High-temperature-resistant cable applied to new energy automobile and preparation method of high-temperature-resistant cable
Through multi-layer multi-gradient coating technology and the use of graphene materials, the problem of signal control wire core breakage, insulating layer aging and poor wear resistance of charging cables of new energy vehicles is solved, and the high temperature and friction resistance of the cable is improved. Extend service life and reduce maintenance costs.
Patent Information
- Application Number
- CN202411083292.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-12
AI Technical Summary
During the use of charging cables for new energy vehicles, there are problems such as signal control wire core breakage, accelerated aging of insulation layer and poor wear resistance, resulting in short service life and increased maintenance costs.
Using multi-layer multi-gradient coating technology, conductor layer, insulating layer, flame retardant layer, high-temperature resistance layer, buffer layer and wear-resistant layer are designed. By wrapping glass fibers and adding graphene materials, the cables are improved with high temperature resistance, friction resistance and Material toughness.
It significantly improves the high temperature, friction resistance and material strength of the cable, extends the service life and reduces maintenance costs.
Smart Images

Figure CN118942786A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of vehicle cables, and in particular to a high temperature resistant cable used in new energy vehicles and a preparation method thereof. Background Art
[0002] With the development of the new energy vehicle industry, new energy vehicles have experienced a blowout growth since 2016, and a large number of charging station infrastructures have been built. As of the end of 2017, there were 214,000 public charging piles and 232,000 private charging piles built with vehicles. Charging cables for new energy vehicles are mainly used to connect electric vehicle charging devices (charging piles) with charging infrastructure (charging guns) to transmit power to electric vehicles. The rapid development of new energy vehicles has driven the development of charging cables. In 2017, the demand for charging cables reached 2,000 km. In response to the problems of long charging time and short driving range faced by the promotion of new energy vehicles, in 2016, Swiss Haoxun Cable released a cooling charging cable and its connector, which can achieve high-power and fast charging of electric vehicles. In the face of the problems existing in the use of charging cables and the demand for high-power and fast charging, a high-temperature resistant DC charging cable for new energy vehicles has been successfully developed through structural design, material selection, and process optimization.
[0003] Charging cables for new energy vehicles include AC charging cables and DC charging cables. Both can perform signal testing and temperature monitoring while meeting the requirements of power transmission, thereby ensuring a safe and reliable charging process. However, after tracking and investigating the use of existing charging cables for new energy vehicles, it was found that the following major problems still exist when using charging cables: 1. Since DC charging cables have not only power cores but also signal control cores, different cores have different cross-sections and can withstand different tensile forces. Therefore, during use, there is a phenomenon of signal control core breakage, which causes the charging signal or temperature to lose monitoring and the electronic lock signal to be abnormal. 2. In order to increase the charging speed and charging efficiency, the current charging current of the charging pile has reached 250A, which is bound to increase the heating of the conductor. Under the impact of long-term high current, the insulation layer of the charging cable will accelerate aging and reduce its service life. 3. Charging cables are used outdoors for a long time, exposed to wind and sun, and also suffer from dragging friction during use. Conventional thermoplastic elastomer materials with poor wear resistance, sticky surface, and non-resistant printing are no longer applicable. The above three problems seriously affect the service life of charging cables for new energy vehicles, resulting in them having to be replaced within 3 years, which is bound to increase maintenance costs.
[0004] Therefore, based on the multi-level and multi-gradient coating of the core material and the performance modification of different layers, this method proposes a high-temperature resistant cable for new energy vehicles and its preparation method. On the basis of ensuring the performance of the original cable, the high-temperature resistance, friction resistance and material toughness of the cable under the new process are greatly improved, which is suitable for industrial promotion. Summary of the invention
[0005] The present invention aims to provide a high temperature resistant cable for use in new energy vehicles and a preparation method thereof. By improving relevant processes and raw materials, the high temperature resistance and material strength of the high temperature resistant cable for new energy vehicles are improved.
[0006] The key points of this method are: 1. From the inside to the outside, this product is a conductor layer, an insulating layer, a flame retardant layer, a high temperature resistant layer, a buffer layer and a wear-resistant layer, and the order between the layers cannot be changed; 2. Before coating the insulating layer, a circle of glass fiber is wrapped around the surface of the conductor layer, which can improve the bonding strength between the insulating layer and the conductor layer during the later coating process, and avoid the problem of local failure of the insulating layer due to high temperature or other reasons; 3. In this product, adding graphene material to the buffer layer is beneficial to the thermal conductivity of the material buffer layer. In this method, the buffer layer foaming material has a large number of pores that will reduce the thermal conductivity of the material, causing local heat to rise and causing separation between different layers due to uneven heat.
[0007] The specific implementation scheme of a high temperature resistant cable applied to new energy vehicles and a preparation method thereof according to the present invention is as follows:
[0008] S1. preparing a copper conductor layer by microalloying and twisting copper wires;
[0009] Microalloying: The surface of the copper wire is microalloyed under vacuum conditions at 550-600°C. The alloying element is one of zinc, aluminum, magnesium, silver, etc. The surface content after alloying treatment is 0.001-0.01%, and the diameter of the copper wire is 0.1-0.3mm;
[0010] Twisting: twisting multiple alloyed copper wires in the same direction to obtain a copper conductor layer;
[0011] S2. A polytetrafluoroethylene insulation layer is obtained by winding glass fiber and polytetrafluoroethylene around the outer layer of the copper conductor;
[0012] Winding glass fiber: In S1, the outer layer of the copper conductor is wound with glass fiber, the winding angle is 45°-60°, the middle span is 1-5mm, and the diameter of a single strand of glass fiber is 0.2-0.5mm;
[0013] Polytetrafluoroethylene coating: Put the polytetrafluoroethylene insulation material into the extruder, and extrude and coat it on the surface of the copper conductor layer coated with glass fiber to form a polytetrafluoroethylene insulation layer;
[0014] S3. Preparing a flame retardant layer on the surface of the insulating layer by mixing and coating the flame retardant layer;
[0015] Mixing: 80-120 parts of silicone rubber, 150-250 parts of metal hydroxide, 60-100 parts of unsaturated carboxylate, 5-10 parts of peroxide, 20-22 parts of montmorillonite, and 1-3 parts of graphene are mixed at 20-100° C. for 5-30 minutes, and then vulcanized on a flat vulcanizer at 150-200° C. for 10-30 minutes to obtain a flame retardant rubber;
[0016] Insulation layer coating: Extruding and coating the prepared flame-retardant rubber on the surface of the polytetrafluoroethylene insulation layer prepared in step S2 to obtain a flame-retardant layer;
[0017] S4. Preparing a flame retardant layer with a high temperature resistant surface layer by mixing and coating the high temperature layer;
[0018] Mixing: 60-80 parts of methyl vinyl rubber, 0.8-1.2 parts of white carbon black activated dispersant, 15-25 parts of white carbon black, 1-2 parts of iron oxide, 1-3 parts of zinc oxide, 2-4 parts of high temperature resistant agent, 0.8-1.2 parts of accelerator dibenzothiazole disulfide, 1.2-1.8 parts of benzoyl peroxide, 2-3 parts of 2,2,4-trimethyl-1,2-dihydroquinoline polymer, 5-15 parts of methyl tin heat stabilizer, 2-7 parts of vulcanizing agent are mixed until uniform, and then vulcanized on a flat vulcanizer at 120-200°C for 10-30 minutes to obtain high temperature resistant rubber;
[0019] Flame retardant layer coating: Extruding and coating the prepared high temperature resistant rubber on the surface of the flame retardant layer prepared in step S3 to obtain a high temperature resistant layer;
