115] Specific examples of the alcohol compound include 2-hydroxyethyl methacrylate (2-hydroxyethyl methacrylate: HEMA), 2-hydroxyethyl acrylate, 4-hydroxyethyl methacrylate, and 4-hydroxyethyl acrylate.
[0116] The isocyanate compound reacts with the amino group of the dehydrated ring-closed polyimide to form a urea bond.
[0117] The chloride-based compound reacts with the amino group of the dehydrated ring-closed polyimide to form an amide bond.
[0118] The alcohol compound reacts with the carboxyl group of the dehydration-ring-closed polyimide to form an ester bond.
[0119] The method for reacting the isocyanate compound is not particularly limited, and the isocyanate compound can be reacted with the amino group of the dehydrated ring-closed polyimide by stirring at room temperature.
[0120] The method for reacting the chloride-based compound is not particularly limited, and the chloride-based compound may be added dropwise to the dehydrated polyimide solution by cooling it with ice, and react with the amino group of the dehydrated polyimide.
[0121] The method for reacting the alcohol compound is not particularly limited, and the alcohol compound can be reacted with the carboxyl group of the dehydrated ring-closed polyimide using a condensation agent such as N,N′-dicyclohexylcarbodiimide (DCC) or an esterification catalyst such as p-toluenesulfonic acid.
[0122] In the production of the polyimide (A), a reaction solvent may be used in order to efficiently proceed the reaction in a homogeneous system.
[0123] The reaction solvent is not particularly limited as long as it can uniformly dissolve or suspend the tetracarboxylic dianhydride, the diamine, and the compound having a polymerizable functional group at the terminal, and examples thereof include γ-butyrolactone (GBL), dimethyl sulfoxide, N,N-dimethylacetoacetamide, 1,3-dimethyl-2-imidazolidinone, 3-methoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropionamide, N,N-dimethylformamide, N-methyl-2-pyrrolidone (NMP), N-ethyl-2-pyrrolidone, N,N-dimethylacetamide, and the like.
[0124] The (A) polyimide can be purified by a known method described in Japanese Patent Application Laid-Open No. 2012-194520. Examples thereof include a method of removing unreacted products by dropping a solution obtained by dissolving the (A) polyimide in a solvent (I) into water for reprecipitation; a method of removing a condensing agent insoluble in the reaction solvent by filtration; and a method of removing a catalyst by using an ion exchange resin. After these purifications, the (A) polyimide can be dried by a known method and isolated in a powder state.
[0125] The negative photosensitive resin composition of the present application preferably contains 20 to 70% by mass, more preferably 25 to 65% by mass of the (A) polyimide, based on the total solid content mass.
[0126] (B) Polymerizable compound having urea bond
[0127] The negative photosensitive resin composition of the present application contains (B) a polymerizable compound having a urea bond, and thus the negative photosensitive resin composition of the present application is excellent in adhesion to copper and oxygen barrier properties.
[0128] The reason why the above-mentioned effect is exerted by using the (B) polymerizable compound having a urea bond is not clear, but the present inventors consider it as follows.
[0129] The urea site in the polymerizable compound having a urea bond (B) shows a strong interaction with the copper surface. Furthermore, by reacting the polymerizable site in the polymerizable compound having a urea bond (B) with the polyimide terminal, the polymerizable compound having a urea bond (B) acts as a binder between the photosensitive resin composition and the copper surface, thereby improving the adhesion to copper.
[0130] In addition, since the urea sites strongly interact not only with copper but also with each other, the (A) polyimide and the (B) polymerizable compound having a urea bond in the photosensitive resin composition are densely packed, thereby improving the oxygen barrier property.
[0131] The polymerizable compound (B) having a urea bond can be used without particular limitation as long as it has a polymerizable functional group that can be polymerized by light or heat, and a radical polymerizable compound is preferred. The polymerizable compound (B) having a urea bond may have one polymerizable functional group or two or more polymerizable functional groups.
[0132] (B) Examples of the polymerizable compound having a urea bond include compounds represented by the following formula (29).
[0133]
[0134] {In formula (29), E represents a structure derived from diamine. Z3 and Z4 may be the same or different and represent a monovalent organic group including a urea bond as a linking group and a polymerizable functional group. r and s are integers of 0 to 2 and satisfy r+s≥1.}
[0135] (B) The polymerizable compound having a urea bond can be synthesized from, for example, a diamine and an isocyanate compound. In formula (29), E represents a structure derived from a diamine, and Z3 and Z4 represent structures derived from an isocyanate compound.
[0136] The structure of E in the formula (29) is not particularly limited as long as it is a known structure derived from a diamine, but for example, structures derived from a diamine of the following formulas (30) and (31) are preferred.
[0137]
[0138]
[0139] In addition, among the diamine-derived structures of formulae (30) to (31), from the viewpoint of the elongation of the cured film obtained from the negative photosensitive resin composition of the present application, the diamine-derived structures of the following formulae (32) to (38) are preferred. Furthermore, from the viewpoint of the heat resistance of the cured film, the diamine-derived structures of the following formulae (39) to (42) are preferred.
[0140]
[0141]
[0142] In terms of compatibility with the (A) polyimide, the (A) polyimide and the (B) polymerizable compound having a urea bond preferably have a skeleton (structure) derived from the same diamine, and more preferably have a structure derived from a diamine of formulas (30) to (31).
[0143] When the compatibility of the polymerizable compound (B) having a urea bond and the polyimide (A) is excellent, the polymerizable functional group at the terminal of the polyimide (A) and the polymerizable functional group of the polymerizable compound (B) having a urea bond are easily reacted, and the mechanical strength (elongation) of the cured film formed by curing the photosensitive resin composition containing the polyimide (A) and the polymerizable compound (B) is easily improved, which is preferred.
[0144] The structures of Z3 and Z4 in formula (29) are not particularly limited as long as they are known structures derived from isocyanate compounds, and examples thereof include structures derived from isocyanate compounds of the following formulae (43) to (46).
[0145]
[0146]
[0147] (* in formulae (43) to (46) represents a bonding site with the diamine (A).)
[0148] <(B) Method for producing a polymerizable compound having a urea bond>
[0149] (B) The polymerizable compound having a urea bond can be produced, for example, by reacting an amino group derived from a diamine compound with an isocyanate group derived from an isocyanate compound.
[0150] In addition, the modification rate of the polymerizable compound (B) having a urea bond is measured by the method described in Examples.
[0151] The temperature at which the diamine compound and the isocyanate compound are reacted is not particularly limited, and the diamine compound and the isocyanate compound may be reacted by stirring at room temperature for about 10 hours, for example.
[0152] The diamine compound is not particularly limited, and specific examples thereof include 4,4'-diaminodiphenyl ether (DADPE), 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), 1,3-bis(3-aminophenoxy)benzene (APB), 1,4-bis(4-aminophenoxy)benzene (TPE-Q), 6-(4-aminophenoxy)biphenyl-3-amine (PDPE), 4,4'-bis(4-aminophenoxy)biphenyl, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(4-aminophenoxy)phenyl]sulfone (BAPS), 9,9-bis(4-aminophenyl)fluorene (BAFL), 2,2'-dimethylbenzidine, 2,2'-bis(trifluoromethyl)benzidine (TFMB), and 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane (HFBAPP).
[0153] From the viewpoint of elongation of a cured film obtained from the negative photosensitive resin composition of the present application, 4,4'-diaminodiphenyl ether (DADPE), 1,4-bis(4-aminophenoxy)benzene (TPE-Q) and 6-(4-aminophenoxy)biphenyl-3-amine (PDPE) are preferred, and from the viewpoint of heat resistance, 9,9-bis(4-aminophenyl)fluorene (BAFL) is preferred.
[0154] The isocyanate compound is not particularly limited, and examples thereof include 2-methacryloyloxyethyl isocyanate, 2-acryloyloxyethyl isocyanate, 1,1-(bisacryloyloxymethyl)ethyl isocyanate, and 2-(2-methacryloyloxyethyloxy)ethyl isocyanate.
[0155] In the production of the polymerizable compound having a urea bond (B), a reaction solvent may be used in order to efficiently carry out the reaction in a homogeneous system.
[0156] The reaction solvent is not particularly limited as long as it can uniformly dissolve or suspend the diamine, the isocyanate compound, and the polymerizable compound having a urea bond.
[0157] Examples of the reaction solvent include γ-butyrolactone (GBL), dimethyl sulfoxide, N,N-dimethylacetoacetamide, 1,3-dimethyl-2-imidazolidinone, 3-methoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropionamide, N,N-dimethylformamide, N-methyl-2-pyrrolidone (NMP), N-ethyl-2-pyrrolidone, and N,N-dimethylacetamide.
[0158] From the viewpoint of copper adhesion and oxygen barrier properties, the (B) polymerizable compound having a urea bond is preferably contained in an amount of 0.1 to 60 parts by mass or 0.1 to 50 parts by mass, more preferably 1 to 60 parts by mass, further preferably 2 to 50 parts by mass, and particularly preferably 3 to 40 parts by mass, relative to 100 parts by mass of the (A) polyimide.
[0159] From the viewpoint of copper adhesion, the lower limit of the content of the polymerizable compound having a urea bond (B) is preferably 0.1 parts by mass or more, more preferably 1 part by mass or more, further preferably 2 parts by mass or more, particularly preferably 3 parts by mass or more, based on 100 parts by mass of the polyimide (A).
[0160] From the viewpoint of suppressing cure shrinkage (low cure shrinkage) and the elongation of the cured film, the upper limit of the content of the polymerizable compound having a urea bond (B) is more preferably 50 parts by mass or less, and further preferably 40 parts by mass or less, based on 100 parts by mass of the polyimide (A).
[0161] From the viewpoint of oxygen barrier properties, the negative photosensitive resin composition of the present embodiment has an oxygen permeability (cc / m 2 ·24h·atm) is preferably less than 1000, more preferably 500 or more and less than 1000, further preferably 200 or more and less than 500, particularly preferably less than 200.