[0020] S5. Preparing a high temperature resistant surface buffer layer by mixing and coating the buffer layer;
[0021] Mixing: 90-120 parts of EPDM rubber, 20-40 parts of chloroprene rubber, 20-30 parts of stainless steel fiber, 3-8 parts of graphene, 3-7 parts of stearic acid, 15-25 parts of zinc borate, 5-25 parts of calcium carbonate, 5-20 parts of antimony trioxide, 1-2 parts of sulfur, 4-8 parts of accelerator, and 5-10 parts of foaming agent are mixed evenly, and then evenly spread on the surface of PET fluoroplastic release film, placed in a drying oven, and vulcanized and foamed at 120-150°C to obtain porous rubber, wherein the stainless steel fiber has a wire diameter of 10-30um;
[0022] Buffer layer coating: Extruding and coating the prepared porous rubber on the high temperature resistant surface prepared in step S4 to obtain a buffer layer;
[0023] S6. Preparing a wear-resistant layer on the surface of the buffer layer by mixing and coating the wear-resistant layer;
[0024] Mixing: 100-150 parts of styrene-butadiene rubber, 80-120 parts of natural rubber, 2-10 parts of graphene, 3-8 parts of stearic acid, 3-7 parts of accelerator, 0.5-1.5 parts of antioxidant, 10-20 parts of alumina powder, 10-200 parts of white carbon black, 3-8 parts of coupling agent, 5-10 parts of phenolic resin, 0.5-1.0 parts of HMT, 5-8 parts of sulfur, 5-15 parts of antimony trioxide and 10-30 parts of aluminum hydroxide are mixed to obtain wear-resistant rubber;
[0025] Wear-resistant layer coating: Extruding and coating the prepared porous rubber on the surface of the wear-resistant layer prepared in step S5 to obtain a buffer layer;
[0026] S7. The coated cable is cooled in a continuous cooling water tank and then wound up using a wire take-up machine to obtain a cable product.
[0027] Beneficial effects:
[0028] (1) The cable structure designed by the present invention includes a conductor layer, an insulating layer, a flame retardant layer, a high temperature resistant layer, a buffer layer and a wear-resistant layer from the inside to the outside, which fully considers the thermal conductivity of the material, the bonding strength between the layers and the impact and friction resistance of the material, and has excellent overall performance;
[0029] (2) In the method designed by the present invention, graphene and white carbon black components are added to the flame retardant layer, the high temperature resistant layer, the buffer layer, and the wear resistant layer, which is conducive to the material transferring a large amount of heat from the conductor layer to avoid local overheating. In addition, these two materials are also conducive to improving the mechanical strength of different layers;
[0030] (3) The stainless steel fiber added to the buffer layer in the method designed by the present invention significantly improves the thermal conductivity and strength of the buffer layer. In addition, the stainless steel fiber can also play a good shielding effect to prevent the conductor layer from generating large electromagnetic radiation and affecting other electrical components. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The present invention is a preparation flow chart of a high temperature resistant cable used in new energy vehicles and a preparation method thereof;
[0032] Figure 2 The product structure diagram of a high temperature resistant cable used in new energy vehicles and its preparation method. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0034] The embodiment of the present invention provides a high temperature resistant cable for use in new energy vehicles and a preparation method thereof, the method mainly comprising the following steps:
[0035] S1. preparing a copper conductor layer by microalloying and twisting copper wires;
[0036] S2. A polytetrafluoroethylene insulation layer is obtained by winding glass fiber and polytetrafluoroethylene around the outer layer of the copper conductor;
[0037] S3. Preparing a flame retardant layer on the surface of the insulating layer by mixing and coating the flame retardant layer;
[0038] S4. Preparing a flame retardant layer with a high temperature resistant surface layer by mixing and coating the high temperature layer;
[0039] S5. Preparing a high temperature resistant surface buffer layer by mixing and coating the buffer layer;
[0040] S6. Preparing a wear-resistant layer on the surface of the buffer layer by mixing and coating the wear-resistant layer;
[0041] S7. After the coated cable is cooled in a continuous cooling water tank, the cable is wound up using a take-up machine to obtain a cable product;
[0042] As an embodiment, the following content of the embodiments of the present invention gives several specific examples of the aforementioned high temperature resistant cable applied to new energy vehicles and its preparation method, such as Example 1, Example 2, Example 3 and Examples 1-7 for comparison and explanation.
[0043] Embodiment 1:
[0044] S1. preparing a copper conductor layer by microalloying and twisting copper wires;
[0045] Microalloying: The surface of the copper wire is microalloyed at 550°C under vacuum conditions. The alloying element is one of zinc, aluminum, magnesium, silver, etc. The surface content after alloying treatment is 0.001%, and the diameter of the copper wire is 0.1mm.
[0046] Twisting: twisting multiple alloyed copper wires in the same direction to obtain a copper conductor layer;
[0047] S2. A polytetrafluoroethylene insulation layer is obtained by winding glass fiber and polytetrafluoroethylene around the outer layer of the copper conductor;
[0048] Winding glass fiber: In S1, the outer layer of the copper conductor is wound with glass fiber, the winding angle is 45°, the middle span is 1mm, and the diameter of a single strand of glass fiber is 0.2mm;
[0049] Polytetrafluoroethylene coating: Put the polytetrafluoroethylene insulation material into the extruder, and extrude and coat it on the surface of the copper conductor layer coated with glass fiber to form a polytetrafluoroethylene insulation layer;
[0050] S3. Preparing a flame retardant layer on the surface of the insulating layer by mixing and coating the flame retardant layer;
[0051] Mixing: 80 parts of silicone rubber, 150 parts of metal hydroxide, 60 parts of unsaturated carboxylate, 5 parts of peroxide, 20 parts of montmorillonite and 1 part of graphene were mixed at 20°C for 5 minutes, and then vulcanized on a flat vulcanizer at 150°C for 10 minutes to obtain a flame retardant rubber;
[0052] Insulation layer coating: Extruding and coating the prepared flame-retardant rubber on the surface of the polytetrafluoroethylene insulation layer prepared in step S2 to obtain a flame-retardant layer;
[0053] S4. Preparing a flame retardant layer with a high temperature resistant surface layer by mixing and coating the high temperature layer;
[0054] Mixing: 60 parts of methyl vinyl rubber, 0.8 parts of white carbon black activated dispersant, 15 parts of white carbon black, 1 part of iron oxide, 1 part of zinc oxide, 2 parts of high temperature resistant agent, 0.8 parts of accelerator dibenzothiazole disulfide, 1.2 parts of benzoyl peroxide, 2 parts of 2,2,4-trimethyl-1,2-dihydroquinoline polymer, 5 parts of methyl tin heat stabilizer, and 2 parts of vulcanizing agent are mixed until uniform, and then vulcanized on a flat vulcanizer at 120°C for 10 minutes to obtain a high temperature resistant rubber;
[0055] Flame retardant layer coating: Extruding and coating the prepared high temperature resistant rubber on the surface of the flame retardant layer prepared in step S3 to obtain a high temperature resistant layer;
[0056] S5. Preparing a high temperature resistant surface buffer layer by mixing and coating the buffer layer;
[0057] Mixing: 90 parts of EPDM rubber, 20 parts of chloroprene rubber, 20 parts of stainless steel fiber, 3 parts of graphene, 3 parts of stearic acid, 15 parts of zinc borate, 5 parts of calcium carbonate, 5 parts of antimony trioxide, 1 part of sulfur, 4 parts of accelerator, and 5 parts of foaming agent are mixed evenly, and then evenly spread on the surface of PET fluoroplastic release film, placed in a drying oven, and vulcanized and foamed at 120°C to obtain porous rubber, wherein the stainless steel fiber has a wire diameter of 10um;
[0058] Buffer layer coating: Extruding and coating the prepared porous rubber on the high temperature resistant surface prepared in step S4 to obtain a buffer layer;
[0059] S6. Preparing a wear-resistant layer on the surface of the buffer layer by mixing and coating the wear-resistant layer;
[0060] Mixing: 100 parts of styrene-butadiene rubber, 80 parts of natural rubber, 2 parts of graphene, 3 parts of stearic acid, 3 parts of accelerator, 0.5 parts of antioxidant, 10 parts of alumina powder, 10 parts of white carbon black, 3 parts of coupling agent, 5 parts of phenolic resin, 0.5 parts of HMT, 5 parts of sulfur, 5 parts of antimony trioxide and 10 parts of aluminum hydroxide are mixed to obtain wear-resistant rubber;
[0061] Wear-resistant layer coating: Extruding and coating the prepared porous rubber on the surface of the wear-resistant layer prepared in step S5 to obtain a buffer layer;
[0062] S7. The coated cable is cooled in a continuous cooling water tank and then wound up using a wire take-up machine to obtain a cable product.
[0063] Embodiment 2:
[0064] S1. preparing a copper conductor layer by microalloying and twisting copper wires;
[0065] Microalloying: The surface of the copper wire is microalloyed at 600°C under vacuum conditions. The alloying element is one of zinc, aluminum, magnesium, silver, etc. The surface content after alloying treatment is 0.01%, and the diameter of the copper wire is 0.3mm.
[0066] Twisting: twisting multiple alloyed copper wires in the same direction to obtain a copper conductor layer;
[0067] S2. A polytetrafluoroethylene insulation layer is obtained by winding glass fiber and polytetrafluoroethylene around the outer layer of the copper conductor;
[0068] Winding glass fiber: In S1, the outer layer of the copper conductor is wound with glass fiber, the winding angle is 60°, the middle span is 5mm, and the diameter of a single strand of glass fiber is 0.5mm;
[0069] Polytetrafluoroethylene coating: Put the polytetrafluoroethylene insulation material into the extruder, and extrude and coat it on the surface of the copper conductor layer coated with glass fiber to form a polytetrafluoroethylene insulation layer;
[0070] S3. Preparing a flame retardant layer on the surface of the insulating layer by mixing and coating the flame retardant layer;
[0071] Mixing: 120 parts of silicone rubber, 250 parts of metal hydroxide, 100 parts of unsaturated carboxylate, 10 parts of peroxide, 22 parts of montmorillonite and 3 parts of graphene were mixed at 100°C for 30 minutes, and then vulcanized on a flat vulcanizer at 200°C for 30 minutes to obtain a flame retardant rubber;
[0072] Insulation layer coating: Extruding and coating the prepared flame-retardant rubber on the surface of the polytetrafluoroethylene insulation layer prepared in step S2 to obtain a flame-retardant layer;
[0073] S4. Preparing a flame retardant layer with a high temperature resistant surface layer by mixing and coating the high temperature layer;
[0074] Mixing: 80 parts of methyl vinyl rubber, 1.2 parts of white carbon black activated dispersant, 25 parts of white carbon black, 2 parts of iron oxide, 1-3 parts of zinc oxide, 4 parts of high temperature resistant agent, 1.2 parts of accelerator dibenzothiazole disulfide, 1.8 parts of benzoyl peroxide, 3 parts of 2,2,4-trimethyl-1,2-dihydroquinoline polymer, 15 parts of methyl tin heat stabilizer, and 7 parts of vulcanizing agent are mixed until uniform, and then vulcanized on a flat vulcanizer at 200°C for 30 minutes to obtain high temperature resistant rubber;
[0075] Flame retardant layer coating: Extruding and coating the prepared high temperature resistant rubber on the surface of the flame retardant layer prepared in step S3 to obtain a high temperature resistant layer;
[0076] S5. Preparing a high temperature resistant surface buffer layer by mixing and coating the buffer layer;
[0077] Mixing: 120 parts of EPDM rubber, 40 parts of chloroprene rubber, 30 parts of stainless steel fiber, 8 parts of graphene, 7 parts of stearic acid, 25 parts of zinc borate, 25 parts of calcium carbonate, 20 parts of antimony trioxide, 2 parts of sulfur, 8 parts of accelerator, and 10 parts of foaming agent are mixed evenly, and then evenly spread on the surface of PET fluoroplastic release film, placed in a drying oven, and vulcanized and foamed at 150°C to obtain porous rubber, wherein the stainless steel fiber has a wire diameter of 30um;
[0078] Buffer layer coating: Extruding and coating the prepared porous rubber on the high temperature resistant surface prepared in step S4 to obtain a buffer layer;
[0079] S6. Preparing a wear-resistant layer on the surface of the buffer layer by mixing and coating the wear-resistant layer;
[0080] Mixing: 150 parts of styrene-butadiene rubber, 120 parts of natural rubber, 10 parts of graphene, 8 parts of stearic acid, 7 parts of accelerator, 1.5 parts of antioxidant, 20 parts of alumina powder, 200 parts of white carbon black, 8 parts of coupling agent, 10 parts of phenolic resin, 1.0 parts of HMT, 8 parts of sulfur, 5-15 parts of antimony trioxide and 30 parts of aluminum hydroxide are mixed to obtain wear-resistant rubber;
[0081] Wear-resistant layer coating: Extruding and coating the prepared porous rubber on the surface of the wear-resistant layer prepared in step S5 to obtain a buffer layer;
[0082] S7. The coated cable is cooled in a continuous cooling water tank and then wound up using a wire take-up machine to obtain a cable product.
[0083] Embodiment 3:
[0084] S1. preparing a copper conductor layer by microalloying and twisting copper wires;
[0085] Microalloying: The surface of the copper wire is microalloyed at 580℃ under vacuum conditions. The alloying element is one of zinc, aluminum, magnesium, silver, etc. The surface content after alloying treatment is 0.005%, and the diameter of the copper wire is 0.2mm.