[0162] (Oxygen barrier properties)
[0163] The oxygen barrier property of a cured film obtained by curing the negative photosensitive resin composition of the present embodiment was measured by the following method.
[0164] The negative photosensitive resin composition of the present embodiment is pre-baked to form a thin film of about 7 μm thick before curing. The thin film is post-baked in a nitrogen atmosphere at 170° C. for 120 minutes to cure, and a cured thin film (a cured film in one embodiment) of about 6 μm thick (5.0 to 7.0 μm thick in one embodiment) is prepared.
[0165] The oxygen permeability (cc / m2) was measured using a gas permeability measuring device (manufactured by GTR TEC Co., Ltd., product name: GTR-10XF (isobaric GC)) based on the isobaric GC method of JIS K 7126-2. 2 ·24h·atm).
[0166] <(C) Photopolymerization initiator>
[0167] (C) The photopolymerization initiator is a compound that generates radicals by active light and polymerizes a compound containing an ethylenically unsaturated group or the like.
[0168] Examples of the initiator that generates radicals by active light include compounds including structures such as benzophenone, N-alkylaminoacetophenone, oxime ester, acridine, phosphine oxide, and 2,4,5-triphenylimidazole (lophine).
[0169] Specific examples include aromatic ketones such as benzophenone, N,N,N',N'-tetramethyl-4,4'-diaminobenzophenone (Michler's ketone), N,N,N',N'-tetraethyl-4,4'-diaminobenzophenone, 4-methoxy-4'-dimethylaminobenzophenone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propanone-1, acrylated benzophenone, and 4-benzoyl-4'-methyldiphenyl sulfide;
[0170] Benzoin ether compounds such as benzoin methyl ether, benzoin ethyl ether and benzoin phenyl ether;
[0171] Benzoin compounds such as benzoin, methylbenzoin and ethylbenzoin;
[0172] 1,2-octanedione, 1-[4-(phenylthio)-2-(O-benzoyl oxime)], ethyl ketone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-1-(O-acetyl oxime) (manufactured by BASF JAPAN, Irgacure Oxe02), 1-[4-(phenylthio)phenyl]-3-cyclopentylpropane-1,2-dione-2-(o-benzoyl oxime) (manufactured by Changzhou Qiangli New Electronic Materials Co., Ltd., PBG305), 1-(6-O-methylbenzoyl-9-ethylcarbazole-3-yl)-(3-cyclopentylacetone)-1-oxime acetate (manufactured by Changzhou Qiangli New Electronic Materials Co., Ltd., TR-PBG-304), trade name : TR-PBG-3057 (manufactured by Changzhou Qiangli New Electronic Materials Co., Ltd.), 1,2-propanedione, 3-cyclohexyl-1-[9-ethyl-6-(2-furylcarbonyl)-9H-carbazole-3-yl]-, 2-(O-acetoxime) (manufactured by Nihon Kemtech Co., Ltd., product name: TR-PBG-326), trade name: NCI-831 (manufactured by ADEKA Co., Ltd.) and other oxime ester compounds;
[0173] Benzil derivatives such as benzil dimethyl ketal;
[0174] Acridine derivatives such as 9-phenylacridine and 1,7-bis(9,9'-acridinyl)heptane;
[0175] N-phenylglycine and other N-phenylglycine derivatives;
[0176] Coumarin compounds;
[0177] Oxazole compounds;
[0178] Phosphine oxide compounds such as 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide,
[0179] 2,4,5-triphenylimidazole compounds such as 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, etc., but are not limited to these.
[0180] (C) The photopolymerization initiator may be used alone or in combination of two or more. Among the above-mentioned photopolymerization initiators, oxime ester compounds are more preferred from the viewpoint of resolution.
[0181] The content of the photopolymerization initiator (C) is preferably 1 part by mass or more and 30 parts by mass or less relative to 100 parts by mass of the polyimide (A). From the viewpoint of photocurability, the lower limit of the content of the photopolymerization initiator (C) is more preferably 2 parts by mass or more relative to 100 parts by mass of the polyimide (A).
[0182] The upper limit of the content of the (C) photopolymerization initiator is more preferably 20 parts by mass or less relative to 100 parts by mass of the (A) polyimide from the viewpoint of bottom curing of the relief pattern.
[0183] (D) Monomer having a polymerizable functional group but not having a urea bond
[0184] In order to improve the resolution of the cured relief pattern and suppress the cure shrinkage during thermal curing, the photosensitive resin composition of the present application may optionally contain (D) a monomer having a polymerizable functional group without a urea bond.
[0185] As the (D) monomer having a polymerizable functional group without a urea bond (a free radical polymerizable compound in one embodiment), a (meth)acrylic compound that can undergo a free radical polymerization reaction by the (C) photopolymerization initiator is preferred. The (D) monomer having a polymerizable functional group without a urea bond more preferably includes a monofunctional monomer (D1) having one polymerizable functional group in the molecule and / or a polyfunctional monomer (D2) having two or more polymerizable functional groups in the molecule.
[0186] In particular, although not limited to the following, examples of the monofunctional monomer (D1) include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl methacrylate, 2-hydroxybutyl methacrylate, 4-hydroxybutyl acrylate, 2-hydroxy-3-phenoxypropyl acrylate, 2-ethylhexyl (meth)acrylate, butoxydiethylene glycol methacrylate, isobornyl (meth)acrylate, m-phenoxybenzyl acrylate, o-phenylphenoxyethyl acrylate, 4-methacryloyloxybenzophenone, EO (ethylene oxide)-modified p-cumylphenol acrylate, nonylphenoxyethyl acrylate, 6-acrylamidocaproic acid, and tris-(2-acryloyloxyethyl)isocyanurate.
[0187] Examples of the polyfunctional monomer (D2) include di(meth)acrylates of ethylene glycol or polyethylene glycol represented by diethylene glycol dimethacrylate and tetraethylene glycol dimethacrylate, di(meth)acrylates of propylene glycol or polypropylene glycol, di(meth)acrylates or tri(meth)acrylates of glycerol, cyclohexane di(meth)acrylate, di(meth)acrylate of 1,4-butanediol, di(meth)acrylate of 1,6-hexanediol, di(meth)acrylate of neopentyl glycol, di(meth)acrylate of bisphenol A,
[0188] (Meth)acrylamide and its derivatives,
[0189] trimethylolpropane tri(meth)acrylate, di(meth)acrylate or tri(meth)acrylate of glycerol, di(meth)acrylate, tri(meth)acrylate or tetra(meth)acrylate of pentaerythritol, ethylene oxide (e.g. 4-hydroxybutyl acrylate glycidyl ether) or propylene oxide adducts of these compounds,
[0190] Product name: KRM7735 (manufactured by DAICEL-ALLNEX LTD.), product name: EBECRYL230 (manufactured by DAICEL-ALLNEX LTD.), product name: EBECRYL4491 (manufactured by DAICEL-ALLNEX LTD.), product name: EBECRYL8413 (manufactured by DAICEL-ALLNEX LTD.), product name: EBECRYL8411 (manufactured by DAICEL-ALLNEX LTD.), product name: EBECRYL8402 (manufactured by DAICEL-ALLNEX LTD.), product name: EBECRYL8465 (manufactured by DAICEL-ALLNEX LTD.), product name: EBECRYL8667 (manufactured by DAICEL-ALLNEX LTD.), product name: EBECRYL4740 (manufactured by DAICEL-ALLNEX LTD.), product name: KRM9276 (manufactured by DAICEL-ALLNEX LTD.) and other urethane acrylate compounds such as tris-(2-hydroxyethyl)isocyanurate acrylate.
[0191] Among these radically polymerizable compounds, from the viewpoint of suppressing cure shrinkage, it is preferred to contain a compound having three or more radically polymerizable functional groups.
[0192] Among these monomers, the weight ratio of the monofunctional monomer (D1) to the polyfunctional monomer (D2) is preferably greater than 0.01 from the viewpoint of flatness during coating, and is preferably less than 1.5 from the viewpoint of flatness after curing.
[0193] It is preferable that content of the (D) monomer which does not have a urea bond and has a polymerizable functional group in the photosensitive resin composition is 0.5 mass part - 100 mass parts with respect to 100 mass parts of (A) polyimide.
[0194] The lower limit of the content of the (D) monomer having a polymerizable functional group without a urea bond is preferably 5 parts by mass or more, further preferably 10 parts by mass or more, and particularly preferably 20 parts by mass or more, based on 100 parts by mass of the (A) polyimide, from the viewpoint of photocurability.
[0195] The upper limit of the content of the (D) monomer having a polymerizable functional group without a urea bond is more preferably 60 parts by mass or less, and further preferably 50 parts by mass or less, based on 100 parts by mass of the (A) polyimide, from the viewpoint of copper adhesion and bottom curing of the pattern.
[0196] (E) Silane coupling agent
[0197] In order to improve the copper adhesion of the cured relief pattern, the negative photosensitive resin composition of the present application may optionally contain (E) a silane coupling agent.
[0198] The silane coupling agent (E) preferably has a structure represented by the following general formula (47) or formula (48).
[0199]
[0200] In formulas (47) and (48), R 10 is at least one selected from the group consisting of substituents containing an epoxy group, a phenylamino group, an ureide group, an isocyanate group, and an isocyanuric acid group, and R 11 is an alkyl group having 1 to 4 carbon atoms, R 12 is a hydroxyl group or an alkyl group having 1 to 4 carbon atoms, a is an integer of 1 to 3, and i is an integer of 1 to 6.
[0201] In the general formulae (47) and (48), a is not limited as long as it is an integer of 1 to 3, and is preferably 2 or 3, and more preferably 3, from the viewpoint of adhesion to the metal redistribution layer. i is not limited as long as it is an integer of 1 to 6, and is preferably 1 to 4 from the viewpoint of adhesion to the metal redistribution layer. From the viewpoint of resolution, it is preferably 2 to 5.