[0086] Twisting: twisting multiple alloyed copper wires in the same direction to obtain a copper conductor layer;
[0087] S2. A polytetrafluoroethylene insulation layer is obtained by winding glass fiber and polytetrafluoroethylene around the outer layer of the copper conductor;
[0088] Winding glass fiber: In S1, the outer layer of the copper conductor is wound with glass fiber, the winding angle is 50°, the middle span is 3mm, and the diameter of a single strand of glass fiber is 0.3mm;
[0089] Polytetrafluoroethylene coating: Put the polytetrafluoroethylene insulation material into the extruder, and extrude and coat it on the surface of the copper conductor layer coated with glass fiber to form a polytetrafluoroethylene insulation layer;
[0090] S3. Preparing a flame retardant layer on the surface of the insulating layer by mixing and coating the flame retardant layer;
[0091] Mixing: 100 parts of silicone rubber, 200 parts of metal hydroxide, 80 parts of unsaturated carboxylate, 8 parts of peroxide, 21 parts of montmorillonite, and 2 parts of graphene are mixed at 60°C for 20 minutes, and then vulcanized on a flat vulcanizer at 180°C for 20 minutes to obtain a flame retardant rubber;
[0092] Insulation layer coating: Extruding and coating the prepared flame-retardant rubber on the surface of the polytetrafluoroethylene insulation layer prepared in step S2 to obtain a flame-retardant layer;
[0093] S4. Preparing a flame retardant layer with a high temperature resistant surface layer by mixing and coating the high temperature layer;
[0094] Mixing: 70 parts of methyl vinyl rubber, 1 part of white carbon black activated dispersant, 20 parts of white carbon black, 1.5 parts of iron oxide, 2 parts of zinc oxide, 3 parts of high temperature resistant agent, 1 part of accelerator dibenzothiazole disulfide, 1.6 parts of benzoyl peroxide, 2 parts of 2,2,4-trimethyl-1,2-dihydroquinoline polymer, 10 parts of methyl tin heat stabilizer, and 5 parts of vulcanizing agent are mixed until uniform, and then vulcanized on a flat vulcanizer at 160°C for 20 minutes to obtain a high temperature resistant rubber;
[0095] Flame retardant layer coating: Extruding and coating the prepared high temperature resistant rubber on the surface of the flame retardant layer prepared in step S3 to obtain a high temperature resistant layer;
[0096] S5. Preparing a high temperature resistant surface buffer layer by mixing and coating the buffer layer;
[0097] Mixing: 100 parts of EPDM rubber, 30 parts of chloroprene rubber, 25 parts of stainless steel fiber, 5 parts of graphene, 5 parts of stearic acid, 20 parts of zinc borate, 15 parts of calcium carbonate, 15 parts of antimony trioxide, 2 parts of sulfur, 6 parts of accelerator, and 8 parts of foaming agent are mixed evenly, and then evenly spread on the surface of PET fluoroplastic release film, placed in a drying oven, and vulcanized and foamed at 130°C to obtain porous rubber, wherein the stainless steel fiber has a wire diameter of 20um, wherein the stainless steel fiber has a wire diameter of 20um;
[0098] Buffer layer coating: Extruding and coating the prepared porous rubber on the high temperature resistant surface prepared in step S4 to obtain a buffer layer;
[0099] S6. Preparing a wear-resistant layer on the surface of the buffer layer by mixing and coating the wear-resistant layer;
[0100] Mixing: 130 parts of styrene-butadiene rubber, 100 parts of natural rubber, 6 parts of graphene, 5 parts of stearic acid, 5 parts of accelerator, 1 part of antioxidant, 15 parts of alumina powder, 100 parts of white carbon black, 6 parts of coupling agent, 7 parts of phenolic resin, 0.7 parts of HMT, 6 parts of sulfur, 10 parts of antimony trioxide and 20 parts of aluminum hydroxide are mixed to obtain wear-resistant rubber;
[0101] Wear-resistant layer coating: Extruding and coating the prepared porous rubber on the surface of the wear-resistant layer prepared in step S5 to obtain a buffer layer;
[0102] S7. The coated cable is cooled in a continuous cooling water tank and then wound up using a wire take-up machine to obtain a cable product.
[0103] Comparative Example 1:
[0104] S1. A copper conductor layer is prepared by twisting copper wires;
[0105] Twisting: twisting multiple alloyed copper wires in the same direction to obtain a copper conductor layer;
[0106] S2. A polytetrafluoroethylene insulation layer is obtained by winding glass fiber and polytetrafluoroethylene around the outer layer of the copper conductor;
[0107] Winding glass fiber: In S1, the outer layer of the copper conductor is wound with glass fiber, the winding angle is 50°, the middle span is 3mm, and the diameter of a single strand of glass fiber is 0.3mm;
[0108] Polytetrafluoroethylene coating: Put the polytetrafluoroethylene insulation material into the extruder, and extrude and coat it on the surface of the copper conductor layer coated with glass fiber to form a polytetrafluoroethylene insulation layer;
[0109] S3. Preparing a flame retardant layer on the surface of the insulating layer by mixing and coating the flame retardant layer;
[0110] Mixing: 100 parts of silicone rubber, 200 parts of metal hydroxide, 80 parts of unsaturated carboxylate, 8 parts of peroxide, 21 parts of montmorillonite, and 2 parts of graphene are mixed at 60°C for 20 minutes, and then vulcanized on a flat vulcanizer at 180°C for 20 minutes to obtain a flame retardant rubber;
[0111] Insulation layer coating: Extruding and coating the prepared flame-retardant rubber on the surface of the polytetrafluoroethylene insulation layer prepared in step S2 to obtain a flame-retardant layer;
[0112] S4. Preparing a flame retardant layer with a high temperature resistant surface layer by mixing and coating the high temperature layer;
[0113] Mixing: 70 parts of methyl vinyl rubber, 1 part of white carbon black activated dispersant, 20 parts of white carbon black, 1.5 parts of iron oxide, 2 parts of zinc oxide, 3 parts of high temperature resistant agent, 1 part of accelerator dibenzothiazole disulfide, 1.6 parts of benzoyl peroxide, 2 parts of 2,2,4-trimethyl-1,2-dihydroquinoline polymer, 10 parts of methyl tin heat stabilizer, and 5 parts of vulcanizing agent are mixed until uniform, and then vulcanized on a flat vulcanizer at 160°C for 20 minutes to obtain a high temperature resistant rubber;
[0114] Flame retardant layer coating: Extruding and coating the prepared high temperature resistant rubber on the surface of the flame retardant layer prepared in step S3 to obtain a high temperature resistant layer;
[0115] S5. Preparing a high temperature resistant surface buffer layer by mixing and coating the buffer layer;
[0116] Mixing: 100 parts of EPDM rubber, 30 parts of chloroprene rubber, 25 parts of stainless steel fiber, 5 parts of graphene, 5 parts of stearic acid, 20 parts of zinc borate, 15 parts of calcium carbonate, 15 parts of antimony trioxide, 2 parts of sulfur, 6 parts of accelerator, and 8 parts of foaming agent are mixed evenly, and then evenly spread on the surface of PET fluoroplastic release film, placed in a drying oven, and vulcanized and foamed at 130°C to obtain porous rubber, wherein the stainless steel fiber has a wire diameter of 20um;
[0117] Buffer layer coating: Extruding and coating the prepared porous rubber on the high temperature resistant surface prepared in step S4 to obtain a buffer layer;
[0118] S6. Preparing a wear-resistant layer on the surface of the buffer layer by mixing and coating the wear-resistant layer;
[0119] Mixing: 130 parts of styrene-butadiene rubber, 100 parts of natural rubber, 6 parts of graphene, 5 parts of stearic acid, 5 parts of accelerator, 1 part of antioxidant, 15 parts of alumina powder, 100 parts of white carbon black, 6 parts of coupling agent, 7 parts of phenolic resin, 0.7 parts of HMT, 6 parts of sulfur, 10 parts of antimony trioxide and 20 parts of aluminum hydroxide are mixed to obtain wear-resistant rubber;
[0120] Wear-resistant layer coating: Extruding and coating the prepared porous rubber on the surface of the wear-resistant layer prepared in step S5 to obtain a buffer layer;
[0121] S7. The coated cable is cooled in a continuous cooling water tank and then wound up using a wire take-up machine to obtain a cable product.
[0122] Comparative Example 2:
[0123] S1. preparing a copper conductor layer by microalloying and twisting copper wires;
[0124] Microalloying: The surface of the copper wire is microalloyed at 580℃ under vacuum conditions. The alloying element is one of zinc, aluminum, magnesium, silver, etc. The surface content after alloying treatment is 0.005%, and the diameter of the copper wire is 0.2mm.
[0125] Twisting: twisting multiple alloyed copper wires in the same direction to obtain a copper conductor layer;
[0126] S2. A polytetrafluoroethylene insulation layer is obtained by coating the outer layer of the copper conductor with tetrafluoroethylene;
[0127] Polytetrafluoroethylene coating: Put the polytetrafluoroethylene insulation material into the extruder, and extrude and coat it on the surface of the copper conductor layer coated with glass fiber to form a polytetrafluoroethylene insulation layer;
[0128] S3. Preparing a flame retardant layer on the surface of the insulating layer by mixing and coating the flame retardant layer;
[0129] Mixing: 100 parts of silicone rubber, 200 parts of metal hydroxide, 80 parts of unsaturated carboxylate, 8 parts of peroxide, 21 parts of montmorillonite, and 2 parts of graphene are mixed at 60°C for 20 minutes, and then vulcanized on a flat vulcanizer at 180°C for 20 minutes to obtain a flame retardant rubber;
[0130] Insulation layer coating: Extruding and coating the prepared flame-retardant rubber on the surface of the polytetrafluoroethylene insulation layer prepared in step S2 to obtain a flame-retardant layer;
[0131] S4. Preparing a flame retardant layer with a high temperature resistant surface layer by mixing and coating the high temperature layer;
[0132] Mixing: 70 parts of methyl vinyl rubber, 1 part of white carbon black activated dispersant, 20 parts of white carbon black, 1.5 parts of iron oxide, 2 parts of zinc oxide, 3 parts of high temperature resistant agent, 1 part of accelerator dibenzothiazole disulfide, 1.6 parts of benzoyl peroxide, 2 parts of 2,2,4-trimethyl-1,2-dihydroquinoline polymer, 10 parts of methyl tin heat stabilizer, and 5 parts of vulcanizing agent are mixed until uniform, and then vulcanized on a flat vulcanizer at 160°C for 20 minutes to obtain a high temperature resistant rubber;
[0133] Flame retardant layer coating: Extruding and coating the prepared high temperature resistant rubber on the surface of the flame retardant layer prepared in step S3 to obtain a high temperature resistant layer;
[0134] S5. Preparing a high temperature resistant surface buffer layer by mixing and coating the buffer layer;
[0135] Mixing: 100 parts of EPDM rubber, 30 parts of chloroprene rubber, 25 parts of stainless steel fiber, 5 parts of graphene, 5 parts of stearic acid, 20 parts of zinc borate, 15 parts of calcium carbonate, 15 parts of antimony trioxide, 2 parts of sulfur, 6 parts of accelerator, and 8 parts of foaming agent are mixed evenly, and then evenly spread on the surface of PET fluoroplastic release film, placed in a drying oven, and vulcanized and foamed at 130°C to obtain porous rubber, wherein the stainless steel fiber has a wire diameter of 20um;
[0136] Buffer layer coating: Extruding and coating the prepared porous rubber on the high temperature resistant surface prepared in step S4 to obtain a buffer layer;
[0137] S6. Preparing a wear-resistant layer on the surface of the buffer layer by mixing and coating the wear-resistant layer;
[0138] Mixing: 130 parts of styrene-butadiene rubber, 100 parts of natural rubber, 6 parts of graphene, 5 parts of stearic acid, 5 parts of accelerator, 1 part of antioxidant, 15 parts of alumina powder, 100 parts of white carbon black, 6 parts of coupling agent, 7 parts of phenolic resin, 0.7 parts of HMT, 6 parts of sulfur, 10 parts of antimony trioxide and 20 parts of aluminum hydroxide are mixed to obtain wear-resistant rubber;
[0139] Wear-resistant layer coating: Extruding and coating the prepared porous rubber on the surface of the wear-resistant layer prepared in step S5 to obtain a buffer layer;
[0140] S7. The coated cable is cooled in a continuous cooling water tank and then wound up using a wire take-up machine to obtain a cable product.
[0141] Comparative Example 3:
[0142] S1. preparing a copper conductor layer by microalloying and twisting copper wires;
[0143] Microalloying: The surface of the copper wire is microalloyed at 580℃ under vacuum conditions. The alloying element is one of zinc, aluminum, magnesium, silver, etc. The surface content after alloying treatment is 0.005%, and the diameter of the copper wire is 0.2mm.
[0144] Twisting: twisting multiple alloyed copper wires in the same direction to obtain a copper conductor layer;
[0145] S2. A polytetrafluoroethylene insulation layer is obtained by winding glass fiber and polytetrafluoroethylene around the outer layer of the copper conductor;
[0146] Winding glass fiber: In S1, the outer layer of the copper conductor is wound with glass fiber, the winding angle is 50°, the middle span is 3mm, and the diameter of a single strand of glass fiber is 0.3mm;
[0147] Polytetrafluoroethylene coating: Put the polytetrafluoroethylene insulation material into the extruder, and extrude and coat it on the surface of the copper conductor layer coated with glass fiber to form a polytetrafluoroethylene insulation layer;
[0148] S3. Preparing a high temperature resistant layer on the surface of the insulating layer by mixing and coating the high temperature layer;
[0149] Mixing: 70 parts of methyl vinyl rubber, 1 part of white carbon black activated dispersant, 20 parts of white carbon black, 1.5 parts of iron oxide, 2 parts of zinc oxide, 3 parts of high temperature resistant agent, 1 part of accelerator dibenzothiazole disulfide, 1.6 parts of benzoyl peroxide, 2 parts of 2,2,4-trimethyl-1,2-dihydroquinoline polymer, 10 parts of methyl tin heat stabilizer, and 5 parts of vulcanizing agent are mixed until uniform, and then vulcanized on a flat vulcanizer at 160°C for 20 minutes to obtain a high temperature resistant rubber;
[0150] Flame retardant layer coating: Extruding and coating the prepared high temperature resistant rubber on the surface of the insulating layer prepared in step S2 to obtain a high temperature resistant layer;
[0151] S4. Preparing a high temperature resistant surface buffer layer by mixing and coating the buffer layer;
[0152] Mixing: 100 parts of EPDM rubber, 30 parts of chloroprene rubber, 25 parts of stainless steel fiber, 5 parts of graphene, 5 parts of stearic acid, 20 parts of zinc borate, 15 parts of calcium carbonate, 15 parts of antimony trioxide, 2 parts of sulfur, 6 parts of accelerator, and 8 parts of foaming agent are mixed evenly, and then evenly spread on the surface of PET fluoroplastic release film, placed in a drying oven, and vulcanized and foamed at 130°C to obtain porous rubber, wherein the stainless steel fiber has a wire diameter of 20um;
[0153] Buffer layer coating: Extruding and coating the prepared porous rubber on the high temperature resistant surface prepared in step S3 to obtain a buffer layer;
[0154] S5. Prepare the wear-resistant layer on the surface of the buffer layer by mixing and coating the wear-resistant layer;
[0155] Mixing: 130 parts of styrene-butadiene rubber, 100 parts of natural rubber, 6 parts of graphene, 5 parts of stearic acid, 5 parts of accelerator, 1 part of antioxidant, 15 parts of alumina powder, 100 parts of white carbon black, 6 parts of coupling agent, 7 parts of phenolic resin, 0.7 parts of HMT, 6 parts of sulfur, 10 parts of antimony trioxide and 20 parts of aluminum hydroxide are mixed to obtain wear-resistant rubber;
[0156] Wear-resistant layer coating: Extruding and coating the prepared porous rubber on the surface of the wear-resistant layer prepared in step S4 to obtain a buffer layer;
[0157] S6. The coated cable is cooled in a continuous cooling water tank and then wound up using a wire take-up machine to obtain a cable product.