[0202] R 10 There is no limitation as long as the substituent includes any structure selected from the group consisting of epoxy group, phenylamino group, ureide group, isocyanate group and isocyanurate group. Among these, from the viewpoint of resolution and adhesion of the metal redistribution layer, at least one selected from the group consisting of substituent including phenylamino group and substituent including ureide group is preferred, and substituent including phenylamino group is more preferred.
[0203] R 11 There is no limitation as long as it is an alkyl group having 1 to 4 carbon atoms, and examples thereof include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, and tert-butyl.
[0204] R 12 There is no limitation as long as it is a hydroxyl group or an alkyl group having 1 to 4 carbon atoms. Examples of the alkyl group having 1 to 4 carbon atoms include 11 Same alkyl group.
[0205] Examples of the epoxy group-containing silane coupling agent include 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 3-glycidoxypropyltriethoxysilane.
[0206] As a phenylamino group-containing silane coupling agent, N-phenyl-3-aminopropyltrimethoxysilane can be exemplified.
[0207] As the ureide group-containing silane coupling agent, 3-ureide propyl trialkoxy silane can be exemplified.
[0208] As an isocyanate group-containing silane coupling agent, 3-isocyanatepropyltriethoxysilane can be exemplified.
[0209] The content of the (E) silane coupling agent in the negative photosensitive resin composition is 0.2 to 10 parts by mass based on 100 parts by mass of the (A) polyimide.
[0210] The lower limit of the content of the silane coupling agent (E) is more preferably 0.5 parts by mass or more, and further preferably 1 part by mass or more, based on 100 parts by mass of the polyimide (A), from the viewpoint of copper adhesion.
[0211] The upper limit of the content of the silane coupling agent (E) is more preferably 8 parts by mass or less, and further preferably 6 parts by mass or less, based on 100 parts by mass of the polyimide (A), from the viewpoint of generation of foreign matter due to precipitation.
[0212] (F) Organic titanium compound
[0213] The negative photosensitive resin composition of the present application may optionally contain (F) an organic titanium compound in order to improve the chemical resistance of the cured film.
[0214] Examples of the (F) organic titanium compound include compounds in which an organic group is bonded to a titanium atom via a covalent bond or an ionic bond. Specific examples of the organic titanium compound are shown in the following I) to VII):
[0215] I) Titanium chelate compounds: Specific examples include titanium (IV) acetylacetonate, bis(triethanolamine)titanium diisopropoxide, di-n-butoxybis(2,4-pentanedione)titanium, diisopropoxybis(2,4-pentanedione)titanium, diisopropoxybis(tetramethylheptanedione)titanium, diisopropoxybis(ethyl acetoacetate)titanium, and the like.
[0216] II) Tetraalkoxytitanium compounds: for example, titanium tetra-n-butoxide, titanium tetraethoxide, titanium tetra(2-ethylhexyl)oxide, titanium tetraisobutoxide, titanium tetraisopropoxide, titanium tetramethoxide, titanium tetramethoxypropoxide, titanium tetramethylphenoxide, titanium tetra-n-nonoxide, titanium tetra-n-propoxide, titanium tetrastearylate, titanium tetra[bis{2,2-(allyloxymethyl)butoxide}], and the like.
[0217] III) Titanocene compounds: for example, pentamethylcyclopentadienyl titanium trimethoxide, bis(η 5 -2,4-cyclopentadien-1-yl)bis(2,6-difluorophenyl)titanium, bis(η 5 -2,4-cyclopentadien-1-yl)bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium, etc.
[0218] IV) Monoalkoxy titanium compounds: for example, tri(dioctylphosphate)titanium isopropoxide, tri(dodecylbenzenesulfonyl)titanium isopropoxide and the like.
[0219] V) Titanium oxide compounds: for example, bis(pentanedione)titanium oxide, bis(tetramethylheptanedione)titanium oxide, titanium phthalocyanine, and the like.
[0220] VI) Titanium tetraacetylacetonate compounds: for example, titanium tetraacetylacetonate and the like.
[0221] VII) Titanate coupling agent: for example, isopropyl tri(dodecylbenzenesulfonyl) titanate, etc.
[0222] The (F) organic titanium compound is preferably at least one compound selected from the group consisting of I) titanium chelate compounds, II) tetraalkoxytitanium compounds, and III) titanocene compounds, from the viewpoint of exhibiting better chemical resistance.
[0223] Particularly preferred are diisopropoxybis(ethyl acetoacetate)titanium, tetra-n-butoxide titanium, bis(η 5 -2,4-cyclopentadien-1-yl)bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium and acetylacetonatooxytitanium(IV), etc.
[0224] When the negative photosensitive resin composition of the present application contains the (F) organic titanium compound, the content of the (F) organic titanium compound is preferably 0.05 parts by mass or more and 10 parts by mass or less relative to 100 parts by mass of the (A) polyimide.
[0225] The lower limit of the content of the (F) organic titanium compound is more preferably 0.5 parts by mass or more relative to 100 parts by mass of the (A) polyimide, from the viewpoint of heat resistance and chemical resistance of the obtained cured film.
[0226] The upper limit of the content of the (F) organic titanium compound is more preferably 2 parts by mass or less relative to 100 parts by mass of the (A) polyimide, from the viewpoint of the storage stability of the negative photosensitive resin composition.
[0227] (G) Thermal crosslinking agent
[0228] The negative photosensitive resin composition of the present application may optionally contain (G) a thermal crosslinking agent from the viewpoint of suppressing cure shrinkage of the cured film.
[0229] In the present application, (G) thermal crosslinking agent refers to a compound that undergoes addition reaction or polycondensation reaction by heat. These reactions occur between (A) polyimide and (G) thermal crosslinking agent, between (G) thermal crosslinking agents, and in a combination of (G) thermal crosslinking agent and other components described below, and the reaction temperature is preferably 150° C. or higher.
[0230] Examples of the (G) thermal crosslinking agent include alkoxymethyl compounds, epoxy compounds, oxetane compounds, bismaleimide compounds, allyl compounds, and blocked isocyanate compounds. From the viewpoint of suppressing cure shrinkage, the (G) thermal crosslinking agent preferably contains a nitrogen atom.
[0231] Examples of the alkoxymethyl compound include compounds represented by the following general formulae (49) to (50), but are not limited thereto.
[0232]
[0233]
[0234] Examples of the epoxy compound include 4-hydroxybutyl acrylate glycidyl ether, epoxy compounds containing a bisphenol A type group, and hydrogenated bisphenol A diglycidyl ether (for example, manufactured by Kyoeisha Chemical Co., Ltd., trade name: Epolight 4000).
[0235] Examples of the oxetane compound include 1,4-bis{[(3-ethyl-3-oxetanyl)methoxy]methyl}benzene, bis[1-ethyl(3-oxetanyl)]methyl ether, 4,4′-bis[(3-ethyl-3-oxetanyl)methyl]biphenyl, 4,4′-bis(3-ethyl-3-oxetanylmethoxy)biphenyl, ethylene glycol bis(3-ethyl-3-oxetanylmethyl)ether, diethylene glycol bis(3-ethyl-3-oxetanylmethyl)ether, and bis(3-ethyl-3-oxetanylmethyl)diphenol. esters, trimethylolpropane tris(3-ethyl-3-oxetanylmethyl) ether, pentaerythritol tetra(3-ethyl-3-oxetanylmethyl) ether, poly[[3-[(3-ethyl-3-oxetanyl)methoxy]propyl]silsesquioxane] derivatives, silicate oxetanyl esters, phenol novolac type oxetane, 1,3-bis[(3-ethyloxetan-3-yl)methoxy]benzene, trade name: OXT121 (manufactured by Toagosei Co., Ltd.) and trade name: OXT221 (manufactured by Toagosei Co., Ltd.), etc.
[0236] Examples of the bismaleimide compound include 1,2-bis(maleimide)ethane, 1,3-bis(maleimide)propane, 1,4-bis(maleimide)butane, 1,5-bis(maleimide)pentane, 1,6-bis(maleimide)hexane, 2,2,4-trimethyl-1,6-bis(maleimide)hexane, N,N'-1,3-phenylenebis(maleimide), 4-methyl-N,N'-1,6-bis(maleimide)hexane, -1,3-phenylenebis(maleimide), N,N'-1,4-phenylenebis(maleimide), 3-methyl-N,N'-1,4-phenylenebis(maleimide), 4,4'-bis(maleimide)diphenylmethane, 3,3'-diethyl-5,5'-dimethyl-4,4'-bis(maleimide)diphenylmethane and 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane.
[0237] Examples of the allyl compound include allyl alcohol, allylanisole, allyl benzoate, allyl cinnamate, N-allyloxyphthalimide, allylphenol, allylphenyl sulfone, allyl urea, diallyl phthalate, diallyl isophthalate, diallyl terephthalate, diallyl maleate, diallyl isocyanurate, triallylamine, triallyl isocyanurate, triallyl cyanurate, triallylamine, triallyl 1,3,5-benzenetricarboxylate, triallyl trimellitate, triallyl phosphate, triallyl phosphite, and triallyl citrate.
[0238] Examples of the blocked isocyanate compound include hexamethylene diisocyanate-based blocked isocyanates; trade names: Duranate SBN-70D, SBB-70P, SBF-70E, TPA-B80E, 17B-60P, MF-B60B, E402-B80B, MF-K60B, and WM44-L70G (manufactured by Asahi Kasei Corporation), trade name: Takenate B-882N (manufactured by Mitsui Chemicals, Inc.), trade names: 7960, 7961, 7982, 7991, and 7992 (manufactured by Baxenden Corporation), etc.);
[0239] Toluene diisocyanate-based blocked isocyanate (Mitsui Chemicals, trade name: Takenate B-830, etc.),
[0240] 4,4'-diphenylmethane diisocyanate-based blocked isocyanate (Mitsui Chemicals, trade name: Takenate B-815N), (Daiei Sangyo, trade name: Blonate PMD-OA01 and PMD-MA01), etc.
[0241] 1,3-Bis(isocyanatemethyl)cyclohexane-based blocked isocyanate (Mitsui Chemicals, trade name: Takenate B-846N), (Tosoh Corporation, trade name: Coronate BI-301, 2507, and 2554), etc.