[0158] Comparative Example 4:
[0159] S1. preparing a copper conductor layer by microalloying and twisting copper wires;
[0160] Microalloying: The surface of the copper wire is microalloyed at 580℃ under vacuum conditions. The alloying element is one of zinc, aluminum, magnesium, silver, etc. The surface content after alloying treatment is 0.005%, and the diameter of the copper wire is 0.2mm.
[0161] Twisting: twisting multiple alloyed copper wires in the same direction to obtain a copper conductor layer;
[0162] S2. A polytetrafluoroethylene insulation layer is obtained by winding glass fiber and polytetrafluoroethylene around the outer layer of the copper conductor;
[0163] Winding glass fiber: In S1, the outer layer of the copper conductor is wound with glass fiber, the winding angle is 50°, the middle span is 3mm, and the diameter of a single strand of glass fiber is 0.3mm;
[0164] Polytetrafluoroethylene coating: Put the polytetrafluoroethylene insulation material into the extruder, and extrude and coat it on the surface of the copper conductor layer coated with glass fiber to form a polytetrafluoroethylene insulation layer;
[0165] S3. Preparing a flame retardant layer on the surface of the insulating layer by mixing and coating the flame retardant layer;
[0166] Mixing: 100 parts of silicone rubber, 200 parts of metal hydroxide, 80 parts of unsaturated carboxylate, 8 parts of peroxide, 21 parts of montmorillonite, and 2 parts of graphene are mixed at 60°C for 20 minutes, and then vulcanized on a flat vulcanizer at 180°C for 20 minutes to obtain a flame retardant rubber;
[0167] Insulation layer coating: Extruding and coating the prepared flame-retardant rubber on the surface of the polytetrafluoroethylene insulation layer prepared in step S2 to obtain a flame-retardant layer;
[0168] S4. Preparing a high temperature resistant surface buffer layer by mixing and coating the buffer layer;
[0169] Mixing: 100 parts of EPDM rubber, 30 parts of chloroprene rubber, 25 parts of stainless steel fiber, 5 parts of graphene, 5 parts of stearic acid, 20 parts of zinc borate, 15 parts of calcium carbonate, 15 parts of antimony trioxide, 2 parts of sulfur, 6 parts of accelerator, and 8 parts of foaming agent are mixed evenly, and then evenly spread on the surface of PET fluoroplastic release film, placed in a drying oven, and vulcanized and foamed at 130°C to obtain porous rubber, wherein the stainless steel fiber has a wire diameter of 20um;
[0170] Buffer layer coating: Extruding and coating the prepared porous rubber on the surface of the flame retardant layer prepared in step S3 to obtain a buffer layer;
[0171] S5. Prepare the wear-resistant layer on the surface of the buffer layer by mixing and coating the wear-resistant layer;
[0172] Mixing: 130 parts of styrene-butadiene rubber, 100 parts of natural rubber, 6 parts of graphene, 5 parts of stearic acid, 5 parts of accelerator, 1 part of antioxidant, 15 parts of alumina powder, 100 parts of white carbon black, 6 parts of coupling agent, 7 parts of phenolic resin, 0.7 parts of HMT, 6 parts of sulfur, 10 parts of antimony trioxide and 20 parts of aluminum hydroxide are mixed to obtain wear-resistant rubber;
[0173] Wear-resistant layer coating: Extruding and coating the prepared porous rubber on the surface of the wear-resistant layer prepared in step S4 to obtain a buffer layer;
[0174] S6. The coated cable is cooled in a continuous cooling water tank and then wound up using a wire take-up machine to obtain a cable product.
[0175] Comparative Example 5:
[0176] S1. preparing a copper conductor layer by microalloying and twisting copper wires;
[0177] Microalloying: The surface of the copper wire is microalloyed at 580℃ under vacuum conditions. The alloying element is one of zinc, aluminum, magnesium, silver, etc. The surface content after alloying treatment is 0.005%, and the diameter of the copper wire is 0.2mm.
[0178] Twisting: twisting multiple alloyed copper wires in the same direction to obtain a copper conductor layer;
[0179] S2. A polytetrafluoroethylene insulation layer is obtained by winding glass fiber and polytetrafluoroethylene around the outer layer of the copper conductor;
[0180] Winding glass fiber: In S1, the outer layer of the copper conductor is wound with glass fiber, the winding angle is 50°, the middle span is 3mm, and the diameter of a single strand of glass fiber is 0.3mm;
[0181] Polytetrafluoroethylene coating: Put the polytetrafluoroethylene insulation material into the extruder, and extrude and coat it on the surface of the copper conductor layer coated with glass fiber to form a polytetrafluoroethylene insulation layer;
[0182] S3. Preparing a flame retardant layer on the surface of the insulating layer by mixing and coating the flame retardant layer;
[0183] Mixing: 100 parts of silicone rubber, 200 parts of metal hydroxide, 80 parts of unsaturated carboxylate, 8 parts of peroxide, 21 parts of montmorillonite, and 2 parts of graphene are mixed at 60°C for 20 minutes, and then vulcanized on a flat vulcanizer at 180°C for 20 minutes to obtain a flame retardant rubber;
[0184] Insulation layer coating: Extruding and coating the prepared flame-retardant rubber on the surface of the polytetrafluoroethylene insulation layer prepared in step S2 to obtain a flame-retardant layer;
[0185] S4. Preparing a flame retardant layer with a high temperature resistant surface layer by mixing and coating the high temperature layer;
[0186] Mixing: 70 parts of methyl vinyl rubber, 1 part of white carbon black activated dispersant, 20 parts of white carbon black, 1.5 parts of iron oxide, 2 parts of zinc oxide, 3 parts of high temperature resistant agent, 1 part of accelerator dibenzothiazole disulfide, 1.6 parts of benzoyl peroxide, 2 parts of 2,2,4-trimethyl-1,2-dihydroquinoline polymer, 10 parts of methyl tin heat stabilizer, and 5 parts of vulcanizing agent are mixed until uniform, and then vulcanized on a flat vulcanizer at 160°C for 20 minutes to obtain a high temperature resistant rubber;
[0187] Flame retardant layer coating: Extruding and coating the prepared high temperature resistant rubber on the surface of the flame retardant layer prepared in step S3 to obtain a high temperature resistant layer;
[0188] S5. Prepare the wear-resistant layer on the surface of the buffer layer by mixing and coating the wear-resistant layer;
[0189] Mixing: 130 parts of styrene-butadiene rubber, 100 parts of natural rubber, 6 parts of graphene, 5 parts of stearic acid, 5 parts of accelerator, 1 part of antioxidant, 15 parts of alumina powder, 100 parts of white carbon black, 6 parts of coupling agent, 7 parts of phenolic resin, 0.7 parts of HMT, 6 parts of sulfur, 10 parts of antimony trioxide and 20 parts of aluminum hydroxide are mixed to obtain wear-resistant rubber;
[0190] Wear-resistant layer coating: Extruding and coating the prepared porous rubber on the surface of the wear-resistant layer prepared in step S4 to obtain a buffer layer;
[0191] S6. The coated cable is cooled in a continuous cooling water tank and then wound up using a wire take-up machine to obtain a cable product.