[0242] Isophorone diisocyanate is a blocked isocyanate (manufactured by Baxenden, trade names: 7950, 7951, 7990, etc.).
[0243] Among these compounds, blocked isocyanate compounds and bismaleimide compounds are preferred from the viewpoint of storage stability. (G) The thermal crosslinking agent may be used alone or in combination of two or more.
[0244] It is preferable that content of the (G) heat crosslinking agent in the negative photosensitive resin composition is 0.2 mass part - 40 mass parts with respect to 100 mass parts of (A) polyimide.
[0245] From the viewpoint of chemical resistance, the lower limit of the content of the (G) thermal crosslinking agent is more preferably 1 part by mass or more, and further preferably 2 parts by mass or more, based on 100 parts by mass of the (A) polyimide.
[0246] The upper limit of the content of the (G) thermal crosslinking agent is more preferably 30 parts by mass or less, and further preferably 20 parts by mass or less, based on 100 parts by mass of the (A) polyimide, from the viewpoint of storage stability of the negative photosensitive resin composition.
[0247] (H) Rust inhibitor
[0248] When the negative photosensitive resin composition of the present application is used to form a cured film on a substrate containing copper or a copper alloy, the negative photosensitive resin composition of the present application may optionally contain (H) a rust inhibitor in order to suppress copper discoloration. Examples of the (H) rust inhibitor include azole compounds and purine compounds.
[0249] Examples of the azole compound include 1H-triazole, 5-methyl-1H-triazole, 5-ethyl-1H-triazole, 4,5-dimethyl-1H-triazole, 5-phenyl-1H-triazole, 4-tert-butyl-5-phenyl-1H-triazole, 5-hydroxyphenyl-1H-triazole, phenyltriazole, p-ethoxyphenyltriazole, 5-phenyl-1-(2-dimethylaminoethyl)triazole, 5-benzyl-1H-triazole, hydroxyphenyltriazole, 1,5-dimethyltriazole, 4,5-diethyl-1H-triazole, 1H-benzotriazole, 2-(5-methyl-2-hydroxyphenyl)benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-benzotriazole. 1H-tetrazole, 5-methyl-1H-tetrazole, 5-phenyl-1H-tetrazole, 1H-tetrazole, 5-methyl-1H-tetrazole, 1H-tetrazole, 5-methyl-1H-tetrazole, 1H-tetrazole, 5-phenyl-1H-tetrazole, 5-methyl-1H-tetrazole, 1H-tetrazole, 5-methyl-1H-tetrazole, 5-phenyl-1H-tetrazole, 5-amino-1H-tetrazole, 1H-tetrazole, 1H-tetrazole, 2-(3,5-di-tert-butyl-2-hydroxyphenyl)benzotriazole, 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, hydroxyphenylbenzotriazole, tolyltriazole, 5-methyl-1H-benzotriazole, 4-methyl-1H-benzotriazole, 4-carboxyl-1H-benzotriazole, 5-carboxyl-1H-benzotriazole, 3-mercapto-1,2,4-triazole, 1H-tetrazole, 5-methyl-1H-tetrazole, 5-phenyl-1H-tetrazole, 5-amino-1H-tetrazole, 1-methyl-1H-tetrazole, and the like.
[0250] Particularly preferred are 5-amino-1H-tetrazole, tolyltriazole, 5-methyl-1H-benzotriazole, and 4-methyl-1H-benzotriazole. These azole compounds may be used alone or as a mixture of two or more.
[0251] Specific examples of purine compounds include purine, adenine, guanine, hypoxanthine, xanthine, theobromine, caffeine, uric acid, isoguanine, 2,6-diaminopurine, 9-methyladenine, 2-hydroxyadenine, 2-methyladenine, 1-methyladenine, N-methyladenine, N,N-dimethyladenine, 2-fluoroadenine, 9-(2-hydroxyethyl)adenine, guanine oxime, N-(2-hydroxyethyl)adenine, 8-aminoadenine, Purine, 6-amino-8-phenyl-9H-purine, 1-ethyladenine, 6-ethylaminopurine, 1-benzyladenine, N-methylguanine, 7-(2-hydroxyethyl)guanine, N-(3-chlorophenyl)guanine, N-(3-ethylphenyl)guanine, 2-azaadenine, 5-azaadenine, 8-azaadenine, 8-azaguanine, 8-azapurine, 8-azaxanthine, 8-azahypoxanthine and the like and derivatives thereof.
[0252] Particularly preferably, 8-azaadenine is used. These purine compounds may be used alone or as a mixture of two or more.
[0253] When the negative photosensitive resin composition of the present application contains (H) a rust inhibitor, the content of the (H) rust inhibitor is preferably 0.01 parts by mass or more and 20 parts by mass or less relative to 100 parts by mass of the (A) polyimide.
[0254] From the perspective of suppressing discoloration of the copper or copper alloy surface when forming a negative photosensitive resin composition on copper or copper alloy, the lower limit of the rust inhibitor (H) is more preferably 0.03 parts by mass or more, and further preferably 0.05 parts by mass or more. From the perspective of photosensitivity, the upper limit of the rust inhibitor (H) is more preferably 10 parts by mass or less, and further preferably 5 parts by mass or less.
[0255] The negative photosensitive resin composition of the present application may further contain other components in addition to the above-mentioned components (A) to (H). The other components in addition to the components (A) to (H) are not limited, and examples thereof include thermal polymerization initiators, plasticizers, hindered phenol compounds, adhesive aids, sensitizers, thermal polymerization inhibitors, thermal base generators, and solvents.
[0256] The negative photosensitive resin composition of the present application may contain a thermal polymerization initiator.
[0257] Thermal polymerization initiators are compounds that generate free radicals by heat, and examples thereof include organic peroxides such as dialkyl peroxides, diacyl peroxides, peroxyesters, and peroxyketals, and azo polymerization initiators such as azonitrile, azoesters, and azoamides. Among these, dialkyl peroxides and diacyl peroxides (e.g., dicumyl peroxide) are preferred from the viewpoint of chemical resistance.
[0258] When the negative photosensitive resin composition of the present application contains a thermal polymerization initiator, the content thereof is preferably 0.1 parts by mass or more and 10 parts by mass or less relative to 100 parts by mass of the (A) polyimide.
[0259] From the viewpoint of chemical resistance, the lower limit of the content of the thermal polymerization initiator is more preferably 0.5 parts by mass or more relative to 100 parts by mass of the (A) polyimide.
[0260] From the viewpoint of the storage stability of the negative photosensitive resin composition, the upper limit of the content of the thermal polymerization initiator is more preferably 5 parts by mass or less relative to 100 parts by mass of the (A) polyimide.
[0261] The negative photosensitive resin composition of the present application may contain a plasticizer.
[0262] Examples of the plasticizer include:
[0263] Phthalate ester compounds represented by bis(2-ethylhexyl)phthalate, dicyclohexylphthalate, diphenylphthalate,
[0264] Isophthalic acid ester compounds represented by bis(2-ethylhexyl)isophthalate, dicyclohexylisophthalate, diphenylisophthalate,
[0265] Terephthalate compounds represented by bis(2-ethylhexyl) terephthalate, dicyclohexyl terephthalate, diphenyl terephthalate,
[0266] Trimellitic acid ester compounds represented by tri(2-ethylhexyl) trimellitate, tricyclohexyl trimellitate, and triphenyl trimellitate,
[0267] Pyromellitic acid compounds represented by tetra(2-ethylhexyl)pyromellitate, tetracyclohexylpyromellitate, and tetraphenylpyromellitate,
[0268] Malonic acid ester compounds represented by bis(2-ethylhexyl) malonate, dicyclohexyl malonate, diphenyl malonate,
[0269] Succinate compounds represented by bis(2-ethylhexyl) succinate, dicyclohexyl succinate, diphenyl succinate,
[0270] Glutaric acid ester compounds represented by bis(2-ethylhexyl) glutarate, dicyclohexyl glutarate, diphenyl glutarate,
[0271] Adipate compounds represented by bis(2-ethylhexyl) adipate, dicyclohexyl adipate, diphenyl adipate,
[0272] Pimelate compounds represented by bis(2-ethylhexyl) pimelate, dicyclohexyl pimelate, diphenyl pimelate,
[0273] Suberate ester compounds represented by bis(2-ethylhexyl) suberate, dicyclohexyl suberate, diphenyl suberate,
[0274] Azelaic acid ester compounds represented by bis(2-ethylhexyl) azelate, dicyclohexyl azelate, diphenyl azelate,
[0275] Sebacic acid ester compounds represented by bis(2-ethylhexyl) sebacate, dicyclohexyl sebacate, diphenyl sebacate,
[0276] Aliphatic acid tetrahydrofurfuryl ester compounds represented by tetrahydrofurfuryl propionate, tetrahydrofurfuryl butyrate, and tetrahydrofurfuryl isobutyrate,
[0277] Acrylic acid polymers represented by product name: DISPARLON 230 (manufactured by Kusunoki Chemicals Co., Ltd.) and product name: DISPARLON L-1983N (manufactured by Kusunoki Chemicals Co., Ltd.),
[0278] Silicone compounds represented by product name: DISPARLON 1711EF (manufactured by Kusunoki Chemicals Co., Ltd.), and fluorine compounds represented by product name: DISPARLON U-158 (manufactured by Kusunoki Chemicals Co., Ltd.) and product name: DISPARLON U-160 (manufactured by Kusunoki Chemicals Co., Ltd.).
[0279] Among these compounds, from the viewpoint of compatibility with the (A) polyimide, phthalate compounds, isophthalate compounds, terephthalate compounds, pyromellitic acid ester compounds, trimellitic acid ester compounds, malonate compounds, succinate compounds, glutarate compounds, adipate compounds, pimelate compounds, suberate compounds, azelaic acid ester compounds, sebacate compounds and aliphatic acid tetrahydrofurfuryl compounds are preferred.
[0280] When the negative photosensitive resin composition of the present application contains a plasticizer, the content of the plasticizer is preferably 0.5 parts by mass or more and 40 parts by mass or less relative to 100 parts by mass of the (A) polyimide.
[0281] The lower limit of the content of the plasticizer is more preferably 1 part by mass or more relative to 100 parts by mass of the (A) polyimide from the viewpoint of flatness during coating.
[0282] The upper limit of the content of the plasticizer is more preferably 30 parts by mass or less relative to 100 parts by mass of the (A) polyimide from the viewpoint of flatness during curing.
[0283] The negative photosensitive resin composition of the present application may optionally contain a hindered phenol compound in order to suppress discoloration on the copper surface.
[0284] Examples of the hindered phenol compound include 2,6-di-tert-butyl-4-methylphenol, 2,5-di-tert-butylhydroquinone, octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, isooctyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 4,4'-methylenebis(2,6-di-tert-butylphenol), 4,4'-thiobis(3-methyl-6-tert-butylphenol), 4,4'-butylene-bis(3-methyl-6-tert-butylphenol), triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate], 1,6-hexanediol-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 2,2-thio-diethylenebis[3-( 3,5-di-tert-butyl-4-hydroxyphenyl) propionate], N,N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxy-hydrocinnamic acid), 2,2'-methylene-bis(4-methyl-6-tert-butylphenol), 2,2'-methylene-bis(4-ethyl-6-tert-butylphenol), pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], tris-(3,5-di-tert-butyl-4-hydroxybenzyl)-isocyanurate, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, 1,3,5-tris(3-hydroxy-2,6-dimethyl-4-isopropylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H, 5H)-trione, 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-sec-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris[4-(1-ethylpropyl)-3-hydroxy-2,6-dimethylbenzyl]-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris[4-triethylmethyl-3-hydroxy-2,6-dimethylbenzyl]-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione , 1,3,5-tris(3-hydroxy-2,6-dimethyl-4-phenylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-tert-butyl-3-hydroxy-2,5,6-trimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-tert-butyl-5-ethyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-tert-butyl-6-ethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-Tris(4-tert-butyl-6-ethyl-3-hydroxy-2,5-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-tert-butyl-5,6-diethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-tert-butyl-3-hydroxy-2-methylbenzyl)-1,3 ,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-tert-butyl-3-hydroxy-2,5-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione and 1,3,5-tris(4-tert-butyl-5-ethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, but are not limited thereto.
[0285] Among these, 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione and the like are particularly preferred.
[0286] When the negative photosensitive resin composition of the present application contains a hindered phenol compound, the content thereof is preferably 0.1 parts by mass or more and 20 parts by mass or less relative to 100 parts by mass of the (A) polyimide.
[0287] The lower limit of the hindered phenol compound content is more preferably 0.5 parts by mass or more based on 100 parts by mass of the (A) polyimide from the viewpoint of preventing discoloration and corrosion of copper or copper alloy when forming a negative photosensitive resin composition on copper or copper alloy.
[0288] From the viewpoint of photosensitivity, the upper limit of the content of the hindered phenol compound is more preferably 10 parts by mass or less based on 100 parts by mass of the (A) polyimide.
[0289] In order to improve the adhesion between the film formed using the negative photosensitive resin composition and the substrate, the negative photosensitive resin composition of the present application may optionally contain other adhesive aids in addition to the silane coupling agent. As other adhesive aids, aluminum-based adhesive aids and the like can be used.
[0290] Examples of the aluminum-based adhesion promoter include tris(ethyl acetoacetate)aluminum, trisacetylacetonate aluminum, and ethyl acetoacetate diisopropoxyaluminum.
[0291] When the negative photosensitive resin composition of the present application contains an adhesion aid, the content of the adhesion aid is preferably 0.01 parts by mass or more and 25 parts by mass or less relative to 100 parts by mass of the (A) polyimide.
[0292] From the viewpoint of adhesiveness, the lower limit of the content of the adhesion aid is more preferably 0.5 parts by mass or more relative to 100 parts by mass of the (A) polyimide.
[0293] From the viewpoint of the storage stability of the negative photosensitive resin composition, the upper limit of the content of the adhesion aid is more preferably 20 parts by mass or less relative to 100 parts by mass of the (A) polyimide.
[0294] In order to improve photosensitivity, the negative photosensitive resin composition of the present application may optionally include a sensitizer.
[0295] Examples of the sensitizer include Michler's ketone, 4,4'-bis(diethylamino)benzophenone, 2,5-bis(4'-diethylaminobenzylidene)cyclopentane, 2,6-bis(4'-diethylaminobenzylidene)cyclohexanone, 2,6-bis(4'-diethylaminobenzylidene)-4-methylcyclohexanone, 4,4'-bis(dimethylamino)chalcone, 4,4'-bis(diethylamino)chalcone, p-dimethyl aminocinnamylidene indanone, p-dimethylaminobenzylidene indanone, 2-(p-dimethylaminophenyl biphenylene)benzothiazole, 2-(p-dimethylaminophenyl vinylidene)benzothiazole, 2-(p-dimethylaminophenyl vinylidene)isonaphthothiazole, 1,3-bis(4'-dimethylaminobenzylidene)acetone, 1,3-bis(4'-diethylaminobenzylidene)acetone, 3,3'-carbonyl-bis(7-diethylaminobenzylidene)acetone 3-Acetyl-7-dimethylaminocoumarin, 3-ethoxycarbonyl-7-dimethylaminocoumarin, 3-benzyloxycarbonyl-7-dimethylaminocoumarin, 3-methoxycarbonyl-7-diethylaminocoumarin, 3-ethoxycarbonyl-7-diethylaminocoumarin, N-phenyl-N'-ethylethanolamine, N-phenyldiethanolamine, N-p-tolyldiethanolamine, N-phenylethanolamine, 4-morpholinobenzophenone, isopentyl dimethylaminobenzoate, isopentyl diethylaminobenzoate, 2-mercaptobenzimidazole, 1-phenyl-5-mercaptotetrazole, 2-mercaptobenzothiazole, 2-(p-dimethylaminophenylvinyl)benzoxazole, 2-(p-dimethylaminophenylvinyl)benzothiazole, 2-(p-dimethylaminophenylvinyl)naphtho(1,2-d)thiazole and 2-(p-dimethylaminobenzoyl)styrene, etc. These can be used alone or in combination of two or more, for example, 2 to 5 kinds.
[0296] When the negative photosensitive resin composition of the present application contains a sensitizer for improving photosensitivity, the content of the sensitizer is preferably 0.1 parts by mass or more and 25 parts by mass or less relative to 100 parts by mass of the (A) polyimide.
[0297] In particular, the negative photosensitive resin composition of the present application may optionally contain a thermal polymerization inhibitor in order to improve the viscosity stability and photosensitivity stability when stored in a solution state containing a solvent.
[0298] Examples of the thermal polymerization inhibitor include hydroquinone, N-nitrosodiphenylamine, p-tert-butylcatechol, phenothiazine, N-phenylnaphthylamine, ethylenediaminetetraacetic acid, 1,2-cyclohexanediaminetetraacetic acid, glycol ether diaminetetraacetic acid, 2,6-di-tert-butyl-p-methylphenol, 5-nitroso-8-hydroxyquinoline, 1-nitroso-2-naphthol, 2-nitroso-1-naphthol, 2-nitroso-5-(N-ethyl-N-sulfopropylamino)phenol, N-nitroso-N-phenylhydroxylamine ammonium salt, and N-nitroso-N(1-naphthyl)hydroxylamine ammonium salt.
[0299] The negative photosensitive resin composition of the present application may optionally contain a thermal base generator.
[0300] The negative photosensitive resin composition of the present application may optionally contain a solvent (I). The solvent (I) is not limited as long as it can uniformly dissolve or suspend the (A) polyimide and the (C) photopolymerization initiator.
[0301] Examples of the solvent (I) include γ-butyrolactone (GBL), dimethyl sulfoxide, tetrahydrofurfuryl alcohol, ethyl acetoacetate, N,N-dimethylacetoacetamide, ε-caprolactone, 1,3-dimethyl-2-imidazolidinone, 3-methoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropionamide, N,N-dimethylformamide, N-methyl-2-pyrrolidone (NMP), N-ethyl-2-pyrrolidone, and N,N-dimethylacetamide. These solvents (I) may be used alone or in combination of two or more.
[0302] An appropriate amount of solvent (I) can be used according to the desired coating film thickness and viscosity of the negative photosensitive resin composition. The content of solvent (I) can be, for example, 30 to 1,000 parts by mass, preferably 140 to 1,000 parts by mass, relative to 100 parts by mass of the (A) polyimide.
[0303] When the solvent (I) contains an alcohol having no olefinic double bond, the content of the alcohol having no olefinic double bond in all solvents including the above-mentioned reaction solvent is preferably 5 to 50% by mass. From the viewpoint of storage stability of the negative photosensitive resin composition, the upper limit of the content of the solvent (I) is more preferably 10% by mass or more in all solvents. From the viewpoint of solubility of the (A) polyimide, the lower limit of the content of the solvent (I) is more preferably 30% by mass or less in all solvents.
[0304] <Method for producing a cured relief pattern>
[0305] The method for manufacturing the solidified relief pattern of the present application comprises the following steps:
[0306] (1) a step of coating the negative photosensitive resin composition of the present application on a substrate to form a photosensitive resin layer on the substrate (resin layer forming step);
[0307] (2) a step of exposing the photosensitive resin layer to light (exposure step);
[0308] (3) a step of developing the exposed photosensitive resin layer to form a relief pattern (relief pattern forming step); and
[0309] (4) A step of heat-treating the relief pattern to form a cured relief pattern (cured relief pattern forming step).
[0310] (1) Resin layer forming step
[0311] In this step, the negative photosensitive resin composition of the present application is applied onto a substrate and then dried as necessary to form a photosensitive resin layer.
[0312] As the coating method, a method conventionally used for coating a negative photosensitive resin composition can be used, for example, a method of coating using a spin coater, a bar coater, a blade coater, a curtain coater, a screen printer, or the like, a method of spray coating using a spray coater, or the like.