[0192] Comparative Example 6:
[0193] S1. preparing a copper conductor layer by microalloying and twisting copper wires;
[0194] Microalloying: The surface of the copper wire is microalloyed at 580℃ under vacuum conditions. The alloying element is one of zinc, aluminum, magnesium, silver, etc. The surface content after alloying treatment is 0.005%, and the diameter of the copper wire is 0.2mm.
[0195] Twisting: twisting multiple alloyed copper wires in the same direction to obtain a copper conductor layer;
[0196] S2. A polytetrafluoroethylene insulation layer is obtained by winding glass fiber and polytetrafluoroethylene around the outer layer of the copper conductor;
[0197] Winding glass fiber: In S1, the outer layer of the copper conductor is wound with glass fiber, the winding angle is 50°, the middle span is 3mm, and the diameter of a single strand of glass fiber is 0.3mm;
[0198] Polytetrafluoroethylene coating: Put the polytetrafluoroethylene insulation material into the extruder, and extrude and coat it on the surface of the copper conductor layer coated with glass fiber to form a polytetrafluoroethylene insulation layer;
[0199] S3. Preparing a flame retardant layer on the surface of the insulating layer by mixing and coating the flame retardant layer;
[0200] Mixing: 100 parts of silicone rubber, 200 parts of metal hydroxide, 80 parts of unsaturated carboxylate, 8 parts of peroxide, 21 parts of montmorillonite, and 2 parts of graphene are mixed at 60°C for 20 minutes, and then vulcanized on a flat vulcanizer at 180°C for 20 minutes to obtain a flame retardant rubber;
[0201] Insulation layer coating: Extruding and coating the prepared flame-retardant rubber on the surface of the polytetrafluoroethylene insulation layer prepared in step S2 to obtain a flame-retardant layer;
[0202] S4. Preparing a flame retardant layer with a high temperature resistant surface layer by mixing and coating the high temperature layer;
[0203] Mixing: 70 parts of methyl vinyl rubber, 1 part of white carbon black activated dispersant, 20 parts of white carbon black, 1.5 parts of iron oxide, 2 parts of zinc oxide, 3 parts of high temperature resistant agent, 1 part of accelerator dibenzothiazole disulfide, 1.6 parts of benzoyl peroxide, 2 parts of 2,2,4-trimethyl-1,2-dihydroquinoline polymer, 10 parts of methyl tin heat stabilizer, and 5 parts of vulcanizing agent are mixed until uniform, and then vulcanized on a flat vulcanizer at 160°C for 20 minutes to obtain a high temperature resistant rubber;
[0204] Flame retardant layer coating: Extruding and coating the prepared high temperature resistant rubber on the surface of the flame retardant layer prepared in step S3 to obtain a high temperature resistant layer;
[0205] S5. Preparing a high temperature resistant surface buffer layer by mixing and coating the buffer layer;
[0206] Mixing: 100 parts of EPDM rubber, 30 parts of chloroprene rubber, 5 parts of graphene, 5 parts of stearic acid, 20 parts of zinc borate, 15 parts of calcium carbonate, 15 parts of antimony trioxide, 2 parts of sulfur, 6 parts of accelerator, and 8 parts of foaming agent are mixed evenly, and then evenly spread on the surface of PET fluoroplastic release film, placed in a drying oven, and vulcanized and foamed at 130°C to obtain porous rubber;
[0207] Buffer layer coating: Extruding and coating the prepared porous rubber on the high temperature resistant surface prepared in step S4 to obtain a buffer layer;
[0208] S6. Preparing a wear-resistant layer on the surface of the buffer layer by mixing and coating the wear-resistant layer;
[0209] Mixing: 130 parts of styrene-butadiene rubber, 100 parts of natural rubber, 6 parts of graphene, 5 parts of stearic acid, 5 parts of accelerator, 1 part of antioxidant, 15 parts of alumina powder, 100 parts of white carbon black, 6 parts of coupling agent, 7 parts of phenolic resin, 0.7 parts of HMT, 6 parts of sulfur, 10 parts of antimony trioxide and 20 parts of aluminum hydroxide are mixed to obtain wear-resistant rubber;
[0210] Wear-resistant layer coating: Extruding and coating the prepared porous rubber on the surface of the wear-resistant layer prepared in step S5 to obtain a buffer layer;
[0211] S7. The coated cable is cooled in a continuous cooling water tank and then wound up using a wire take-up machine to obtain a cable product.
[0212] Comparative Example 7:
[0213] S1. preparing a copper conductor layer by microalloying and twisting copper wires;
[0214] Microalloying: The surface of the copper wire is microalloyed at 580℃ under vacuum conditions. The alloying element is one of zinc, aluminum, magnesium, silver, etc. The surface content after alloying treatment is 0.005%, and the diameter of the copper wire is 0.2mm.