[0313] The coating film composed of the negative photosensitive resin composition may be dried as needed.
[0314] As a drying method, air drying, heating drying using an oven or a hot plate, vacuum drying, etc. can be used. Specifically, in the case of air drying or heating drying, the drying can be performed under the conditions of 20°C to 150°C and 1 minute to 1 hour. As described above, a photosensitive resin layer can be formed on the substrate.
[0315] The thickness of the coating film (hereinafter referred to as film thickness) may be appropriately adjusted depending on the desired thickness of the polyimide film and the content of the (A) polyimide in the photosensitive resin composition, and is preferably about 1 to 500 μm, particularly preferably about 3 to 100 μm.
[0316] (2) Exposure process
[0317] In this step, the photosensitive resin layer is exposed through a photomask or photomask having a pattern or directly using an ultraviolet light source, etc., using an exposure device such as a contact aligner, a mirror projector, or a stepper. Through this exposure, the polymerizable functional groups of the (A) polyimide contained in the negative photosensitive resin composition are cross-linked by the action of the (C) photopolymerization initiator. Through this cross-linking, the exposed portion becomes insoluble in the developer described later, so that a relief pattern can be formed.
[0318] After exposure, for the purpose of improving photosensitivity, etc., a post-exposure bake (PEB) or a pre-development bake or both can be performed based on any combination of temperature and time as needed. The baking conditions are preferably a temperature of 40°C to 120°C and a time of 10 seconds to 240 seconds, but are not limited to this range as long as the various properties of the negative photosensitive resin composition of the present application are not hindered.
[0319] (3) Relief pattern forming process
[0320] In this step, unexposed portions in the exposed photosensitive resin layer are developed and removed to form a relief pattern.
[0321] As a developing method for developing the photosensitive resin layer after exposure (irradiation), any method can be selected from the conventionally known developing methods for photoresists, such as a rotary spray method, a paddle method, an immersion method accompanied by ultrasonic treatment, etc. After development, post-development baking can be performed based on any combination of temperature and time as needed for the purpose of adjusting the shape of the relief pattern, etc.
[0322] As a developing solution used for development, for example, a good solvent for the negative photosensitive resin composition, or a combination of a good solvent and a poor solvent is preferable.
[0323] As the good solvent, for example, N-methyl-2-pyrrolidone, N-cyclohexyl-2-pyrrolidone, N,N-dimethylacetamide, cyclopentanone, cyclohexanone, γ-butyrolactone, α-acetyl-γ-butyrolactone, and the like are preferred.
[0324] As the poor solvent, preferably, for example, toluene, xylene, methanol, ethanol, isopropanol, ethyl lactate, propylene glycol methyl ether acetate and water are used. When a good solvent and a poor solvent are mixed for use, it is preferred to adjust the ratio of the poor solvent to the good solvent according to the solubility of the polymer in the negative photosensitive resin composition. The developer may also use two or more, for example, several, good solvents and poor solvents in combination.
[0325] (4) Curing relief pattern forming process
[0326] In this step, the relief pattern obtained by development is subjected to a heat treatment to volatilize the photosensitive component, thereby forming a cured relief pattern composed of polyimide.
[0327] As a method for heat treatment, various methods can be selected, for example, a method using a hot plate, a method using an oven, a method using a temperature-raising oven capable of setting a temperature program, and the like.
[0328] The heat treatment can be performed, for example, at 160° C. to 350° C. for 30 minutes to 5 hours. The temperature of the heat treatment is preferably 300° C. or less, more preferably 250° C. or less, and particularly preferably 200° C. or less. As the atmosphere gas during heat curing, air can be used, or an inert gas such as nitrogen or argon can be used.
[0329] The photosensitive resin layer after exposure has a crosslinked structure formed by crosslinking the polymerizable functional group of (A) polyimide and the polymerizable compound having a urea bond (B).
[0330] <Polyimide Cured Film>
[0331] The present application also provides a cured film formed from the negative photosensitive resin composition of the present application. The cured film of the present application contains a cured product of the negative photosensitive resin composition of the present application.
[0332] <Semiconductor devices>
[0333] In the present application, a semiconductor device is also provided, which has a cured relief pattern obtained from the above-mentioned negative photosensitive resin composition. In detail, a semiconductor device is provided, which has a substrate as a semiconductor element and a cured relief pattern. The cured relief pattern can be manufactured using the above-mentioned negative photosensitive resin composition by the above-mentioned method for manufacturing a cured relief pattern.
[0334] The present application also provides a method for manufacturing a semiconductor device, which uses a semiconductor element as a substrate and includes the method for manufacturing a cured relief pattern of the present embodiment as part of the process. In this case, the cured relief pattern formed by the method for manufacturing a cured relief pattern of the present application can be used as a surface protective film, an interlayer insulating film, an insulating film for rewiring, a protective film for a flip chip device, or a protective film for a semiconductor device having a bump structure, and can be manufactured in combination with a known method for manufacturing a semiconductor device.
[0335] <Display device>
[0336] In the present application, a display device is also provided, which has a display element and a cured film arranged on the upper part of the display element, and the cured film is the above-mentioned cured relief pattern. Here, the cured relief pattern can be laminated directly in contact with the display element, or can be laminated with other layers sandwiched therebetween. The cured film can be applied to, for example, surface protective films, insulating films, planarization films, etc. of TFT liquid crystal display elements and color filter elements; protrusions for MVA type liquid crystal display devices; partition walls for cathodes of organic EL elements, etc.
[0337] The negative photosensitive resin composition of the present application is useful for applications such as interlayer insulation of multilayer circuits, cover coats of flexible copper-clad laminates, solder resists, and liquid crystal alignment films, in addition to being applied to the semiconductor devices described above.
[0338] <Method for producing negative photosensitive resin composition>
[0339] In one embodiment, the method for producing a negative photosensitive resin composition of the present application includes the step of producing (A) a polyimide having a polymerizable functional group at a terminal by the method of the present application as described in the above “Method for producing a polyimide having a polymerizable functional group at a terminal”.
[0340] In one embodiment, the method for producing a negative photosensitive resin composition of the present application includes the step of mixing (A) a polyimide having a polymerizable functional group at a terminal, (B) a polymerizable compound having a urea bond, and (C) a photopolymerization initiator to obtain a negative photosensitive resin composition (hereinafter referred to as a mixing step).
[0341] The mixing step is a step of mixing the above-mentioned (A) polyimide having a polymerizable functional group at the terminal, (B) polymerizable compound having a urea bond, (C) photopolymerization initiator, and (I) solvent to obtain a photosensitive resin composition solution.
[0342] In the mixing step, (A) the polyimide having a polymerizable functional group at the terminal, (B) the polymerizable compound having a urea bond, (C) the photopolymerization initiator, and (I) the solvent are the same as described above.
[0343] Optionally, it may further contain additives selected from the group consisting of (D) a monomer having a polymerizable functional group without a urea bond (in one embodiment, a radical polymerizable compound), (E) a silane coupling agent, (F) an organic titanium compound, (G) a thermal crosslinking agent, and (H) a rust inhibitor, as well as other components.
[0344] Example
[0345] Hereinafter, the present embodiment will be specifically described by way of examples, but the present embodiment is not limited thereto. In the examples, comparative examples, preparation examples, and synthesis examples, the physical properties of the polyimide, the polyimide precursor, or the negative photosensitive resin composition were measured and evaluated by the following methods.
[0346] <Measurement and evaluation methods>
[0347] (1) Determination of weight average molecular weight (Mw) and number average molecular weight (Mn)
[0348] The weight average molecular weight (Mw) and number average molecular weight (Mn) of each resin were measured by gel permeation chromatography (GPC) under the following conditions. In addition, the molecular weight distribution was calculated as Mw / Mn.
[0349] The calibration curve for calculating the weight average molecular weight was prepared using standard polystyrene (Easical Type PS-1, manufactured by Agilent Technologies).
[0350] <GPC conditions>
[0351] Device: HLC-8320GPC (manufactured by Tosoh Corporation)
[0352] Eluent: N-methyl-2-pyrrolidone
[0353] Lithium bromide monohydrate 30mmol / L
[0354] Phosphoric acid 50mmol / L
[0355] Flow rate: 0.5mL / min
[0356] Column: TSK-GEL SUPER HM-H 2 pieces / TSK-GEL SUPER H-RC 1 piece (made by Tosoh)
[0357] Column temperature: 40°C
[0358] Detector: UV-8320
[0359] (2) Evaluation of low curing shrinkage: Method for measuring curing shrinkage
[0360] The negative photosensitive resin composition described below was spin-coated on a 6-inch silicon wafer (manufactured by Fujimi Electronics Co., Ltd., thickness 625±25 μm) using a coater developer (D-Spin60A, manufactured by SOKUDO Corporation), and pre-baked on a hot plate at 110°C for 240 seconds to form a thin film about 7 μm thick before curing.
[0361] The film was irradiated with 800 mJ / cm2 using PrismaGHI (manufactured by Ultratech).2 Next, curing by post-baking was performed at 170° C. for 120 minutes in a nitrogen atmosphere using a temperature-programmed curing oven (VF-2000, manufactured by KOYO LINDBERG) to prepare a 6 μm-thick cured film (cured film in one embodiment).
[0362] The film thickness after pre-baking of the obtained film is defined as film thickness A, and the film thickness after post-baking is defined as film thickness B. The film thickness A and the film thickness B are substituted into the following formula to calculate the cure shrinkage ratio.
[0363] Curing shrinkage [%]={(film thickness A-film thickness B) / film thickness A}×100
[0364] (3) Evaluation of heat resistance: Method for measuring Tg of cured film
[0365] The heat resistance of the post-baked film obtained by the method (2) above was measured by the following method.
[0366] The obtained test piece (width 3 mm) was heated to 350°C at a heating rate of 10°C / min using a thermomechanical analyzer (manufactured by Seiko Instruments Inc., product name: TMA / EXSTAR 6000), and the thermal expansion coefficient of the obtained test piece was measured. Next, the glass transition temperature (Tg) of the cured film was calculated from the inflection point of the thermal expansion coefficient based on the obtained measurement results. The unit of Tg is °C.
[0367] (4) Method for measuring elongation of cured film
[0368] Using the post-baked film obtained by the method (2) above, the elongation of the cured film was measured by the following method.
[0369] The obtained test piece was subjected to a tensile test using a tensile tester (manufactured by ORIENTEC CO., LTD., product name: Tensilon UTM-II-20) at 23°C by a method based on JIS K 7161 to measure the tensile elongation (elongation) of the test piece. The tensile speed in the tensile test was set to 40 mm / min. The unit of the elongation of the cured film is %.
[0370] (5) Copper adhesion measurement and evaluation method
[0371] On a 6-inch silicon wafer (manufactured by Fujimi Electronics Co., Ltd., thickness 625±25μm), a sputtering device (L-440S-FHL type, manufactured by CANON ANELVA CORPORATION) was used to sputter 200nm thick Ti and 400nm thick Cu in sequence. Next, a photosensitive resin composition prepared by the method described below was spin-coated on the wafer using a coating developer (Coater Developer) (D-Spin60A type, manufactured by SOKUDO Co., Ltd.), and pre-baked on a hot plate at 110°C for 240 seconds to form a thin film on Cu.
[0372] The film was irradiated with 800 mJ / cm2 using PrismaGHI (manufactured by Ultratech). 2 Next, a heat treatment was performed at 170° C. for 2 hours in a nitrogen atmosphere using a temperature-programmed curing furnace (VF-2000, manufactured by KOYO LINDBERG), thereby obtaining a cured film of about 6 μm thick made of the photosensitive resin composition on Cu.
[0373] The film after the heat treatment was evaluated for adhesion between the copper substrate and the cured film by the cross-cut method according to JIS K 5600-5-6 based on the following criteria.
[0374] "Excellent": The number of cells of the cured film bonded to the substrate exceeds 100
[0375] "Good": The number of grids of the cured film adhered to the substrate is 80 or more and 100 or less
[0376] "OK": The number of grids of the cured film bonded to the substrate is 50 or more and less than 80
[0377] "No": The number of cells of the cured film bonded to the substrate is less than 50
[0378] (6) Oxygen barrier properties measurement and evaluation methods
[0379] The oxygen barrier properties were measured by the following method using the cured film after post-baking obtained by the method (2) above.
[0380] The oxygen permeability (cc / m2) was measured using a gas permeability measuring device (manufactured by GTR TEC Co., Ltd., product name: GTR-10XF (isobaric GC)) according to the isobaric GC method of JIS K 7126-2. 2 ·24h·atm), and the oxygen barrier properties were evaluated based on the following criteria.
[0381] "Excellent": oxygen permeability (cc / m 2 ·24h·atm) less than 200
[0382] "Good": oxygen permeability (cc / m 2 24h atm) is 200 or more but less than 500
[0383] “Yes”: oxygen permeability (cc / m 2 24h atm) is 500 or more but less than 1000
[0384] “No”: oxygen permeability (cc / m 2 24h atm) is 1000 or more
[0385] <Synthesis Example 1: Polyimide A-1>
[0386]
[0387] In a three-necked flask equipped with a Dean-Stark extractor and purged with nitrogen, 148 g of N-methylpyrrolidone (hereinafter referred to as NMP) and 22.1 g (0.08 mol) of 6-(4-aminophenoxy)biphenyl-3-amine (hereinafter referred to as PDPE) were added and dissolved, and 14.9 g (0.06 mol) of bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride (hereinafter referred to as BCD) and 43.8 g of toluene were added thereto, and heated to 180° C. After confirming that the theoretical amount of water (2.16 g) and the added toluene (43.8 g) were extracted from the Dean-Stark apparatus, the heating was stopped and cooled to room temperature.
[0388] The obtained reaction liquid was added dropwise to 2.0 kg of ethanol to precipitate a polymer, and the resultant was filtered and then vacuum dried to obtain a polyimide powder.
[0389] After adding 148 g of NMP to the obtained polyimide and dissolving it, 6.2 g (0.04 mol) of 2-methacryloyloxyethyl isocyanate with a trade name of KARENZ MΟI (manufactured by Resonac Holdings Corporation) was added, and the mixture was stirred at room temperature for 10 hours to obtain a polymer solution. The obtained polymer solution was added dropwise to 2.0 kg of water to precipitate the polymer, and vacuum dried after filtration to obtain a powder of a solvent-soluble polyimide A-1 having a polymerizable functional group at the end.
[0390] The molecular weight of A-1 was measured by gel permeation chromatography (in terms of standard polystyrene), and the results showed that Mw was 10300, Mn was 7400, and Mw / Mn was 1.39. The terminal modification rate was confirmed to be 99% from the integration ratio of proton NMR.
[0391] <Synthesis Example: Polyimide A-2>
[0392] The reaction was carried out in the same manner as in Synthesis Example 1 except that the PDPE in Synthesis Example 1 was changed to 33.2 g (0.12 mol) and the KARENZ MOI was changed to 18.6 g (0.12 mol), thereby obtaining a solvent-soluble polyimide A-2 having a polymerizable functional group at the terminal.
[0393] The molecular weight of A-2 was measured by gel permeation chromatography (in terms of standard polystyrene), and the results showed that Mw was 5300, Mn was 4800, and Mw / Mn was 1.10. The terminal modification rate was confirmed to be 98% from the integration ratio of proton NMR.
[0394] <Synthesis Example 3: Polyimide A-3>
[0395]
[0396] A solvent-soluble polyimide A-3 having a polymerizable functional group at the terminal was obtained by reacting in the same manner as in Synthesis Example 1 except that BCD in Synthesis Example 1 was changed to 18.6 g (0.06 mol) of 4,4′-oxydiphthalic anhydride (hereinafter referred to as ODPA).
[0397] The molecular weight of A-3 was measured by gel permeation chromatography (in terms of standard polystyrene), and the results showed that Mw was 12100, Mn was 8600, and Mw / Mn was 1.41. In addition, the terminal modification rate was confirmed to be 99% from the integration ratio of proton NMR.
[0398] <Synthesis Example 4: Polyimide A-4>
[0399] The reaction was carried out in the same manner as in Synthesis Example 1 except that KARENZ MOI in Synthesis Example 1 was changed to 8.0 g (0.04 mol) of 2-(2-methacryloyloxyethoxy)ethyl isocyanate with a trade name of KARENZ MOI-EG (manufactured by Resonac Holdings Corporation), thereby obtaining a solvent-soluble polyimide A-4 having a polymerizable functional group at the terminal.
[0400] The molecular weight of A-4 was measured by gel permeation chromatography (in terms of standard polystyrene), and the results showed that Mw was 11400, Mn was 8500, and Mw / Mn was 1.34. In addition, the terminal modification ratio was confirmed to be 100% from the integration ratio of proton NMR.
[0401] <Synthesis Example 5: Polyimide A-5>
[0402] The reaction was carried out in the same manner as in Synthesis Example 1 except that KARENZ MOI in Synthesis Example 1 was replaced with 5.6 g (0.04 mol) of 2-acryloyloxyethyl isocyanate with the trade name of KARENZ AOI (manufactured by Resonac Holdings Corporation) to obtain a solvent-soluble polyimide A-5 having a polymerizable functional group at the terminal.
[0403] The molecular weight of A-5 was measured by gel permeation chromatography (in terms of standard polystyrene), and the results showed that Mw was 10600, Mn was 7700, and Mw / Mn was 1.38. The terminal modification ratio was confirmed to be 100% from the integration ratio of proton NMR.
[0404] <Synthesis Example 6: Polyimide A-6>
[0405] The reaction was carried out in the same manner as in Synthesis Example 1 except that KARENZ MOI in Synthesis Example 1 was replaced with 9.6 g (0.04 mol) of 1,1-(bisacryloyloxymethyl)ethyl isocyanate with the trade name of KARENZ BEI (manufactured by Resonac Holdings Corporation) to obtain a solvent-soluble polyimide A-6 having a polymerizable functional group at the terminal.
[0406] The molecular weight of A-6 was measured by gel permeation chromatography (in terms of standard polystyrene), and the results showed that Mw was 11900, Mn was 8800, and Mw / Mn was 1.35. The terminal modification rate was confirmed to be 98% from the integration ratio of proton NMR.
[0407] <Synthesis Example 7: Polyimide A-7>
[0408] The reaction was carried out in the same manner as in Synthesis Example 1 except that the PDPE in Synthesis Example 1 was changed to 17.5 g (0.06 mol) and the KARENZ MOI was changed to 1.0 g (0.006 mol), thereby obtaining a solvent-soluble polyimide A-7 having a polymerizable functional group at the terminal.
[0409] The molecular weight of A-7 was measured by gel permeation chromatography (in terms of standard polystyrene), and the results showed that Mw was 38700, Mn was 27100, and Mw / Mn was 1.43. The terminal modification rate was confirmed to be 99% from the integration ratio of proton NMR.
[0410] <Synthesis Example: Polyimide A-8>
[0411] The reaction was carried out in the same manner as in Synthesis Example 1 except that the PDPE in Synthesis Example 1 was changed to 49.7 g (0.18 mol) and the KARENZ MOI was changed to 37.2 g (0.24 mol), thereby obtaining a solvent-soluble polyimide A-8 having a polymerizable functional group at the terminal.
[0412] The molecular weight of A-8 was measured by gel permeation chromatography (in terms of standard polystyrene), and the results showed that Mw was 2900, Mn was 2700, and Mw / Mn was 1.07. In addition, the terminal modification rate was confirmed to be 99% from the integration ratio of proton NMR.
[0413] <Synthesis Example 9: Polyimide A-9>
[0414]
[0415] The reaction was carried out in the same manner as in Synthesis Example 1 except that KARENZ MOI of Synthesis Example 1 was not added, thereby obtaining a solvent-soluble polyimide A-9 having no polymerizable functional group at the terminal.