[0215] Twisting: twisting multiple alloyed copper wires in the same direction to obtain a copper conductor layer;
[0216] S2. A polytetrafluoroethylene insulation layer is obtained by winding glass fiber and polytetrafluoroethylene around the outer layer of the copper conductor;
[0217] Winding glass fiber: In S1, the outer layer of the copper conductor is wound with glass fiber, the winding angle is 50°, the middle span is 3mm, and the diameter of a single strand of glass fiber is 0.3mm;
[0218] Polytetrafluoroethylene coating: Put the polytetrafluoroethylene insulation material into the extruder, and extrude and coat it on the surface of the copper conductor layer coated with glass fiber to form a polytetrafluoroethylene insulation layer;
[0219] S3. Preparing a flame retardant layer on the surface of the insulating layer by mixing and coating the flame retardant layer;
[0220] Mixing: 100 parts of silicone rubber, 200 parts of metal hydroxide, 80 parts of unsaturated carboxylate, 8 parts of peroxide, 21 parts of montmorillonite, and 2 parts of graphene are mixed at 60°C for 20 minutes, and then vulcanized on a flat vulcanizer at 180°C for 20 minutes to obtain a flame retardant rubber;
[0221] Insulation layer coating: Extruding and coating the prepared flame-retardant rubber on the surface of the polytetrafluoroethylene insulation layer prepared in step S2 to obtain a flame-retardant layer;
[0222] S4. Preparing a flame retardant layer with a high temperature resistant surface layer by mixing and coating the high temperature layer;
[0223] Mixing: 70 parts of methyl vinyl rubber, 1 part of white carbon black activated dispersant, 20 parts of white carbon black, 1.5 parts of iron oxide, 2 parts of zinc oxide, 3 parts of high temperature resistant agent, 1 part of accelerator dibenzothiazole disulfide, 1.6 parts of benzoyl peroxide, 2 parts of 2,2,4-trimethyl-1,2-dihydroquinoline polymer, 10 parts of methyl tin heat stabilizer, and 5 parts of vulcanizing agent are mixed until uniform, and then vulcanized on a flat vulcanizer at 160°C for 20 minutes to obtain a high temperature resistant rubber;
[0224] Flame retardant layer coating: Extruding and coating the prepared high temperature resistant rubber on the surface of the flame retardant layer prepared in step S3 to obtain a high temperature resistant layer;
[0225] S5. Preparing a high temperature resistant surface buffer layer by mixing and coating the buffer layer;
[0226] Mixing: 100 parts of EPDM rubber, 30 parts of chloroprene rubber, 25 parts of stainless steel fiber, 5 parts of graphene, 5 parts of stearic acid, 20 parts of zinc borate, 15 parts of calcium carbonate, 15 parts of antimony trioxide, 2 parts of sulfur, 6 parts of accelerator, and 8 parts of foaming agent are mixed evenly, and then evenly spread on the surface of PET fluoroplastic release film, placed in a drying oven, and vulcanized and foamed at 130°C to obtain porous rubber, wherein the stainless steel fiber has a wire diameter of 20um;
[0227] Buffer layer coating: Extruding and coating the prepared porous rubber on the high temperature resistant surface prepared in step S4 to obtain a buffer layer;
[0228] S7. The coated cable is cooled in a continuous cooling water tank and then wound up using a wire take-up machine to obtain a cable product.
[0229] tensile strength:
[0230] Tensile strength is the resistance to the maximum uniform plastic deformation of the material. Before the tensile specimen is subjected to the maximum tensile stress, the deformation is uniform and consistent, but after exceeding the maximum tensile stress, the metal begins to shrink, that is, concentrated deformation occurs; for brittle materials with no (or very small) uniform plastic deformation, it reflects the material's fracture resistance. The test standard can refer to the national standard GB / T228-1987), the unit is MPa;
[0231] Elongation after break:
[0232] It refers to the percentage of the elongated length of the specimen to the original length when the material breaks under the action of external force (tension). The test standard can refer to the national standard GB / T 528-2009.
[0233] Table 1
[0234]
[0235] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.
Claims
1. A high temperature resistant cable for new energy vehicles and a preparation method thereof, characterized in that: The steps include: S1. preparing a copper conductor layer by microalloying and twisting copper wires; S2. A polytetrafluoroethylene insulation layer is obtained by winding glass fiber and polytetrafluoroethylene around the outer layer of the copper conductor; S3. Preparing a flame retardant layer on the surface of the insulating layer by mixing and coating the flame retardant layer; S4. Preparing a flame retardant layer with a high temperature resistant surface layer by mixing and coating the high temperature layer; S5. Preparing a high temperature resistant surface buffer layer by mixing and coating the buffer layer; S6. Preparing a wear-resistant layer on the surface of the buffer layer by mixing and coating the wear-resistant layer; S7. The coated cable is cooled in a continuous cooling water tank and then wound up using a wire take-up machine to obtain a cable product.
2. The preparation method according to claim 1, characterized in that: The high temperature resistant cable consists of a conductor layer, an insulation layer, a flame retardant layer, a high temperature resistant layer, a buffer layer and a wear resistant layer from the inside to the outside.
3. The preparation method according to claim 1, characterized in that: In step S1, the process of microalloying the copper wire includes: microalloying the surface of the copper wire under vacuum conditions at 550-600°C, wherein the alloying element is one of zinc, aluminum, magnesium, silver, etc., and the surface content after alloying treatment is 0.001-0.01%, wherein the diameter of the copper wire is 0.1-0.3mm.
4. The preparation method according to claim 1, characterized in that: In step S2, the flame retardant layer is composed of two layers: a glass fiber layer and a polytetrafluoroethylene layer.
5. The preparation method according to claim 1, characterized in that: In step S2, the process of winding glass fiber includes: in S1, the outer layer of the copper conductor is wound with glass fiber, the winding angle is 45°-60°, the middle span is 1-5mm, and the diameter of a single strand of glass fiber is 0.2-0.5mm.
6. The preparation method according to claim 1, characterized in that: In step S3, the raw materials of the flame retardant layer include: 80-120 parts of silicone rubber, 150-250 parts of metal hydroxide, 60-100 parts of unsaturated carboxylate, 5-10 parts of peroxide, 20-22 parts of montmorillonite, and 1-3 parts of graphene.
7. The preparation method according to claim 1, characterized in that: In step S4, the raw materials of the high temperature resistant layer include: 60-80 parts of methyl vinyl rubber, 0.8-1.2 parts of white carbon black activated dispersant, 15-25 parts of white carbon black, 1-2 parts of iron oxide, 1-3 parts of zinc oxide, 2-4 parts of high temperature resistant agent, 0.8-1.2 parts of accelerator dibenzothiazole disulfide, 1.2-1.8 parts of benzoyl peroxide, 2-3 parts of 2,2,4-trimethyl-1,2-dihydroquinoline polymer, 5-15 parts of methyl tin heat stabilizer, and 2-7 parts of vulcanizing agent.
8. The preparation method according to claim 1, characterized in that: In step S5, the buffer layer raw materials include: 90-120 parts of EPDM rubber, 20-40 parts of chloroprene rubber, 20-30 parts of stainless steel fiber, 3-8 parts of graphene, 3-7 parts of stearic acid, 15-25 parts of zinc borate, 5-25 parts of calcium carbonate, 5-20 parts of antimony trioxide, 1-2 parts of sulfur, 4-8 parts of accelerator, and 5-10 parts of foaming agent.
9. The preparation method according to claim 8, characterized in that: The stainless steel fiber has a diameter of 10-30 um.
10. The preparation method according to claim 1, characterized in that: In step S6, the wear-resistant layer raw materials include: 100-150 parts of styrene-butadiene rubber, 80-120 parts of natural rubber, 2-10 parts of graphene, 3-8 parts of stearic acid, 3-7 parts of accelerator, 0.5-1.5 parts of antioxidant, 10-20 parts of alumina powder, 10-200 parts of white carbon black, 3-8 parts of coupling agent, 5-10 parts of phenolic resin, 0.5-1.0 parts of HMT, 5-8 parts of sulfur, 5-15 parts of antimony trioxide, and 10-30 parts of aluminum hydroxide.
Citation Information
Patent Citations
Insect-proof bacteriostatic weather-resistant and flame-retardant cable sheath material and preparation method thereof
CN108264661A
Preparation method of anti-oxidation alloy copper wire
CN109182830A
Graphene natural rubber anti-radiation composite foam material and preparation method thereof
CN111138726A
High-strength pull-resistant cable and preparation method thereof
CN112164490A
High-temperature-resistant flexible cable for new energy automobile and production method of high-temperature-resistant flexible cable