[0416] The molecular weight of A-9 was measured by gel permeation chromatography (in terms of standard polystyrene), and the results showed that Mw was 10200, Mn was 7200, and Mw / Mn was 1.42. In addition, the terminal modification rate was confirmed to be 0% from the integration ratio of proton NMR.
[0417] <Synthesis Example 10: Polyimide Precursor A-10>
[0418] ODPA 18.6 g (0.06 mol) was added to a 1 L separable flask, and γ-butyrolactone 60 g was added. Then, 2-hydroxyethyl methacrylate 15.6 g (0.12 mol) was added, and pyridine 9.5 g (0.12 mol) was added while stirring, and then stirred at 40° C. for 5 hours using an oil bath to obtain a reaction mixture. After the reaction was completed, the mixture was naturally cooled to room temperature and left for 16 hours.
[0419] Then, while stirring the obtained reaction mixture, a solution of 24.2 g (0.12 mol) of N, N'-dicyclohexylcarbodiimide dissolved in 30 g of γ-butyrolactone was added under ice cooling for 40 minutes, and then a solution of 22.1 g (0.08 mol) of PDPE dissolved in 90 g of γ-butyrolactone was added for 60 minutes. After stirring at room temperature for 2 hours, 180 g of ethanol was added and further stirred for 1 hour, and then 140 g of γ-butyrolactone was added. The reaction mixture was filtered to remove the precipitate produced in the reaction system to obtain a reaction solution. The obtained reaction solution was added to 1.4 kg of ethanol to precipitate a crude polymer. The precipitated crude polymer was filtered out and dissolved in 180 g of γ-butyrolactone to obtain a crude polymer solution. The obtained crude polymer solution was added dropwise to 2.0 kg of water to reprecipitate the polymer. After filtering out the obtained reprecipitate, vacuum drying was performed to obtain a powdered polyimide precursor A-10.
[0420] The molecular weight of A-10 was measured by gel permeation chromatography (based on standard polystyrene). As a result, Mw was 12,700, Mn was 6,900, and Mw / Mn was 1.84.
[0421] <Synthesis Example 11: B-1>
[0422]
[0423] 27.6 g (0.10 mol) of PDPE was added to a 300 mL separable flask, and 58.6 g of NMP was added.
[0424] KARENZ MOI: 31.0 g (0.20 mol) of 2-methacryloyloxyethyl isocyanate was added under ice-cooling while stirring, and the mixture was stirred at room temperature for 10 hours to obtain an NMP solution of a polymerizable compound B-1 having a urea bond.
[0425] The modification rate of B-1 was confirmed to be 100% from the integrated ratio of proton NMR.
[0426] <Synthesis Example 12: B-2>
[0427] The reaction was carried out in the same manner as in Synthesis Example 11 except that KARENZ M01 in Synthesis Example 11 was changed to KARENZ M01-EG: 39.8 g (0.20 mol) of 2-(2-methacryloyloxyethyloxy)ethyl isocyanate to obtain an NMP solution of a polymerizable compound B-2 having a urea bond.
[0428] The modification rate of B-2 was confirmed to be 100% from the integrated ratio of proton NMR.
[0429] <Synthesis Example 13: B-3>
[0430] A reaction was carried out in the same manner as in Synthesis Example 11 except that KARENZ MOI in Synthesis Example 11 was changed to KARENZ AOI: 28.2 g (0.20 mol) of 2-acryloyloxyethyl isocyanate to obtain an NMP solution of a polymerizable compound B-3 having a urea bond.
[0431] The modification rate of B-3 was confirmed to be 100% from the integrated ratio of proton NMR.
[0432] <Synthesis Example 14: B-4>
[0433] A reaction was carried out in the same manner as in Synthesis Example 11 except that KARENZ MOI in Synthesis Example 11 was changed to KARENZ BEI: 47.8 g (0.20 mol) of 1,1-(bisacryloyloxymethyl)ethyl isocyanate to obtain an NMP solution of a polymerizable compound B-4 having a urea bond.
[0434] The modification rate of B-4 was confirmed to be 100% from the integrated ratio of proton NMR.
[0435] <Synthesis Example 15: B-5>
[0436] A reaction was carried out in the same manner as in Synthesis Example 11 except that PDPE in Synthesis Example 11 was changed to 20.0 g (0.10 mol) of 4,4′-diaminodiphenyl ether to obtain an NMP solution of a polymerizable compound B-5 having a urea bond.
[0437] The modification rate of B-5 was confirmed to be 100% from the integrated ratio of proton NMR.
[0438] <Example 1> (Preparation of negative photosensitive resin composition)
[0439] A negative photosensitive resin composition was prepared by the following method, and the prepared composition was evaluated.
[0440] A-1: 100 g of a polyimide having a polymerizable functional group at the end (A), B-1: 10 g of a polymerizable compound having a urea bond (B), and TR-PBG-3057 (trade name, manufactured by Changzhou Qiangli Electronic New Materials Co., Ltd.) (C-1): 2 g of a photopolymerization initiator (C) were dissolved in a solvent (I-1): 208 g of N-methyl-2-pyrrolidone (NMP) to prepare a negative photosensitive resin composition having a total solid content of 35% by mass. The composition was evaluated according to the above method. The results are shown in Table 1.
[0441] In addition, the unit of the numerical value described in a table|surface represents a mass part unless otherwise specified.
[0442] <Examples 1 to 28 and Comparative Examples 1 to 3>
[0443] A negative photosensitive resin composition was prepared in the same manner as in Example 1 except that the polymer and other additives (B) to (I) shown in Table 1 were used, and evaluation was performed in the same manner as in Example 1. The results are shown in Table 1.
[0444]
Table 1-1
[0445]
Table 1-1
[0446]
[0447]
Table 1-2
[0448]
Table 1-2
[0449]
[0450]
Table 1-3
[0451]
Table 1-3
[0452]
[0453]
Table 1-4
[0454]
Table 1-4
[0455]
[0456] <Other additives>
[0457] C-1: TR-PBG-3057 (trade name; Changzhou Qiangli Electronic New Materials Co., Ltd.)
[0458] C-2: TR-PBG-304 (trade name; Changzhou Qiangli Electronic New Materials Co., Ltd.)
[0459] D-1: Tetraethylene glycol dimethacrylate
[0460] D-2: Tris-(2-acryloyloxyethyl) isocyanurate
[0461] D-3: Pentaerythritol tetraacrylate
[0462] E-1: N-phenyl-3-aminopropyltrimethoxysilane
[0463] E-2: 3-Glycidoxypropyltrimethoxysilane
[0464] F-1: Titanium(IV) acetylacetonate
[0465] G-1: 1,3-bis(methoxymethyl)urea
[0466] G-2: 1,3,4,6-Tetrakis(methoxymethyl)glycoluril
[0467] H-1: 8-azaadenine
[0468] H-2: 5-amino-1H-tetrazole
[0469] I-1: N-methyl-2-pyrrolidone
[0470] The evaluation results in Table 1 show that Comparative Examples 1 to 3, which do not satisfy the requirements of the present application, cannot achieve good balance in all the properties of low cure shrinkage, heat resistance, elongation of the cured film, copper adhesion, and oxygen barrier properties.
[0471] On the other hand, Examples 1 to 28 showed excellent performance in all of the properties including low cure shrinkage, heat resistance, elongation of the cured film, copper adhesion, and oxygen barrier properties.
[0472] In the present application, excellent performance means that the curing shrinkage is 6% or less, the heat resistance is 235° C. or more, the elongation of the cured film is 20% or more, and the copper adhesion and oxygen barrier properties are "acceptable" or above.
[0473] Industrial Applicability
[0474] By using the photosensitive resin composition of the present invention, a photosensitive resin composition having low curing shrinkage and excellent heat resistance, mechanical strength (elongation of the cured film), adhesion to copper and oxygen barrier properties among the film properties after low-temperature curing can be obtained, as well as a method for producing a cured relief pattern and a polyimide cured film using the same. The present invention can be suitably used in the field of photosensitive materials useful for manufacturing electrical and electronic materials such as semiconductor devices and multilayer wiring substrates.
Claims
1. A negative photosensitive resin composition, comprising: (A) a polyimide having a polymerizable functional group at the terminal, (B) a polymerizable compound having a urea bond, and (C) Photopolymerization initiator.
2. The negative photosensitive resin composition according to claim 1, in, The side chain of the polyimide (A) does not have a polymerizable functional group.
3. The negative photosensitive resin composition according to claim 1 or 2, in, The (A) polyimide and the (B) polymerizable compound have a structure derived from the same diamine.
4. The negative photosensitive resin composition according to claim 1 or 2, in, The content of the (B) polymerizable compound is 0.1 to 50 parts by mass based on 100 parts by mass of the (A) polyimide.
5. The negative photosensitive resin composition according to claim 1 or 2, in, The weight average molecular weight Mw of the (A) polyimide is 3,000 or more and 30,000 or less. 6 . The negative photosensitive resin composition according to claim 1 , further comprising (D) a monomer having a polymerizable functional group and having no urea bond. 7 . The negative photosensitive resin composition according to claim 1 , further comprising (E) a silane coupling agent. 8 . The negative photosensitive resin composition according to claim 1 , further comprising (F) an organic titanium compound. 9 . The negative photosensitive resin composition according to claim 1 , further comprising (G) a thermal crosslinking agent. 10 . The negative photosensitive resin composition according to claim 1 , further comprising (H) a rust inhibitor.
11. A method for manufacturing a solidified relief pattern, comprising the following steps: (1) a step of coating the negative photosensitive resin composition according to claim 1 or 2 on a substrate to form a photosensitive resin layer on the substrate; (2) exposing the photosensitive resin layer to light; (3) developing the exposed photosensitive resin layer to form a relief pattern; and (4) A step of heating the relief pattern to form a cured relief pattern.
12. The negative photosensitive resin composition according to claim 1 or 2, in, The oxygen permeability (cc / m 2 ·24h·atm) is less than 1000.